A bio-based flame-retardant lithium-ion battery separator and preparation method thereof
Bio-based flame-retardant lithium-ion battery separators are prepared from materials such as modified cellulose and double-terminated vinyl phosphorus-containing polysiloxane, which solves the problems of spontaneous combustion and explosion safety hazards of lithium-ion batteries and achieves good heat resistance and flame retardancy. performance and improves the ionic conductivity of the battery separator.
Patent Information
- Application Number
- CN202410347989.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-26
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-03-26
AI Technical Summary
Lithium-ion batteries have potential safety risks of spontaneous combustion and explosion during charging and discharging. Existing separators cannot effectively avoid this problem and lack good flame retardant and heat-resistant properties.
Modified cellulose, double-ended vinyl phosphorus-containing polysiloxane and N,N-dimethylacetamide are used to prepare a casting liquid, and the bio-based flame-retardant lithium-ion battery separator is prepared by scraping and curing to form cross-links. The network structure and high thermal stability porous structure improve the heat resistance and flame retardant performance of the separator.
Significantly improves the heat resistance and flame retardant properties of the lithium-ion battery separator, ensuring stability in high temperature environments, improving ionic conductivity, and reducing the risk of battery short circuit.
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of electrical materials, and in particular to a bio-based flame-retardant lithium-ion battery separator and a preparation method thereof. Background Art
[0002] Lithium-ion batteries have high specific energy density, good cycle performance and environmental friendliness, making them widely used in electric vehicles, electronic products, energy storage and other fields. They are currently the most ideal power source energy storage system. As traditional nickel-metal hydride and nickel-cadmium batteries are gradually replaced, the public's demand for the charging and discharging rate and energy storage capacity of batteries in electronic devices is increasing day by day, but lithium-ion batteries often spontaneously combust or even explode. Therefore, how to avoid the safety hazards of lithium-ion batteries themselves has become the primary issue in the development of lithium battery technology.
[0003] As a storage medium for electrolytes, the porous structure of the battery separator provides an effective channel for the rapid conduction of lithium ions. It is one of the key components to prevent the positive electrode from directly contacting the negative electrode and causing a short circuit in the battery. Therefore, the development of a battery separator with good flame retardant effect and heat resistance has a huge market prospect. Summary of the invention
[0004] The object of the present invention is to provide a bio-based flame-retardant lithium-ion battery separator and a preparation method thereof, so as to solve the problems existing in the prior art.
[0005] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0006] A bio-based flame-retardant lithium-ion battery separator is prepared by mixing modified cellulose, double-terminal vinyl phosphorus-containing polysiloxane, N,N-dimethylacetamide and azobisisobutyronitrile to prepare a casting solution, and then scraping and curing the casting solution.
[0007] As an optimization, the modified cellulose is prepared by reacting microcrystalline cellulose with epichlorohydrin and then with dimethylallylamine.
[0008] As an optimization, the double-terminated vinyl phosphorus-containing polysiloxane is prepared by reacting allyl triphenylphosphine bromide and heptamethylcyclotetrasiloxane, and then reacting with a vinyl double-capped polysiloxane.
[0009] A method for preparing a bio-based flame-retardant lithium-ion battery separator comprises the following preparation steps:
[0010] (1) Mixing microcrystalline cellulose, epichlorohydrin and 10-20% sodium hydroxide solution uniformly, stirring at 20-30° C. and 200-300 r / min for 20-30 min, heating to 60-65° C. and continuing stirring for 6-8 h, centrifuging and washing with isopropanol for 3-5 times to obtain pre-modified cellulose; mixing pre-modified cellulose, dimethylallylamine and isopropanol in a mass ratio of 1:6-8:10-15 uniformly, stirring and refluxing at 70-80° C. and 200-300 r / min for 3-4 h, centrifuging and washing with pure water, 1% sodium hydroxide and 1% hydrochloric acid in turn, washing with pure water for 3-5 times, and drying at 70-80° C. for 10-12 h to obtain modified cellulose;
[0011] (2) mixing phosphorus-containing cyclotetrasiloxane and vinyl double end cap in a mass ratio of 1:0.03-0.04, adding 98% sulfuric acid with a mass fraction of 0.06-0.08 times the mass of phosphorus-containing cyclotetrasiloxane, stirring at 40-50° C. and 200-300 r / min for 8-10 hours, adding sodium bicarbonate to adjust the pH to 6.8-7.2, filtering and placing at 110-120° C. and 50-100 Pa for drying for 10-12 hours to obtain double-terminal vinyl phosphorus-containing polysiloxane;
[0012] (3) The modified cellulose, double-terminal vinyl phosphorus-containing polysiloxane and N,N-dimethylacetamide were uniformly mixed in a mass ratio of 1:0.3-0.4:5-6, and stirred at 200-300 r / min for 1-2 h at 20-30 ° C, and then 0.02-0.03 times the mass of the modified cellulose, azobisisobutyronitrile was added and continued to be stirred for 30-40 min to obtain a casting solution. The casting solution was scraped onto a flat plate and allowed to stand at 70 ° C for 10-12 h. After cooling to room temperature, it was peeled off to obtain a bio-based flame-retardant lithium-ion battery separator.
[0013] As an optimization, the model of the microcrystalline cellulose in step (1) is PH101.
[0014] As an optimization, the mass ratio of the microcrystalline cellulose, epichlorohydrin and 10-20% sodium hydroxide solution in step (1) is 1:20-25:20-25.
[0015] As an optimization, the preparation method of the phosphorus-containing cyclotetrasiloxane in step (2) is: allyl triphenylphosphine bromide and heptamethylcyclotetrasiloxane are added in a molar ratio of 1:1 to n-hexane with a mass of 12 to 16 times that of heptamethylcyclotetrasiloxane, and mixed evenly, and then 0.03 to 0.05 times the mass of heptamethylcyclotetrasiloxane of chloroplatinic acid is added, and the mixture is stirred and refluxed at 70 to 80° C. and 500 to 800 r / min for 4 to 6 hours, and then allowed to stand at 20 to 30° C. and 1 to 2 kPa for 30 to 40 minutes, and then allowed to stand at 20 to 30° C. and 1 to 2 kPa for 6 to 8 hours to prepare the product.
[0016] As an optimization, the preparation method of the bio-based additive in step (3) is: placing phytic acid and creatine in water with a molar ratio of 1:3 with a content of 10 to 12 times the mass of phytic acid, stirring the reaction at 50 to 60° C. for 4 to 6 hours, and drying at 70 to 80° C. and 1 to 2 kPa for 6 to 8 hours to prepare the bio-based additive.
[0017] As an optimization, the mass ratio of the modified cellulose, double-terminated vinyl phosphorus-containing polysiloxane and N,N-dimethylacetamide in step (3) is 1:0.3-0.4:5-6.
[0018] Compared with the prior art, the beneficial effects achieved by the present invention are:
[0019] When preparing a bio-based flame-retardant lithium-ion battery separator, the present invention mixes modified cellulose, double-terminal vinyl phosphorus-containing polysiloxane, N,N-dimethylacetamide and azobisisobutyronitrile to prepare a casting liquid, and the casting liquid is scraped and cured to obtain the bio-based flame-retardant lithium-ion battery separator.
[0020] Firstly, microcrystalline cellulose is reacted with epichlorohydrin and then with dimethylallylamine to obtain modified cellulose, double bonds are introduced into the microcrystalline cellulose, which is easy to participate in the subsequent polymerization of unsaturated bonds initiated by free radicals, thereby improving the formation of a cross-linked network structure, making the structural performance more stable, thereby improving the heat resistance; allyl triphenylphosphine bromide and heptamethylcyclotetrasiloxane are reacted, and then with a vinyl double-end to obtain a double-terminal vinyl phosphorus-containing polysiloxane, the phosphorus element and silicon oxygen structure in the double-terminal vinyl phosphorus-containing polysiloxane improve the flame retardant performance, and the polysiloxane segment in the double-terminal vinyl phosphorus-containing polysiloxane has very high thermal stability and oxidative stability, and can stably exist in a high temperature environment, thereby improving the heat resistance.
[0021] Secondly, the introduction of quaternary ammonium salt structure and triphenylphosphine bromide as ionic structures makes the bio-based flame-retardant lithium-ion battery separator have higher ionic conductivity; and the quaternary ammonium salt structure and triphenylphosphine bromide structure have the same charge, which can promote the dispersion of modified cellulose and double-terminal vinyl phosphorus-containing polysiloxane in the solution, and help to form a more uniform and dense three-dimensional network porous structure, thereby improving the ionic conductivity. DETAILED DESCRIPTION
[0022] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0023] In order to more clearly illustrate the method provided by the present invention, the following examples are described in detail.
[0024] Example 1
[0025] A method for preparing a bio-based flame-retardant lithium-ion battery separator, the method for preparing a bio-based flame-retardant lithium-ion battery separator mainly comprises the following preparation steps:
[0026] (1) Microcrystalline cellulose, epichlorohydrin and 10-20% sodium hydroxide solution are mixed in a mass ratio of 1:20:20, stirred at 20°C and 200 r / min for 30 min, heated to 60°C and continued to stir for 8 h, centrifuged and washed with isopropanol 3 times to obtain pre-modified cellulose, pre-modified cellulose, dimethylallylamine and isopropanol are mixed in a mass ratio of 1:6:10, stirred and refluxed at 70°C and 200 r / min for 4 h, centrifuged and washed with pure water, 1% sodium hydroxide and 1% hydrochloric acid respectively, washed with pure water 3 times, dried at 70°C for 12 h, and obtained modified cellulose;
[0027] (2) Allyl triphenylphosphine bromide and heptamethylcyclotetrasiloxane are added in a molar ratio of 1:1 to n-hexane (12 times the mass of heptamethylcyclotetrasiloxane) and mixed evenly, then 0.03 times the mass of heptamethylcyclotetrasiloxane of chloroplatinic acid is added, stirred and refluxed at 70°C, 500 r / min for 6 hours, allowed to stand at 20°C, 1 kPa for 40 minutes, and allowed to stand at 20°C, 1 kPa for 8 hours to obtain phosphorus-containing cyclotetrasiloxane; phosphorus-containing cyclotetrasiloxane and vinyl double-capped end are mixed evenly at a mass ratio of 1:0.03, then 0.06 times the mass of phosphorus-containing cyclotetrasiloxane is added with 98% sulfuric acid, stirred and reacted at 40°C, 200 r / min for 10 hours, then sodium bicarbonate is added to adjust the pH to 6.8, filtered and dried at 110°C, 50 Pa for 12 hours to obtain double-terminal vinyl phosphorus-containing polysiloxane;
[0028] (3) The modified cellulose, double-terminal vinyl phosphorus-containing polysiloxane and N,N-dimethylacetamide were mixed uniformly in a mass ratio of 1:0.3:5, stirred at 20°C and 200 r / min for 2 h, and then 0.02 times the mass of modified cellulose, azobisisobutyronitrile was added and stirred for 40 min to obtain a casting solution. The casting solution was scraped onto a flat plate and allowed to stand at 70°C for 10 h. After cooling to room temperature, it was peeled off to obtain a bio-based flame-retardant lithium-ion battery separator.
[0029] Example 2
[0030] A method for preparing a bio-based flame-retardant lithium-ion battery separator, the method for preparing a bio-based flame-retardant lithium-ion battery separator mainly comprises the following preparation steps:
[0031] (1) Microcrystalline cellulose, epichlorohydrin and 15% sodium hydroxide solution are mixed in a mass ratio of 1:22:22, stirred at 25°C and 250 r / min for 25 min, heated to 62°C and continued to stir for 7 h, centrifuged and washed with isopropanol 4 times to obtain pre-modified cellulose, pre-modified cellulose, dimethylallylamine and isopropanol are mixed in a mass ratio of 1:7:12, stirred and refluxed at 75°C and 250 r / min for 3.5 h, centrifuged and washed with pure water, 1% sodium hydroxide and 1% hydrochloric acid respectively, then washed with pure water 4 times, dried at 75°C for 11 h, and modified cellulose is obtained;
[0032] (2) Allyl triphenylphosphine bromide and heptamethylcyclotetrasiloxane are added in a molar ratio of 1:1 to n-hexane (14 times the mass of heptamethylcyclotetrasiloxane) and mixed evenly, then 0.04 times the mass of heptamethylcyclotetrasiloxane of chloroplatinic acid is added, stirred and refluxed at 75°C and 600 r / min for 5 hours, allowed to stand at 25°C and 1.5 kPa for 35 minutes, and allowed to stand at 25°C and 1.5 kPa for 7 hours to obtain phosphorus-containing cyclotetrasiloxane; phosphorus-containing cyclotetrasiloxane and vinyl double-capped end are mixed evenly at a mass ratio of 1:0.035, then 0.07 times the mass of phosphorus-containing cyclotetrasiloxane is added with 98% sulfuric acid (mass fraction), stirred and reacted at 45°C and 250 r / min for 9 hours, then sodium bicarbonate is added to adjust the pH to 7, filtered and dried at 115°C and 70 Pa for 11 hours to obtain double-terminal vinyl phosphorus-containing polysiloxane;
[0033] (3) The modified cellulose, double-terminal vinyl phosphorus-containing polysiloxane and N,N-dimethylacetamide were mixed uniformly in a mass ratio of 1:0.35:5.5, stirred at 25°C and 250 r / min for 1.5 h, and then 0.025 times the mass of the modified cellulose, azobisisobutyronitrile was added and stirred for 35 min to obtain a casting solution. The casting solution was scraped onto a flat plate and allowed to stand at 70°C for 11 h. After cooling to room temperature, it was peeled off to obtain a bio-based flame-retardant lithium-ion battery separator.
[0034] Example 3
[0035] A method for preparing a bio-based flame-retardant lithium-ion battery separator, the method for preparing a bio-based flame-retardant lithium-ion battery separator mainly comprises the following preparation steps:
[0036] (1) Microcrystalline cellulose, epichlorohydrin and 20% sodium hydroxide solution are mixed in a mass ratio of 1:25:25, stirred at 30°C and 300 r / min for 20 min, heated to 65°C and continued to stir for 6 h, centrifuged and washed with isopropanol 5 times to obtain pre-modified cellulose, pre-modified cellulose, dimethylallylamine and isopropanol are mixed in a mass ratio of 1:8:15, stirred and refluxed at 80°C and 300 r / min for 3 h, centrifuged and washed with pure water, 1% sodium hydroxide and 1% hydrochloric acid respectively, then washed with pure water 5 times, dried at 80°C for 10 h, and modified cellulose is obtained;
[0037] (2) Allyl triphenylphosphine bromide and heptamethylcyclotetrasiloxane are added in a molar ratio of 1:1 to n-hexane (16 times the mass of heptamethylcyclotetrasiloxane) and mixed evenly, then 0.05 times the mass of heptamethylcyclotetrasiloxane of chloroplatinic acid is added, stirred and refluxed at 80°C and 800 r / min for 4 hours, allowed to stand at 30°C and 2 kPa for 30 minutes, and allowed to stand at 30°C and 2 kPa for 6 hours to obtain phosphorus-containing cyclotetrasiloxane; phosphorus-containing cyclotetrasiloxane and vinyl double-capped end are mixed evenly at a mass ratio of 1:0.04, then 0.08 times the mass of phosphorus-containing cyclotetrasiloxane is added with 98% sulfuric acid (mass fraction), stirred and reacted at 50°C and 300 r / min for 8 hours, then sodium bicarbonate is added to adjust the pH to 7.2, filtered and dried at 120°C and 100 Pa for 10 hours to obtain double-terminal vinyl phosphorus-containing polysiloxane;
[0038] (3) The modified cellulose, double-terminal vinyl phosphorus-containing polysiloxane and N,N-dimethylacetamide were mixed uniformly in a mass ratio of 1:0.4:6, stirred at 30°C and 300 r / min for 1 h, and then 0.03 times the mass of modified cellulose, azobisisobutyronitrile was added and stirred for 30 min to obtain a casting solution. The casting solution was scraped onto a flat plate and allowed to stand at 70°C for 12 h. After cooling to room temperature, it was peeled off to obtain a bio-based flame-retardant lithium-ion battery separator.
[0039] Comparative Example 1
[0040] A method for preparing a bio-based flame-retardant lithium-ion battery separator, the method for preparing a bio-based flame-retardant lithium-ion battery separator mainly comprises the following preparation steps:
[0041] (1) Allyl triphenylphosphine bromide and heptamethylcyclotetrasiloxane are added to n-hexane (14 times the mass of heptamethylcyclotetrasiloxane) in a molar ratio of 1:1 and mixed evenly, then 0.04 times the mass of heptamethylcyclotetrasiloxane of chloroplatinic acid is added, stirred and refluxed at 75°C and 600 r / min for 5 hours, allowed to stand at 25°C and 1.5 kPa for 35 minutes, and allowed to stand at 25°C and 1.5 kPa for 7 hours to obtain phosphorus-containing cyclotetrasiloxane; phosphorus-containing cyclotetrasiloxane and vinyl double-capped end are mixed evenly in a mass ratio of 1:0.035, then 0.07 times the mass of phosphorus-containing cyclotetrasiloxane is added with 98% sulfuric acid, stirred and reacted at 45°C and 250 r / min for 9 hours, then sodium bicarbonate is added to adjust the pH to 7, filtered and dried at 115°C and 70 Pa for 11 hours to obtain double-terminal vinyl phosphorus-containing polysiloxane;
[0042] (2) Microcrystalline cellulose, double-terminated vinyl phosphorus-containing polysiloxane, and N,N-dimethylacetamide were uniformly mixed in a mass ratio of 1:0.35:5.5, stirred at 25°C and 250 r / min for 1.5 h, and then 0.025 times the mass of modified cellulose, azobisisobutyronitrile was added and stirred for 35 min to obtain a casting solution. The casting solution was scraped onto a flat plate and allowed to stand at 70°C for 11 h. After cooling to room temperature, it was peeled off to obtain a bio-based flame-retardant lithium-ion battery separator.
[0043] Comparative Example 2
[0044] A method for preparing a bio-based flame-retardant lithium-ion battery separator, the method for preparing a bio-based flame-retardant lithium-ion battery separator mainly comprises the following preparation steps:
[0045] (1) Microcrystalline cellulose, epichlorohydrin and 15% sodium hydroxide solution are mixed in a mass ratio of 1:22:22, stirred at 25°C and 250 r / min for 25 min, heated to 62°C and continued to stir for 7 h, centrifuged and washed with isopropanol 4 times to obtain pre-modified cellulose, pre-modified cellulose, dimethylallylamine and isopropanol are mixed in a mass ratio of 1:7:12, stirred and refluxed at 75°C and 250 r / min for 3.5 h, centrifuged and washed with pure water, 1% sodium hydroxide and 1% hydrochloric acid respectively, then washed with pure water 4 times, dried at 75°C for 11 h, and modified cellulose is obtained;
[0046] (2) octamethylcyclotetrasiloxane and vinyl double end cap were mixed uniformly in a mass ratio of 1:0.035, and then 0.07 times the mass of phosphorus-containing cyclotetrasiloxane was added with 98% sulfuric acid by mass, and the mixture was stirred at 45°C and 250 r / min for 9 hours, and then sodium bicarbonate was added to adjust the pH to 7, and the mixture was filtered and dried at 115°C and 70 Pa for 11 hours to obtain double-terminal vinyl polysiloxane;
[0047] (3) Modified cellulose, double-terminal vinyl polysiloxane and N,N-dimethylacetamide were mixed in a mass ratio of 1:0.35:5.5, stirred at 25°C and 250 r / min for 1.5 h, and then 0.025 times the mass of modified cellulose, azobisisobutyronitrile was added and stirred for 35 min to obtain a casting solution. The casting solution was scraped onto a flat plate and allowed to stand at 70°C for 11 h. After cooling to room temperature, it was peeled off to obtain a bio-based flame-retardant lithium-ion battery separator.
[0048] Comparative Example 3
[0049] A method for preparing a bio-based flame-retardant lithium-ion battery separator, the method for preparing a bio-based flame-retardant lithium-ion battery separator mainly comprises the following preparation steps:
[0050] (1) Microcrystalline cellulose, epichlorohydrin and 15% sodium hydroxide solution are mixed in a mass ratio of 1:22:22, stirred at 25°C and 250 r / min for 25 min, heated to 62°C and continued to stir for 7 h, centrifuged and washed with isopropanol 4 times to obtain pre-modified cellulose, pre-modified cellulose, dimethylallylamine and isopropanol are mixed in a mass ratio of 1:7:12, stirred and refluxed at 75°C and 250 r / min for 3.5 h, centrifuged and washed with pure water, 1% sodium hydroxide and 1% hydrochloric acid respectively, then washed with pure water 4 times, dried at 75°C for 11 h, and modified cellulose is obtained;
[0051] (2) The modified cellulose, vinyl double head and N,N-dimethylacetamide were mixed in a mass ratio of 1:0.35:5.5, stirred at 25°C and 250 r / min for 1.5 h, and then 0.025 times the mass of modified cellulose, azobisisobutyronitrile was added and stirred for 35 min to obtain a casting liquid. The casting liquid was scraped onto a flat plate and allowed to stand at 70°C for 11 h. After cooling to room temperature, it was peeled off to obtain a bio-based flame-retardant lithium-ion battery separator.
[0052] Test Example 1
[0053] Heat resistance and flame retardancy testing
[0054] Heat resistance test method: The bio-based flame-retardant lithium-ion battery separator obtained in each embodiment and comparative example is scraped to a thickness of 50 μm, cut into a circle with a diameter of 10 cm at 20°C, heated to 120°C and measured and calculated again. The heat shrinkage rate is calculated as 1-120°C area / 20°C area.
[0055] Flame retardant performance test method: The bio-based flame retardant lithium ion battery separator obtained in each example and the comparative example material were tested for limiting oxygen index according to ISO4589-2 standard. The results are shown in Table 1.
[0056] Table 1
[0057] Thermal shrinkage Limiting oxygen index Example 1 0.3% 35.3% Example 2 0.3% 35.8% Example 3 0.2% 36.2% Comparative Example 1 2.0% 35.6% Comparative Example 2 0.3% 30.8% Comparative Example 3 0.9% 28.1%
[0058] From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 3 in Table 1, it can be found that the bio-based flame retardant lithium ion battery separator prepared by the present invention has good heat resistance and flame retardancy.
[0059] By comparing the data of Examples 1 to 3 and Comparative Example 1, it can be found that the thermal shrinkage rates of Examples 1 to 3 are low, which indicates that the microcrystalline cellulose is modified and double bonds are introduced into the microcrystalline cellulose, which is easy to participate in the subsequent polymerization of unsaturated bonds initiated by free radicals, thereby improving the formation of a cross-linked network structure, making the structural performance more stable, thereby improving the heat resistance.
[0060] By comparing the data of Examples 1 to 3 and Comparative Example 2, it can be found that the limiting oxygen index of Examples 1 to 3 is high, which indicates that the double-terminal vinyl phosphorus-containing polysiloxane prepared by the reaction involving allyl triphenylphosphine bromide can obtain a better flame retardant effect.
[0061] By comparing the data of Examples 1 to 3 and Comparative Example 3, it can be found that Examples 1 to 3 have low thermal shrinkage and high limiting oxygen index; this indicates that the polysiloxane segment in the double-ended vinyl phosphorus-containing polysiloxane has very high thermal stability and oxidative stability, and can stably exist in a high temperature environment, thereby improving the heat resistance; the high limiting oxygen index is due to the same reasons as in Comparative Example 2, and the silicon content in the double-ended vinyl phosphorus-containing polysiloxane is higher than that in the vinyl double-end.
[0062] Test Example 2
[0063] Ionic conductivity test
[0064] Test method: The bio-based flame-retardant lithium-ion battery separators obtained in each embodiment and comparative example are cut into discs of the same size, and the lithium-ion electrolyte LB-302 is absorbed to saturation. The positive and negative electrodes are steel sheets, and the blocked cells are assembled. The assembled blocked cells are tested by an electrochemical workstation. The test method is AC impedance measurement (impedance-frequency scanning), wherein the test frequency range is 0.01 Hz to 100 KHz. The test data can be fitted to obtain the body impedance value R b Calculate ionic conductivity = membrane surface area / (R b * Diaphragm thickness). The results are shown in Table 2
[0065] Table 2
[0066] Ionic conductivity Ionic conductivity Example 1 2.13mS / cm Comparative Example 1 1.54mS / cm Example 2 2.18mS / cm Comparative Example 2 1.62mS / cm Example 3 2.19mS / cm Comparative Example 3 1.27mS / cm
[0067] From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 3 in Table 2, it can be found that the bio-based flame-retardant lithium-ion battery separator prepared by the present invention has good ionic conductivity.
[0068] By comparing the data of Examples 1 to 3 and Comparative Examples 1 to 3, it can be found that Examples 1 to 3 have high ionic conductivity, which indicates that the introduction of the quaternary ammonium salt structure and the triphenylphosphine bromide structure makes the bio-based flame-retardant lithium-ion battery separator have higher ionic conductivity; and the quaternary ammonium salt structure and the triphenylphosphine bromide structure have the same charge, which can promote the dispersion of modified cellulose and double-terminal vinyl phosphorus-containing polysiloxane in the solution, and help to form a more uniform and dense three-dimensional network porous structure, thereby improving the ionic conductivity.
[0069] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.
Claims
1. A method for preparing a bio-based flame-retardant lithium-ion battery separator, It is characterized in that The method comprises the following preparation steps: (1) mixing microcrystalline cellulose, epichlorohydrin and 10-20% by mass sodium hydroxide solution, stirring at 200-300 r / min at 20-30° C. for 20-30 min, heating to 60-65° C. and continuing stirring for 6-8 h, centrifuging and washing with isopropanol for 3-5 times to obtain pre-modified cellulose; Pre-modified cellulose, dimethylallylamine and isopropanol are mixed uniformly in a mass ratio of 1:6-8:10-15, stirred and refluxed at 70-80°C and 200-300r / min for 3-4h, centrifuged and washed with pure water, 1% sodium hydroxide and 1% hydrochloric acid in sequence, then washed with pure water for 3-5 times, and dried at 70-80°C for 10-12h to obtain modified cellulose; (2) Allyl triphenylphosphine bromide and heptamethylcyclotetrasiloxane are added in a molar ratio of 1:1 to n-hexane with a mass of 12 to 16 times that of heptamethylcyclotetrasiloxane, and mixed evenly, and then 0.03 to 0.05 times the mass of heptamethylcyclotetrasiloxane of chloroplatinic acid is added, and the mixture is stirred and refluxed at 70 to 80° C. and 500 to 800 r / min for 4 to 6 hours, and then allowed to stand at 20 to 30° C. and 1 to 2 kPa for 30 to 40 minutes, and then allowed to stand at 20 to 30° C. and 1 to 2 kPa for 6 to 8 hours to obtain phosphorus-containing cyclotetrasiloxane. Phosphorus-containing cyclotetrasiloxane and vinyl double-end are mixed evenly in a mass ratio of 1:0.03-0.04, and then 0.06-0.08 times the mass of phosphorus-containing cyclotetrasiloxane is added with 98% sulfuric acid, and the mixture is stirred at 40-50°C and 200-300r / min for 8-10h, and then sodium bicarbonate is added to adjust the pH to 6.8-7.2, and the mixture is filtered and placed at 110-120°C and 50-100Pa for drying for 10-12h to obtain double-end vinyl phosphorus-containing polysiloxane; (3) The modified cellulose, double-terminal vinyl phosphorus-containing polysiloxane and N,N-dimethylacetamide were uniformly mixed in a mass ratio of 1:0.3-0.4:5-6, and stirred at 200-300 r / min for 1-2 h at 20-30 ° C, and then 0.02-0.03 times the mass of the modified cellulose, azobisisobutyronitrile was added and continued to be stirred for 30-40 min to obtain a casting solution. The casting solution was scraped onto a flat plate and allowed to stand at 70 ° C for 10-12 h. After cooling to room temperature, it was peeled off to obtain a bio-based flame-retardant lithium-ion battery separator.
2. The method for preparing a bio-based flame-retardant lithium-ion battery separator according to claim 1, It is characterized in that The model of the microcrystalline cellulose in step (1) is PH101.
3. The method for preparing a bio-based flame-retardant lithium-ion battery separator according to claim 1, It is characterized in that The mass ratio of the microcrystalline cellulose, epichlorohydrin and 10-20% sodium hydroxide solution in step (1) is 1:20-25:20-25.
4. The method for preparing a bio-based flame-retardant lithium-ion battery separator according to claim 1, It is characterized in that In step (3), the mass ratio of the modified cellulose, double-terminal vinyl phosphorus-containing polysiloxane and N,N-dimethylacetamide is 1:0.3-0.4:5-6.
5. A bio-based flame retardant lithium-ion battery separator prepared according to the method for preparing a bio-based flame retardant lithium-ion battery separator according to any one of claims 1 to 4.