A bimetallic composite bend and its preparation method
By employing milling, X-bevel rolling, and specific heat treatment processes, the problems of low production efficiency and unstable quality of small-diameter bimetallic composite bends have been solved, achieving an efficient and stable preparation method that ensures stress release and excellent material properties of the cladding during the forming process.
Patent Information
- Application Number
- CN202410361893.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-28
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2044-03-28
AI Technical Summary
Existing technologies for manufacturing small-diameter bimetallic composite bends suffer from low production efficiency, high costs, unstable product quality, and difficulty in controlling the welding process, which can easily lead to dilution of alloying elements in the bonding layer and welding quality issues.
After milling and X-bevel rolling, only the base layer and transition layer are welded. After hot bending, the cladding layer is welded and then quenched and normalized to ensure that the cladding layer has stress release space during the forming process. Combined with a specific heat treatment temperature range, the material properties are optimized.
It improves production efficiency, avoids multilayer bulging and wrinkling, enhances intergranular corrosion and mechanical properties of products, and ensures product quality stability and service life.
Smart Images

Figure CN118188920B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of pipeline equipment technology, and in particular to a bimetallic composite bend and its preparation method. Background Technology
[0002] Bimetallic composite pipe fittings are commonly used for natural gas transportation and are among the most dangerous gathering and transmission pipelines. Currently, for small-diameter bimetallic composite bends, existing technologies generally employ welding overlay methods for fabrication. This method is time-consuming, inefficient, involves a large amount of welding work, and has high manufacturing costs. Welding overlays can dilute the alloy material in the bonding layer, and the instability of the alloy element composition reduces corrosion resistance and other properties, resulting in unreliable product quality. Furthermore, the technical expertise of welding manufacturers varies, making it difficult to repair weld overlays with quality problems. Therefore, there is an urgent need to find a method for manufacturing bimetallic composite bends that offers high production efficiency and stable product quality. Summary of the Invention
[0003] To address the aforementioned problems, this invention provides a bimetallic composite bend and its preparation method. The composite layer is less prone to bulging and wrinkling, exhibits excellent intergranular corrosion and mechanical properties, and also boasts high production efficiency and a long service life.
[0004] To address the aforementioned technical problems, the present invention provides the following technical solution.
[0005] In a first aspect, the present invention provides a method for preparing a bimetallic composite bend, comprising the following steps:
[0006] S1, mill the edges of the bimetallic composite sheet, use an X-groove for the butt weld, roll the tube to obtain a tube blank; the bimetallic composite sheet includes a base layer, a transition layer and a cladding layer;
[0007] S2, Weld the base layer and transition layer of the tube blank to obtain a welded tube blank;
[0008] S3, the welded tube blank is loaded into the bending machine, positioned, and hot-bent to obtain a bent tube blank;
[0009] S4, weld the cladding layer of the bent pipe blank to obtain a welded bent pipe;
[0010] S5, the welded bend is quenched at 930-970℃ and cooled; then normalized at 880-920℃ and cooled to obtain a bimetallic composite bend.
[0011] Compared with existing technologies, the bimetallic composite pipe preparation method provided by this invention only welds the base layer and transition layer of the pipe blank after rolling, without welding the cladding layer. This leaves a gap allowance for the deformation of the cladding layer during the subsequent hot bending forming process, allowing the cladding layer to have space for stress release during the forming process, effectively avoiding the separation of the base layer and cladding layer during the forming process (including bulging and wrinkling). Then, the welded pipe blank is placed on a bending machine, hot bent into a pipe blank, and then the cladding layer is welded and subjected to subsequent heat treatment.
[0012] Generally, for single materials, normalizing carbon steel or pipeline steel fittings within a temperature range of 880–940℃ and solution treatment of stainless steel fittings at a temperature not lower than 1040℃ can ensure that their corresponding ferrite, hardness, and intergranular corrosion resistance all meet the requirements. Through extensive experimentation, the inventors discovered that for bimetallic composite fittings, quenching at 930–970℃ ensures excellent intergranular corrosion resistance in the cladding layer (stainless steel); normalizing at 880–920℃ ensures excellent hardness and toughness in the base layer (carbon steel or pipeline steel); and the combination of quenching and normalizing heat treatment ensures excellent overall performance of the bimetallic composite fittings, thus guaranteeing product quality.
[0013] The method for preparing bimetallic composite bends provided by this invention replaces the conventional welding process, is simple and easy to operate, greatly shortens time and labor costs, effectively improves production efficiency, and has high economic benefits and market value.
[0014] Preferably, in step S1, the base layer of the bimetallic composite plate is carbon steel or pipeline steel, and the cladding layer of the bimetallic composite plate is austenitic stainless steel or nickel-based stainless steel.
[0015] It should be noted that the transition layer of the bimetallic composite panel is defined as the fusion layer between the base layer and the cladding layer, that is, the material of the transition layer is a mixture of metallic elements fused together from the base layer and the cladding layer. It is generally believed that the thicker the transition layer of the bimetallic composite panel, the greater the bonding force between the base layer and the cladding layer. This invention does not impose requirements on the thickness of the transition layer of the bimetallic composite panel; commercially available bimetallic composite panels are suitable for this invention.
[0016] Preferably, the diameter of the bimetallic composite bend is DN150 to DN700.
[0017] Preferably, the thickness of the bimetallic composite bend is 8-30 mm; wherein, the thickness of the base layer of the bimetallic composite bend is 6-25 mm, and the thickness of the cladding layer of the bimetallic composite bend is 2-6 mm.
[0018] This invention replaces the commonly used welding process for manufacturing small-diameter bimetallic composite bends, solves the problem of unstable product quality of small-diameter bimetallic composite bends, and greatly improves the production efficiency of small-diameter bimetallic composite bends.
[0019] For example, in step S1, before milling the edges, the bimetallic composite sheet needs to be re-inspected, including its chemical composition, appearance, thickness and consistency of the base layer and the cladding layer, mechanical properties and non-destructive testing, to confirm that the quality of the bimetallic composite sheet meets the requirements.
[0020] For example, in step S1, during the edge milling process, the base layer of the bimetallic composite sheet is on top and the cladding layer of the bimetallic composite sheet is on the bottom, so as to protect the cladding layer from damage during the edge milling process.
[0021] The butt weld in step S1 of this invention adopts an X-groove, which is beneficial for subsequent batch welding (welding the base layer and transition layer first, hot bending and forming, and then welding the cladding layer); in addition, the cladding layer of the tube blank is not welded in step S2, and in the subsequent forming process, the gap of the X-groove provides a specific space for stress release of the cladding layer of the tube blank.
[0022] For example, in step S1, before rolling the tube, the rollers of the tube rolling machine need to be cleaned and their surfaces trimmed, and then covered with adhesive tape or paper that does not contain iron ions to prevent the introduction of impurities during the rolling process, which would affect the quality of the bimetallic composite bend.
[0023] For example, in step S1, before the tube is rolled, the base layer of the bimetallic composite sheet is on the bottom and the cladding layer of the bimetallic composite sheet is on the top, so that in the resulting tube blank, the base layer is on the outside and the cladding layer is on the inside.
[0024] Preferably, in step S2, the welding thickness of the transition layer of the tube blank is 3-5 mm.
[0025] In this invention, the thickness of the transition layer of the tube blank and the transition layer of the bimetallic composite plate are basically the same. Since the thickness of the transition layer is small and difficult to measure, this invention sets the welding thickness of the transition layer of the tube blank to 3-5mm. This ensures that the transition layer is fully welded while ensuring that most of the cladding layer is not welded, leaving room for the X-groove gap in the subsequent hot bending forming process of the tube. This allows the stress of the cladding layer to be released during the forming process, effectively preventing the separation of the base layer and the cladding layer during the forming process.
[0026] It should be noted that the welding thickness of the transition layer of the tube blank (3-5mm) is centered on the contact line between the base layer and the cladding layer (the contact surface between the base layer and the cladding layer is linear when viewed from the cross-section), offset by 2-4mm towards the base layer and 1-2mm towards the cladding layer.
[0027] Preferably, in step S3, the hot bending forming is achieved by using a medium-frequency coil for heating and water cooling.
[0028] For example, in step S3, the water cooling uses circulating water.
[0029] For example, in step S3, before the first hot bending, it is necessary to check for any abnormalities in the bending machine, heating coil, and water pump to ensure that the hot bending can proceed normally. Adjust the boom of the pipe bending machine to the 0° position, adjust the required bending radius, and use an overhead crane to load the welded pipe blank onto the bending machine.
[0030] In step S3 of this invention, the end of the welded tube blank is positioned appropriately by positioning, allowing it to be held by the rotating arm, which facilitates subsequent hot bending. Furthermore, after positioning, the weld seam of the welded tube blank faces upwards. During the hot bending process, the welded tube blank is bent horizontally, and the upward-facing weld seam ensures that the weld seam of the resulting bent tube blank is in a position without stress (or with minimal stress). This reduces the likelihood of cracking at the weld seam during subsequent use of the bimetallic composite bent tube, thereby extending its service life.
[0031] Preferably, in step S3, the conditions for hot bending include: a heating temperature of 800–1000°C and a pushing speed of 30–40 cm / min.
[0032] In step S3 of this invention, the heating temperature is related to the base material of the bimetallic composite plate / bimetallic composite bend, and can be adjusted according to the specific grade of the base material.
[0033] For example, in step S4, before welding, the weld area needs to be cleaned to avoid introducing impurities during the welding process, thereby ensuring the mechanical properties of the weld.
[0034] Preferably, in step S5, the furnace entry temperature for the quenching treatment is 930–970°C.
[0035] Preferably, in step S5, the furnace entry temperature for the normalizing treatment is 930–970°C.
[0036] Through numerous experiments, the inventors discovered that when performing quenching and normalizing treatments, heating the empty furnace to 930–970°C before loading the welded bend can reduce the residence time of the cladding layer in the sensitization temperature zone, thereby further ensuring intergranular corrosion resistance.
[0037] Preferably, in step S5, the holding time for the quenching treatment is 30 to 60 minutes.
[0038] Preferably, in step S5, the holding time for the normalizing treatment is 30 to 60 minutes.
[0039] For example, in step S5, the holding time for both the quenching treatment and the normalizing treatment is not less than 1.2 min / mm.
[0040] For example, in step S5, the cooling process of the quenching treatment includes: first water cooling the heated welded bend to 400-460°C, and then air cooling to room temperature.
[0041] For example, in step S5, the cooling process of the normalizing treatment includes: air cooling the heated welded bend to room temperature.
[0042] For example, the method for preparing the bimetallic composite bend further includes:
[0043] S6. The bimetallic composite bend is machined, surface treated, beveled, and subjected to non-destructive testing.
[0044] For example, the surface treatment includes sandblasting the base layer of the bimetallic composite bend and polishing the cladding layer of the bimetallic composite bend.
[0045] For example, the nondestructive testing includes magnetic particle testing, ultrasonic testing, penetrant testing, and radiographic testing of welds.
[0046] Secondly, the present invention provides a bimetallic composite bend obtained by the above-described method for preparing a bimetallic composite bend.
[0047] Compared with existing technologies, the bimetallic composite bend provided by this invention is less prone to bulging and wrinkling of the cladding layer, and at the same time, it exhibits excellent intergranular corrosion resistance and mechanical properties. Attached Figure Description
[0048] Figure 1 This is a metallographic diagram of the cladding layer of the bimetallic composite bend in Embodiment 1 of the present invention;
[0049] Figure 2 This is a metallographic diagram of the cladding layer of the bimetallic composite bend of Comparative Example 4 of the present invention. Detailed Implementation
[0050] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention.
[0051] This invention does not impose excessive requirements on the specific materials of the base layer and cladding layer of the bimetallic composite sheet. As long as the base layer is carbon steel or pipeline steel and the cladding layer is austenitic stainless steel or nickel-based stainless steel, it is applicable to this invention. In the bimetallic composite sheets used in the embodiments and comparative examples of this invention, the base layer material is L360 and the cladding layer material is 304L.
[0052] To better illustrate the present invention, further examples are provided below.
[0053] Example 1
[0054] This embodiment provides a method for preparing a bimetallic composite bend, including the following steps:
[0055] S1. Mill the edges of the bimetallic composite sheet (the base layer thickness of the bimetallic composite sheet is 12mm and the cladding layer thickness is 3mm, denoted as 12+3) that has passed the re-inspection and quality test, use the X bevel for the butt weld, roll the pipe to obtain the pipe blank.
[0056] S2, the base layer and transition layer of the above-mentioned tube blank are welded sequentially to obtain a welded tube blank. The welding thickness of the transition layer is 4mm, and it is offset 3mm towards the base layer and 1mm towards the cladding layer, with the contact line between the base layer and the cladding layer as the center.
[0057] S3. Adjust the swing arm of the pipe bending machine to the 0° position, adjust the required bending radius, load the above-mentioned welded pipe blank onto the bending machine, position it, and perform hot bending at 850°C with a pushing speed of 35cm / min to obtain the bent pipe blank.
[0058] S4. Clean the weld seam of the above-mentioned bent pipe blank, and weld the cladding layer of the bent pipe blank to obtain a welded bent pipe.
[0059] S5. Heat the furnace to 950℃ in an empty oven, load the above-mentioned welded bend into the furnace, quench it at 950℃, hold it for 40 minutes, water cool it to 450℃, and then air cool it to room temperature. Heat the furnace to 950℃ in an empty oven, load the quenched and cooled welded bend into the furnace, normalize it at 900℃, hold it for 40 minutes, and then air cool it to room temperature to obtain a Φ355.6×(10+3) bimetallic composite bend.
[0060] It should be noted that Φ355.6×(10+3) indicates that the outer diameter of the bimetallic composite bend is 355.6mm, the base layer thickness is 10mm, and the cladding layer thickness is 3mm.
[0061] Example 2
[0062] This embodiment provides a method for preparing a bimetallic composite bend, including the following steps:
[0063] S1. Mill the edges of the bimetallic composite plate (14+3) that has passed the re-inspection, use the X bevel for the butt weld, roll the pipe to obtain the pipe blank.
[0064] S2, the base layer and transition layer of the above-mentioned tube blank are welded sequentially to obtain a welded tube blank. The welding thickness of the transition layer is 4mm, and it is offset 3mm towards the base layer and 1mm towards the cladding layer, with the contact line between the base layer and the cladding layer as the center.
[0065] S3. Adjust the swing arm of the pipe bending machine to the 0° position, adjust the required bending radius, load the above-mentioned welded pipe blank onto the bending machine, position it, and perform hot bending at 840°C with a pushing speed of 36cm / min to obtain the bent pipe blank.
[0066] S4. Clean the weld seam of the above-mentioned bent pipe blank, and weld the cladding layer of the bent pipe blank to obtain a welded bent pipe.
[0067] S5. The furnace is heated to 950℃ in an empty furnace, and the above-mentioned welded bend is placed in it. It is then quenched at 945℃ and held for 45 minutes. After being water-cooled to 420℃, it is air-cooled to room temperature. The furnace is then heated to 945℃ in an empty furnace, and the quenched and cooled welded bend is placed in it. It is then normalized at 910℃ and held for 45 minutes. After being air-cooled to room temperature, a bimetallic composite bend with a diameter of Φ355.6×(12+3) is obtained.
[0068] Example 3
[0069] This embodiment provides a method for preparing a bimetallic composite bend, including the following steps:
[0070] S1. Mill the edges of the bimetallic composite plate (26+6) that has passed the re-inspection and quality test, use the X bevel for the butt weld, roll the tube to obtain the tube blank.
[0071] S2, the base layer and transition layer of the above-mentioned tube blank are welded sequentially to obtain a welded tube blank. The welding thickness of the transition layer is 5mm, and it is offset 3mm towards the base layer and 2mm towards the cladding layer, with the contact line between the base layer and the cladding layer as the center.
[0072] S3. Adjust the swing arm of the pipe bending machine to the 0° position, adjust the required bending radius, load the above-mentioned welded pipe blank onto the bending machine, position it, and perform hot bending at 900°C with a pushing speed of 30cm / min to obtain the bent pipe blank.
[0073] S4. Clean the weld seam of the above-mentioned bent pipe blank, and weld the cladding layer of the bent pipe blank to obtain a welded bent pipe.
[0074] S5. Heat the furnace to 970℃ in an empty oven, load the welded bend described above, and quench it at 970℃ for 60 minutes. Then, water-cool it to 457℃ and air-cool it to room temperature. Heat the furnace to 970℃ in an empty oven, load the quenched and cooled welded bend, and normalize it at 920℃ for 60 minutes. Then, air-cool it to room temperature to obtain a Φ711×(25+6) bimetallic composite bend (corresponding to a diameter of DN700).
[0075] Example 4
[0076] This embodiment provides a method for preparing a bimetallic composite bend, including the following steps:
[0077] S1. Mill the edges of the bimetallic composite plate (8+2) that has passed the re-inspection and quality test, use the X bevel for the butt weld, roll the tube to obtain the tube blank.
[0078] S2, the base layer and transition layer of the above-mentioned tube blank are welded sequentially to obtain a welded tube blank. The welding thickness of the transition layer is 3mm, with the contact line between the base layer and the cladding layer as the center, offset 2mm towards the base layer and 1mm towards the cladding layer.
[0079] S3. Adjust the swing arm of the pipe bending machine to the 0° position, adjust the required bending radius, load the above-mentioned welded pipe blank onto the bending machine, position it, and perform hot bending at 800°C with a pushing speed of 40cm / min to obtain the bent pipe blank.
[0080] S4. Clean the weld seam of the above-mentioned bent pipe blank, and weld the cladding layer of the bent pipe blank to obtain a welded bent pipe.
[0081] S5. The furnace is heated to 930℃ in an empty furnace, and the above-mentioned welded bend is placed in it. The bend is then quenched at 930℃ for 30 minutes, water-cooled to 402℃, and then air-cooled to room temperature. The furnace is then heated to 930℃ in an empty furnace, and the quenched and cooled welded bend is placed in it. The bend is then normalized at 880℃ for 30 minutes, and then air-cooled to room temperature to obtain a Φ168.3×(6+2) bimetallic composite bend.
[0082] Comparative Example 1
[0083] This comparative example provides a method for preparing a bimetallic composite bend, similar to Example 1, including the following steps:
[0084] S1 is the same as in Example 1, and will not be described again.
[0085] S2, the base layer, transition layer and cladding layer of the above tube blank are welded in sequence to obtain a welded tube blank.
[0086] S3, same as in Example 1, will not be described again. Bubbling and wrinkling occur in the multilayer, resulting in molding failure.
[0087] Comparative Example 2
[0088] This comparative example provides a method for preparing a bimetallic composite bend, similar to Example 1, including the following steps:
[0089] S1 to S4 are the same as in Example 1, and will not be described again.
[0090] S5. Heat the furnace to 1050℃ in an empty oven, load the above-mentioned welded bend into the furnace, quench it at 1050℃, hold it for 40 minutes, water cool it to 450℃, and then air cool it to room temperature. Heat the furnace to 950℃ in an empty oven, load the quenched and cooled welded bend into the furnace, normalize it at 900℃, hold it for 40 minutes, and then air cool it to room temperature to obtain a Φ355.6×(10+3) bimetallic composite bend.
[0091] Comparative Example 3
[0092] This comparative example provides a method for preparing a bimetallic composite bend, similar to Example 1, including the following steps:
[0093] S1 to S4 are the same as in Example 1, and will not be described again.
[0094] S5. Heat the furnace to 950℃ in an empty oven, load the above-mentioned welded bend into the furnace, quench it at 950℃ for 40 minutes, water cool it to 450℃, and then air cool it to room temperature. Heat the furnace to 700℃ in an empty oven, load the quenched and cooled welded bend into the furnace, temper it at 620℃ for 50 minutes, and then air cool it to room temperature to obtain a Φ355.6×(10+3) bimetallic composite bend.
[0095] Comparative Example 4
[0096] This comparative example provides a method for preparing a bimetallic composite bend, similar to Example 1, including the following steps:
[0097] S1 to S4 are the same as in Example 1, and will not be described again.
[0098] S5, heat the empty furnace to 950℃, put in the above-mentioned welded bend, normalize at 950℃, hold for 40 minutes, air cool to room temperature, and obtain a Φ355.6×(10+3) bimetallic composite bend.
[0099] Performance testing
[0100] To verify the performance of the bimetallic composite pipe bends, ferrite, hardness, and intergranular corrosion tests were conducted on the bimetallic composite pipe bends of Examples 1-4 and Comparative Examples 1-4. The test results are shown in Table 1. Table 1 shows that the ferrite content of the bimetallic composite pipe bends provided in the embodiments of the present invention is all below 8%, the hardness of the base layer is all below 231 HB, the hardness of the cladding layer is all below 190 HB, the tensile strength is all above 460 MPa, the yield strength is all above 360 MPa, and the elongation is all above 21%. No cracks caused by intergranular corrosion were found under a 10x magnifying glass, fully meeting production requirements. The hardness test results of the welded bends after quenching and cooling in Examples 1-4 show that the base layer hardness of the welded bends after quenching and cooling is relatively high (>231 HB). The embodiments of the present invention, through subsequent normalizing treatment (high-temperature heating, short holding time), reduce the base layer hardness of the bimetallic composite pipe and improve the overall performance of the bimetallic composite pipe.
[0101] Compared with Example 1, Comparative Example 1 first welded all the welds (base layer, transition layer and cladding layer) and then performed hot bending. Due to the difference in strength and elongation of the base layer and cladding layer materials of the bimetallic composite sheet, the base layer and cladding layer generated stress on each other during the forming process without any space for release. When the stress between the base layer and cladding layer was greater than the bonding force between the two, the cladding layer bulged and separated from the base layer, resulting in forming failure.
[0102] Compared with Example 1, the quenching temperature of Comparative Example 2 is higher, resulting in greater deformation of the base layer of the bimetallic composite bend and an increase in oxide scale. Although all indicators are qualified, it makes it difficult to obtain bimetallic composite bends with qualified appearance and mechanical properties (including plasticity and impact resistance).
[0103] Compared with Example 1, Comparative Example 3 underwent tempering after quenching, and the hardness of the bimetallic composite bend failed to meet the requirements.
[0104] Compared with Example 1, the heat treatment of Comparative Example 4 omitted the quenching process and only performed normalizing. Metallographic examination was conducted on the cladding of the bimetallic composite bends of Example 1 and Comparative Example 4, and the results are as follows. Figures 1-2 As shown in the figure, the metallographic structure of the cladding layer in Example 1 is austenitic, while the cladding layer in Comparative Example 4 contains a small amount of martensite. For the cladding layer (austenitic stainless steel) of the bimetallic composite bend, the austenitic structure is more suitable for the working conditions of the bimetallic composite bend.
[0105] Table 1. Performance test results of bimetallic composite pipe bends in the embodiments and comparative examples.
[0106]
[0107]
[0108]
[0109] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions or improvements made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A method for preparing a bimetallic composite bend, characterized in that, Includes the following steps: S1, mill the edges of the bimetallic composite sheet, use an X-groove for the butt weld, roll the tube to obtain a tube blank; the bimetallic composite sheet includes a base layer, a transition layer and a cladding layer; S2, Weld the base layer and transition layer of the tube blank to obtain a welded tube blank; S3, the welded tube blank is loaded into the bending machine, positioned, and hot-bent to obtain a bent tube blank; S4, weld the cladding layer of the bent pipe blank to obtain a welded bent pipe; S5, the welded bend is quenched at 930~970℃ and cooled; then normalized at 880~920℃ and cooled to obtain a bimetallic composite bend.
2. The method for preparing the bimetallic composite bend as described in claim 1, characterized in that, In step S1, the base layer of the bimetallic composite plate is carbon steel or pipeline steel, and the cladding layer of the bimetallic composite plate is austenitic stainless steel or nickel-based stainless steel.
3. The method for preparing the bimetallic composite bend as described in claim 1, characterized in that, The diameter of the bimetallic composite bend is DN150~DN700.
4. The method for preparing the bimetallic composite bend as described in claim 1, characterized in that, The thickness of the bimetallic composite bend is 8~30mm; wherein, the thickness of the base layer of the bimetallic composite bend is 6~25mm, and the thickness of the cladding layer of the bimetallic composite bend is 2~6mm.
5. The method for preparing the bimetallic composite bend as described in claim 1, characterized in that, In step S2, the welding thickness of the transition layer of the tube blank is 3~5mm.
6. The method for preparing the bimetallic composite bend as described in claim 1, characterized in that, In step S3, the hot bending forming is achieved by heating with a medium-frequency coil and cooling with water.
7. The method for preparing the bimetallic composite bend as described in claim 1, characterized in that, In step S3, the conditions for hot bending include: heating temperature of 800~1000℃ and pushing speed of 30~40cm / min.
8. The method for preparing the bimetallic composite bend as described in claim 1, characterized in that, In step S5, the furnace temperature for quenching is 930~970℃, and the holding time for quenching is 30~60min.
9. The method for preparing the bimetallic composite bend as described in claim 1, characterized in that, In step S5, the furnace temperature for the normalizing treatment is 930~970℃, and the holding time for the normalizing treatment is 30~60min.
10. A bimetallic composite bend, characterized in that, It is prepared by the method of any one of claims 1 to 9.
Citation Information
Patent Citations
Bimetal composite pipe fitting and preparation method thereof
CN117961446A
Bimetal composite tee joint and preparation method thereof
CN117961447A