Method for selectively extracting lithium, aluminum-based lithium adsorption fiber, preparation method and application
Through the preparation of aluminum-based lithium adsorbed fibers, Li/Al-LDHs are synthesized in situ on the fiber surface using a mixed liquid of alumina sol and lithium-aluminum, which solves the complex process, low efficiency and cycle of existing lithium-ion sieves during lithium extraction. The problem of poor performance has achieved efficient lithium ion adsorption and desorption, improving the efficiency and selectivity of lithium extraction.
Patent Information
- Application Number
- CN202410049298.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-12
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-01-12
AI Technical Summary
The existing lithium ion sieves have complex processes, low lithium extraction efficiency and poor circulation during the lithium extraction process, resulting in high cost and low elution efficiency in neutral deionized water or low ionic strength solutions.
Aluminum-based lithium adsorbent fiber is used to soak the fiber material in a hydrocarbamate sol and react with a mixed liquid of lithium aluminum to form aluminum lithium adsorbent fibers. The Li/Al-LDHs material is synthesized in situ on the surface of the fibers by combining co-precipitation method. Achieve selective adsorption and desorption of lithium ions.
The lithium extraction process is simplified, and the selectivity and lithium extraction efficiency of lithium ions are improved. The lithium ion adsorption capacity reaches 14.74 mg/g. It remains 13.71 mg/g after 10 cycles, and it is manifested in a multi-ion system where lithium-magnesium coexistence is performed. Excellent adsorption performance.
Smart Images

Figure CN118222851B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to lithium extraction, and in particular to a method for selectively extracting lithium, aluminum-based lithium adsorption fiber, a preparation method and application thereof. Background Art
[0002] Lithium and its compounds are widely used in lithium-ion batteries, new energy vehicles and other fields. In recent years, the new energy industry has experienced explosive growth, and the demand for lithium resources has continued to increase, resulting in a serious imbalance between domestic supply and demand. Salt lake brine contains abundant resources such as lithium and magnesium. Moreover, the cost of extracting lithium from brine is lower than that from ore, which can avoid the high energy consumption and high pollution problems caused by mining and smelting. However, lithium ions will still remain in the old brine after potassium extraction, so that lithium resources are not fully utilized.
[0003] The Chinese invention patent application with publication number CN111139356A describes a method for extracting lithium from lithium-containing low-magnesium brine, which comprises CaO, water and excess Na 2 CO 3 The mixture was mixed and reacted, and the obtained reaction solution was filtered to obtain an alkaline solution and CaCO 3 Solid; add alkaline solution to lithium-containing low-magnesium brine, gradually adjust the pH of lithium-containing low-magnesium brine to above 11, and precipitate basic magnesium carbonate and Mg(OH) 2 The method comprises the following steps: precipitating to obtain a lithium-containing brine after magnesium removal; extracting lithium from the lithium-containing brine after magnesium removal by using a composite organic extraction system to obtain a loaded organic phase and a raffinate; mixing the loaded organic phase with an acidic aqueous solution, and stripping the lithium from the loaded organic phase into an aqueous phase to obtain a lithium-containing aqueous solution and a lithium-depleted organic phase.
[0004] Although the above patent application can extract lithium from lithium-containing low-magnesium brine; however, the extraction method used to extract lithium will complicate the process and is not conducive to industrial operation. In order to achieve one-step lithium extraction, the current research direction in the field of lithium extraction is mainly focused on lithium ion sieve adsorption and lithium extraction. Commonly used lithium ion sieves are manganese-based and titanium-based lithium ion sieves; however, since the lithium ion sieve uses acid to remove lithium, the lattice structure is distorted and dissolved, and Mn / Ti is dissolved during the lithium removal process, resulting in poor lithium extraction cyclicity and high cost. Although hydrotalcite-like enriched materials can be easily eluted in neutral deionized water or low ionic strength solutions without dissolving; however, their lithium extraction efficiency is not outstanding.
[0005] In view of this, it is necessary to provide a method for selectively extracting lithium, an aluminum-based lithium adsorption fiber, a preparation method and an application, so as to solve or at least alleviate the technical defects of the above-mentioned prior art, such as complex procedures, low lithium extraction efficiency and poor recyclability. Summary of the invention
[0006] The main purpose of the present invention is to provide a method for selectively extracting lithium, aluminum-based lithium adsorption fiber, preparation method and application, aiming to solve the technical problems of complex procedures, low lithium extraction efficiency and poor recyclability in the above-mentioned prior art.
[0007] To achieve the above object, the present invention provides a method for selectively extracting lithium, comprising the steps of:
[0008] S1, obtaining a liquid to be extracted, wherein the liquid to be extracted contains Li + ;
[0009] S2, performing lithium extraction treatment on the liquid to be extracted;
[0010] The lithium extraction process comprises: mixing aluminum-based lithium adsorbing fibers into the solution to be extracted to obtain a first treatment solution; then, performing a first mixing operation on the first treatment solution to remove Li + Adsorbing into the aluminum-based lithium adsorption fiber to obtain a lithium extraction product;
[0011] The preparation process of the aluminum-based lithium adsorption fiber includes: soaking the fiber material in diaspore sol to obtain a precursor material; reacting the precursor material with a lithium-aluminum mixed solution at 80-90° C. for 18-30 hours to obtain an intermediate material; aging the intermediate material to obtain the aluminum-based lithium adsorption fiber; wherein the mass volume ratio of the precursor material to the lithium-aluminum mixed solution is 0.1-0.5 g: 50-150 mL, and the molar ratio of lithium ions to aluminum ions in the lithium-aluminum mixed solution is 1: 1-1.3;
[0012] S3, delithiation treatment of the lithium extraction product in a neutral solution to obtain a lithium-rich solution.
[0013] Furthermore, the Li + The concentration of Mg is 0.2-60mmol / L, the pH of the extract is 5.5-8; the extract also contains Mg 2+ , Ca 2+ 、Na + , K + , B 3+ One or more of .
[0014] Furthermore, the first mixing operation has a rotation speed of 50-200 rpm and a duration of 1-5 hours.
[0015] Furthermore, the neutral solution includes water or lithium chloride solution, and the concentration of lithium ions in the lithium chloride solution is not higher than 0.5 mmol / L;
[0016] The lithium removal treatment includes: mixing the lithium extraction product into the neutral solution to obtain a second treatment liquid; then performing a second mixing operation on the second treatment liquid to remove the lithium element in the lithium extraction product; wherein the rotation speed of the second mixing operation is 50-200rpm and the duration is 0.5-1.5h.
[0017] Furthermore, the fiber material includes one or more of polyacrylonitrile fiber, polyvinyl chloride fiber, and polyvinylidene fluoride fiber.
[0018] Furthermore, the method for obtaining the diaspore sol includes: performing a third mixing operation on diaspore powder and a dispersant to obtain a pretreatment liquid, wherein the dispersant includes water; dropping a nitric acid solution into the pretreatment liquid, and performing a fourth mixing operation on the nitric acid solution and the pretreatment liquid to obtain the diaspore sol;
[0019] The mass percentage of the diaspore powder and the dispersant is 5-8%, the concentration of nitric acid in the nitric acid solution is 1.5-2.5 mol / L, and the molar ratio of the nitric acid to the aluminum ion in the diaspore is 0.4-0.6:1;
[0020] The third mixing operation and the fourth mixing operation are both performed at 60-80° C., the third mixing operation lasts for 0.5-2 h, and the fourth mixing operation lasts for 3-6 h.
[0021] Furthermore, the method for obtaining the lithium aluminum mixed solution comprises: + and Al 3+ An alkaline solution is added dropwise to the ion mixed solution until the pH of the ion mixed solution is 5.3-5.8 to obtain the lithium aluminum mixed solution; during the process of adding the alkaline solution dropwise, the temperature of the ion mixed solution is maintained at 60-80°C.
[0022] The present invention also provides a method for preparing aluminum-based lithium-absorbed fibers, comprising: soaking a fiber material in a diaspore sol to obtain a precursor material; reacting the precursor material with a lithium-aluminum mixed solution at 80-90° C. for 18-30 hours to obtain an intermediate material; aging the intermediate material to obtain the aluminum-based lithium-absorbed fibers;
[0023] The mass volume ratio of the precursor material to the lithium aluminum mixed solution is 0.1-0.5 g: 50-150 mL, and the molar ratio of lithium ions to aluminum ions in the lithium aluminum mixed solution is 1: 1-1.3.
[0024] The present invention also provides an aluminum-based lithium adsorbing fiber, which is prepared by any of the preparation methods described above.
[0025] The present invention also provides a use of any of the aluminum-based lithium adsorption fibers described above in extracting lithium.
[0026] Compared with the prior art, the present invention has at least the following advantages:
[0027] The present invention can simplify the lithium extraction process; the present invention comprises: + Aluminum-based lithium adsorption fibers are mixed into the liquid to be extracted and an oscillation operation is performed to separate and extract lithium from the liquid to be extracted; the lithium extraction product is then de-lithiated in a neutral solution to obtain a lithium-rich solution.
[0028] The present invention has excellent lithium extraction efficiency and lithium ion selectivity; moreover, the present invention can also perform cyclic lithium extraction based on aluminum-based lithium adsorption fibers; specifically, the lithium ion adsorption capacity of the present invention can reach 14.74 mg / g, and the lithium ion adsorption capacity after 10 cycles can still reach 13.71 mg / g; even in a multi-ion system where lithium and magnesium coexist, the lithium ion adsorption capacity of the present invention can reach 12.61 mg / g, while the magnesium ion adsorption capacity is only 0.7 mg / g. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.
[0030] Figure 1 This is a scanning electron microscope (SEM) image of the product prepared in Example 1 of the present invention magnified 20,000 times;
[0031] Figure 2 is the XRD pattern of the product prepared in Example 1 of the present invention;
[0032] Figure 3 This is a graph showing the adsorption data of lithium ions in Example 2 of the present invention;
[0033] Figure 4 This is a scanning electron microscope (SEM) image of the product prepared in Comparative Example 1 of the present invention magnified 30,000 times;
[0034] Figure 5 This is the XRD pattern of the product prepared in Comparative Example 1 of the present invention;
[0035] Figure 6 This is a scanning electron microscope (SEM) image of the product prepared in Comparative Example 2 of the present invention magnified 30,000 times;
[0036] Figure 7This is the XRD diagram of the product prepared in Comparative Example 2 of the present invention;
[0037] Figure 8 This is a scanning electron microscope (SEM) image of the product prepared in Comparative Example 3 of the present invention, magnified 30,000 times.
[0038] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with the implementation methods and with reference to the accompanying drawings. DETAILED DESCRIPTION
[0039] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0040] Furthermore, the technical solutions between the various embodiments of the present invention may be combined with each other, but this must be based on the fact that they can be implemented by ordinary technicians in the field. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such combination of technical solutions does not exist and is not within the scope of protection required by the present invention.
[0041] The present invention provides a method for selectively extracting lithium, comprising the steps of:
[0042] S1, obtaining a liquid to be extracted, wherein the liquid to be extracted contains Li + .
[0043] The Li + The concentration of can be 0.2-60mmol / L, specifically 10-20mmol / L; the pH of the extract can be 5.5-8, preferably 6-8; the extract can also contain Mg 2+ , Ca 2+ 、Na + , K + , B 3+ For example, the extract may also contain 0.001-10 mol / L Mg 2+ ; The liquid to be extracted can be lithium-containing brine.
[0044] S2, performing lithium extraction treatment on the liquid to be extracted.
[0045] The lithium extraction treatment includes: mixing aluminum-based lithium adsorption fibers into the liquid to be extracted to obtain a first treatment liquid; the amount of the aluminum-based lithium adsorption fibers can be adjusted according to actual conditions; illustratively, the mass volume ratio of the aluminum-based lithium adsorption fibers and the first treatment liquid can be 0.1-30g / L; specifically, it can be 0.05g:50mL; the aluminum-based lithium adsorption fibers can generally be in a film shape.
[0046] After obtaining the first treatment liquid, a first mixing operation is performed on the first treatment liquid to separate the Li + Adsorbed into the aluminum-based lithium adsorption fiber to obtain a lithium extraction product; wherein, the first mixing operation refers to stirring or flowing the first treatment liquid; the rotation speed of the first mixing operation is 50-200rpm, and the duration is 1-5h.
[0047] It should be noted that, by subjecting the first treatment liquid to the first mixing operation, the aluminum-based lithium adsorption fiber can adsorb lithium ions in the liquid to be extracted; after completing the first mixing operation, the product of the first mixing operation is usually required to undergo a solid-liquid separation operation to obtain a separated liquid and the lithium extraction product, wherein the separated liquid is the liquid obtained by separating the liquid to be extracted after completing the lithium extraction treatment; the lithium extraction product is the aluminum-based lithium adsorption fiber on which lithium ions (derived from the liquid to be extracted) are adsorbed.
[0048] It should also be noted that the preparation process of the aluminum-based lithium adsorption fiber includes: soaking the fiber material (the fiber material can usually be in the form of a film) in diaspore sol (AlOOH sol) to obtain a precursor material; reacting the precursor material and a lithium-aluminum mixed solution at 80-90°C for 18-30h to obtain an intermediate material, and the reaction of the precursor material and the lithium-aluminum mixed solution is usually carried out in a reactor, which is equivalent to a hydrothermal reaction; aging the intermediate material to obtain the aluminum-based lithium adsorption fiber; wherein the mass volume ratio of the precursor material and the lithium-aluminum mixed solution is 0.1-0.5g:50-150mL, the lithium-aluminum mixed solution can be a mixed solution of lithium chloride and aluminum chloride, and the molar ratio of lithium ions to aluminum ions in the lithium-aluminum mixed solution is 1:1-1.3.
[0049] S3, delithiation treatment of the lithium extraction product in a neutral solution to obtain a lithium-rich solution and the aluminum-based lithium adsorption fiber; the amount of the neutral solution may not be specifically limited, as long as it can at least cover the lithium extraction product; the neutral solution may include water or lithium chloride solution, and the concentration of lithium ions in the lithium chloride solution is not higher than 0.5mmol / L.
[0050] It should be noted that the lithium extraction product is subjected to the lithium removal treatment in a neutral solution, so that the lithium ions adsorbed in the aluminum-based lithium adsorption fiber can be desorbed (derived from the solution to be extracted), thereby completing the extraction of lithium ions in the solution to be extracted, and making the aluminum-based lithium adsorption fiber reusable after the desorption treatment. Therefore, after the lithium removal treatment is completed, the product of the lithium removal treatment can be subjected to a solid-liquid separation operation, thereby separating the lithium-rich solution and the recyclable aluminum-based lithium adsorption fiber.
[0051] It should also be noted that the lithium removal treatment may include: mixing the lithium extraction product into the neutral solution to obtain a second treatment solution; and then performing a second mixing operation on the second treatment solution to remove the lithium element from the lithium extraction product. The second mixing operation refers to stirring or flowing the second treatment solution; the speed of the second mixing operation is 50-200 rpm and the duration is 0.5-1.5 hours.
[0052] The present invention also provides a method for preparing aluminum-based lithium adsorbing fibers, comprising: immersing a fiber material in a diaspore sol (AlOOH sol) to obtain a precursor material; reacting the precursor material and a lithium-aluminum mixed solution at 80-90° C. for 18-30 hours to obtain an intermediate material; aging the intermediate material to obtain the aluminum-based lithium adsorbing fibers; wherein the mass volume ratio of the precursor material to the lithium-aluminum mixed solution is 0.1-0.5 g: 50-150 mL, the lithium-aluminum mixed solution can be a mixed solution of lithium chloride and aluminum chloride, and the molar ratio of lithium ions to aluminum ions in the lithium-aluminum mixed solution is 1:1-1.3.
[0053] It should be pointed out that lithium aluminum double hydroxide (Li / Al-LDHs) is a powder and is usually granulated before use. This process will cause part of the powder to be buried and unable to function, and the loss of adsorption capacity before and after granulation is about 40%; and even the ungranulated lithium aluminum double hydroxide powder has a need to improve its adsorption capacity. However, the carrier materials currently used, such as activated carbon, cannot solve the problem of uniform dispersion on its surface, causing carbon pores to be blocked, which reduces the reaction activity; and the lithium adsorption capacity of the current industrial aluminum-based lithium adsorbent is only one-tenth of that of the lithium ion sieve. The limited adsorption capacity is the main reason that hinders the application and promotion of aluminum-based lithium adsorbents. Therefore, how to obtain a suitable carrier, and how to combine lithium aluminum double hydroxide to a suitable carrier and make it play an excellent lithium ion adsorption performance are the main difficulties faced in the research process. The present invention overcomes the above technical difficulties, so that Li / Al-LDHs are evenly distributed on the fiber surface, have a developed pore structure, and can effectively adsorb and desorb lithium ions.
[0054] In the present invention, in order to ensure that an aluminum-based lithium-absorbing fiber that can absorb lithium ions can be obtained, the fiber material can be a nanofiber; the fiber material can include one or more of polyacrylonitrile fiber, polyvinyl chloride fiber, and polyvinylidene fluoride fiber. Specifically, the aluminum-based lithium-absorbing fiber can include one or more of polyacrylonitrile (PAN), polyvinyl chloride (PVC), and polyvinylidene fluoride (PVDF) prepared by electrospinning.
[0055] In the present invention, the fiber material is immersed in the diaspore sol, and the lithium-aluminum mixed solution is used to synthesize Li / Al-LDHs material in situ on the surface of the fiber material through a co-precipitation method in combination with reaction temperature and time; the fiber material, as a high specific surface area carrier, effectively expands the contact area between Li / Al-LDHs and target lithium ions, thereby improving the lithium adsorption capacity of the material.
[0056] It should be noted that only by using the diaspore sol as a primer and the lithium-aluminum mixed solution as a reaction solution can the surface of the aluminum-based lithium adsorption fiber have in-situ self-grown Li / Al-LDHs hydrotalcite, thereby ensuring the acquisition of the aluminum-based lithium adsorption fiber. If the fiber material is directly reacted in the lithium-aluminum mixed solution, or the aluminum ions in the lithium-aluminum mixed solution are omitted, a stable Li / Al-LDHs hydrotalcite structure cannot be formed on the fiber surface, and the lithium extraction effect cannot be achieved.
[0057] In the present invention, the method for obtaining the diaspore sol may include: performing a third mixing operation on diaspore powder and a dispersant to obtain a pretreatment liquid, wherein the dispersant includes water; dropping a nitric acid solution into the pretreatment liquid, and performing a fourth mixing operation on the nitric acid solution and the pretreatment liquid to obtain the diaspore sol; the dropping rate of the nitric acid solution may be 1-3 mL / min.
[0058] In the present invention, the diaspore may include one or more of boehmite and pseudo-boehmite; the mass percentage of the diaspore powder and the dispersant is 5-8%, the concentration of nitric acid in the nitric acid solution is 1.5-2.5 mol / L, and the molar ratio of the nitric acid to the aluminum in the diaspore is 0.4-0.6:1, preferably 0.5-0.6:1; the third mixing operation and the fourth mixing operation are both carried out at 60-80°C, the duration of the third mixing operation is 0.5-2h, the duration of the fourth mixing operation is 3-6h, and the rotation speed of the third mixing operation and the fourth mixing operation can both be 100-200rpm.
[0059] It has been found through research that by controlling the solid content of diaspore in the diaspore sol, it is beneficial to obtain a fiber material with a high porosity ratio and help improve the lithium adsorption capacity of the obtained fiber material. When the solid content is too large, the gel is agglomerated on the fiber surface, and the lithium adsorption capacity is reduced. When the solid content is too small, Li / Al-LDHs cannot be synthesized on the fiber surface, and the lithium adsorption capacity is reduced. Therefore, the solid content of diaspore in the diaspore sol needs to be controlled at 5-8%, and the solid content of diaspore in the diaspore sol corresponds to the mass percentage of the diaspore powder and the dispersant.
[0060] In the present invention, the method for obtaining the lithium aluminum mixed solution may include: + and Al 3+ Add an alkaline solution to the ion mixed solution until the pH of the ion mixed solution is 5.3-5.8 to obtain the lithium aluminum mixed solution. The alkaline solution may include one or more of sodium hydroxide and potassium hydroxide. In addition, during the process of adding the alkaline solution, the temperature of the ion mixed solution is maintained at 60-80°C, so that aluminum ions and lithium ions can co-precipitate to form a layered material. Note: Room temperature cannot promote the lithium aluminum metal co-precipitation process. During the process of adding the alkaline solution, the ion mixed solution can be kept in a stirring state. Among them, Li + Can be derived from lithium chloride and Al 3+ It can be derived from aluminum chloride. The concentration of the alkaline substance in the alkaline solution can be 0.5-1.5 mol / L; the dropping rate of the alkaline solution can be 4-6 mL / min.
[0061] In the present invention, the soaking treatment may include: soaking the fiber material in the diaspore sol for multiple times and drying it for multiple times, each soaking time is 5-10 minutes, the total soaking time can be 15-30 minutes, and the drying can be natural drying, and the time for each natural drying can be 8-15 minutes; specifically, the soaking and the drying are performed alternately. It can be understood by those skilled in the art that during the soaking process, the fiber material is usually immersed in a large amount of the diaspore sol to achieve complete coverage of the fiber material by the diaspore sol, and therefore, the ratio of the fiber material to the diaspore sol does not need to be specifically limited.
[0062] The aging treatment may include: drying the intermediate material at 70-80° C. for 12 to 18 hours; that is, in the present invention, the aging treatment operation process may be understood as a drying process, thereby achieving aging of the aluminum-based lithium adsorption fiber.
[0063] The present invention also provides an aluminum-based lithium adsorbing fiber, which is prepared by any of the above-mentioned methods for preparing the aluminum-based lithium adsorbing fiber.
[0064] The present invention also provides an application of any of the aluminum-based lithium adsorption fibers described above in extracting lithium. In addition to the lithium extraction method shown in the present invention, the aluminum-based lithium adsorption fiber can also be used as a filter medium to allow the liquid to be extracted to pass through the aluminum-based lithium adsorption fiber, thereby obtaining the lithium extraction product.
[0065] The following are specific examples of the present invention:
[0066] Example 1
[0067] 1. Preparation of adsorption materials:
[0068] 1. Obtaining diaspore sol (AlOOH sol): Disperse diaspore powder in pure water at a solid content of 7% (i.e., the mass percentage of diaspore powder and pure water is 7%), and heat and stir at 70°C for 60 minutes, with a stirring speed of 120 rpm, to obtain a pretreatment solution. Subsequently, a nitric acid solution with a concentration of 2 mol / L is slowly added to the pretreatment solution at a rate of 2 mL / min, with a molar ratio of nitric acid to aluminum in diaspore being 0.5; after the addition is completed, continue to heat and stir at 70°C at a speed of 120 rpm for 4 hours, and then cool to room temperature to obtain diaspore sol.
[0069] 2. Obtaining precursor materials: completely immerse the film-like polyacrylonitrile fiber in the diaspore sol, then take it out and dry it; the immersion time is 5 minutes, and the drying time is 10 minutes; repeat the above immersion and drying operations in the original diaspore sol, the number of immersion and drying operations is 3 times, and the precursor material is obtained.
[0070] 3. Obtain a lithium-aluminum mixed solution: dissolve 0.1 mol of lithium chloride and 0.125 mol of aluminum chloride in 100 mL of pure water to obtain an ion mixed solution; slowly add a 1 mol / L sodium hydroxide solution to the ion mixed solution at a rate of 5 mL / min until the pH of the solution is 5.5 to obtain a lithium-aluminum mixed solution; and in the process of adding the sodium hydroxide solution, maintain the temperature of the ion mixed solution at 70°C, and stir the ion mixed solution at a speed of 120 rpm.
[0071] 4. Obtain the adsorption material: react 0.1 g of the precursor material with 100 mL of a lithium-aluminum mixed solution in a reactor at 85°C for 24 hours to obtain an intermediate material; use ethanol to remove excess solution on the intermediate material, and then age the intermediate material at 70°C for 12 hours to obtain a prepared product (aluminum-based lithium adsorption fiber material) used as an adsorption material.
[0072] In this embodiment, refer to Figure 1As shown, the surface of the aluminum-based lithium adsorbed fiber has in-situ self-grown Li / Al-LDHs hydrotalcite, and Li / Al-LDHs is uniformly distributed on the fiber surface.
[0073] Reference Figure 2 As shown in the XRD results, after comparison with the standard PDF card, it was confirmed that the attachment on the surface of the aluminum-based lithium adsorption fiber was Li / Al-LDHs.
[0074] In this embodiment, the specific surface area of the prepared product was measured to be 177 cm 2 / g.
[0075] 2. Static adsorption of lithium ions:
[0076] 0.05 g of the prepared product of this example was weighed as an adsorption material, and added to 50 mL of a simulated solution at room temperature to carry out a static adsorption test to obtain a lithium extraction product.
[0077] The simulated solution is lithium chloride solution. + The initial concentration was 100 mg / L (about 14.3 mmol / L), and the pH of the simulated solution was 6.5. The adsorption test was carried out under room temperature oscillation conditions with an oscillation speed of 100 rpm. The adsorption time was 4 h.
[0078] In this embodiment, after 4 hours of adsorption, the aluminum-based lithium adsorption fiber is + The adsorption amount is 14.74 mg / g.
[0079] 3. Aluminum-based lithium adsorption fiber recycling:
[0080] The lithium extraction product obtained by adsorption for 4 hours was placed in 100 mL of a lithium chloride solution with a concentration of 0.01 mmol / L, and desorbed by oscillation at room temperature. The oscillation speed was 100 rpm, the desorption time was 60 minutes, and the desorption efficiency was 99.9%.
[0081] After desorption, the solid-liquid separation was performed to obtain a lithium-rich solution and aluminum-based lithium adsorption fibers. The aluminum-based lithium adsorption fibers were dried and put into the next adsorption cycle (same as the second part of this embodiment). After 10 adsorptions and 10 desorption cycles, the aluminum-based lithium adsorption fibers were regenerated to have a high adsorption capacity. + The 4h adsorption capacity is 13.71mg / g.
[0082] Example 2
[0083] 1. Obtain a first comparative material (denoted as NF): Take a film-like polyacrylonitrile fiber (same as in Example 1) as the first comparative material.
[0084] 2. Obtain a second comparative material (denoted as LDHs): dissolve 0.1 mol lithium chloride and 0.125 mol aluminum chloride in 100 mL of pure water to obtain an ion mixed solution; slowly add a 1 mol / L sodium hydroxide solution to the ion mixed solution at a rate of 5 mL / min until the pH of the solution is 5.5 to obtain a lithium aluminum mixed solution; and in the process of adding the sodium hydroxide solution, maintain the temperature of the ion mixed solution at 70°C, and stir the ion mixed solution at a speed of 120 rpm.
[0085] The lithium aluminum mixed solution was transferred to a reactor and reacted at 85° C. for 24 h, followed by solid-liquid separation by suction filtration and aging at 70° C. for 12 h to obtain Li / Al-LDHs powder (second comparative material).
[0086] 3. Obtain test materials (referred to as LDHs NF): Take the product prepared in Example 1 as the test material.
[0087] 4. The first comparative material, the second comparative material and the test material are respectively used as the test substances for static adsorption test, as follows:
[0088] Weigh 0.05 g of the substance to be tested and add it to 50 mL of simulated solution at room temperature for a static adsorption test to obtain a lithium extraction product.
[0089] The simulated solution is a lithium chloride solution with a preset Li + Initial concentration, pH of the simulated solution was 6.5; the adsorption test was carried out under room temperature oscillation conditions, the oscillation speed was 100 rpm; the adsorption time was 4 h.
[0090] In this embodiment, the preset Li + The initial concentrations are 10 mg / L, 20 mg / L, 50 mg / L, 80 mg / L, and 100 mg / L. + Static adsorption tests were carried out on each substance to be tested at the initial concentration.
[0091] The test results of this embodiment are as follows Figure 3 As shown, it can be seen that: as Li + With the increase of Li concentration, LDHs and LDHs NF + The adsorption amount increases accordingly. When Li + When the initial concentration reaches 100 mg / L, the adsorption amount reaches the peak value; + Li at concentration + The adsorption amount was less than 0.1 mg / g, so it was not Figure 3 Listed in.
[0092] The effects of unmodified fiber membrane (NF), Li / Al-LDHs particles (LDHs) and fiber membrane with Li / Al-LDHs particles (LDHs NF) on Li + It can be seen from the adsorption effect that loading LDHs particles on the fiber surface can significantly increase the + adsorption capacity.
[0093] Example 3
[0094] 1. Preparation of adsorption materials:
[0095] Compared with Example 1, the only difference is that in the process of obtaining the diaspore sol, the solid content of the boehmite powder is adjusted to 5% (that is, the mass percentage of the boehmite powder and pure water is 5%), and the other conditions are the same as Example 1.
[0096] In this embodiment, the specific surface area of the prepared product (aluminum-based lithium adsorbing fiber material) was measured to be 149 cm 2 / g.
[0097] 2. Static adsorption of lithium ions:
[0098] Compared with Example 1, the only difference is that the prepared product of this example is used as the adsorption material, and the other conditions are the same as Example 1.
[0099] In this embodiment, after 4 hours of adsorption, the aluminum-based lithium adsorption fiber is + The adsorption capacity is 13.96 mg / g.
[0100] 3. Aluminum-based lithium adsorption fiber recycling:
[0101] Compared with Example 1, the only difference is that the lithium extraction product obtained by adsorption for 4 hours in this example is used for desorption and recycling, and other conditions are the same as in Example 1.
[0102] In this embodiment, after 10 cycles of adsorption and 10 cycles of desorption, the aluminum-based lithium adsorption fiber is + The 4h adsorption capacity is 13.13mg / g.
[0103] Example 4
[0104] 1. Preparation of adsorption materials:
[0105] Compared with Example 1, the only difference is that in the process of obtaining the precursor material, the polyacrylonitrile fiber is adjusted to polyvinyl chloride fiber, and the other conditions are the same as Example 1.
[0106] In this embodiment, the specific surface area of the prepared product (aluminum-based lithium adsorbing fiber material) was measured to be 136 cm 2 / g.
[0107] 2. Static adsorption of lithium ions:
[0108] Compared with Example 1, the only difference is that the prepared product of this example is used as the adsorption material, and the other conditions are the same as Example 1.
[0109] In this embodiment, after 4 hours of adsorption, the aluminum-based lithium adsorption fiber is + The adsorption capacity is 12.25 mg / g.
[0110] 3. Aluminum-based lithium adsorption fiber recycling:
[0111] Compared with Example 1, the only difference is that the lithium extraction product obtained by adsorption for 4 hours in this example is used for desorption and recycling, and other conditions are the same as in Example 1.
[0112] In this embodiment, after 10 cycles of adsorption and 10 cycles of desorption, the aluminum-based lithium adsorption fiber is + The 4h adsorption capacity is 11.75mg / g.
[0113] Example 5
[0114] 1. Preparation of adsorption materials:
[0115] Same as Example 1.
[0116] 2. Static adsorption of lithium ions:
[0117] Compared with Example 1, the only difference is that the simulated solution used is a lithium-magnesium solution, and other conditions remain unchanged; wherein the lithium-magnesium solution contains Li + and Mg 2+ , Li + The initial concentration of Mg is 100 mg / L (about 14.3 mmol / L), 2+ The initial concentration of the lithium magnesium solution was 5 g / L (about 0.2 mol / L), and the pH of the lithium magnesium solution was 6.
[0118] In this embodiment, after 4 hours of adsorption, the aluminum-based lithium adsorption fiber is + The adsorption capacity of Mg is 12.61 mg / g. 2+ The adsorption capacity is 0.7 mg / g.
[0119] Comparative Example 1
[0120] The difference between this comparative example and Example 1 is that the polyacrylonitrile fiber is not immersed in the diaspore sol, but directly subjected to coprecipitation reaction; the details are as follows:
[0121] 1. Preparation of adsorption materials:
[0122] 0.1 g of polyacrylonitrile fiber (same as in Example 1) and 100 mL of lithium aluminum mixed solution (same as in Example 1) were reacted in a reactor at 85° C. for 24 h to obtain an intermediate material; ethanol was used to remove excess solution on the intermediate material, and then the intermediate material was aged at 70° C. for 12 h to obtain the prepared product.
[0123] In this comparative example, reference Figure 4 As shown, the fiber surface in the prepared product remains smooth and no Li / Al-LDHs particles grow.
[0124] Reference Figure 5 The XRD spectrum results shown in the figure show that the polymer has no fixed crystal diffraction peak, which is mainly because the fiber is not immersed in diaspore sol and there is no fixed aluminum source on the surface, so Li / Al-LDHs cannot grow on the fiber surface.
[0125] In this comparative example, the specific surface area of the prepared product is 92 cm 2 / g.
[0126] 2. Static adsorption of lithium ions:
[0127] Compared with Example 1, the only difference is that the prepared product of this comparative example is used as the adsorption material, and the other conditions are the same as Example 1.
[0128] In this comparative example, after 4 h of adsorption, the prepared product was Li + The adsorption amount is <0.1mg / g.
[0129] Comparative Example 2
[0130] 1. Preparation of adsorption materials:
[0131] Compared with Example 1, the only difference is that, in the process of obtaining the lithium-aluminum mixed solution, the ion mixed solution is replaced with a lithium chloride solution with a concentration of 1 mol / L (that is, 0.1 mol of lithium chloride is dissolved in 100 mL of pure water); then, a sodium hydroxide solution with a concentration of 1 mol / L is added dropwise to the lithium chloride solution, and stirred at a speed of 120 rpm at 70°C until the pH of the solution is 5.5; other conditions are the same as in Example 1.
[0132] In this comparative example, reference Figure 6 As shown, no Li / Al-LDHs grew on the fiber surface.
[0133] Reference Figure 7 As shown, some diffraction peaks appeared in the XRD spectrum, and according to the PDF card comparison, they were mainly AlOOH diffraction peaks; therefore, although the diaspore sol was coated on the fiber surface after immersion, after the lithium-aluminum mixed solution was replaced by lithium chloride solution, Li / Al-LDHs particles could not grow on the fiber surface.
[0134] In this comparative example, the specific surface area of the prepared product is 95 cm 2 / g.
[0135] 2. Static adsorption of lithium ions:
[0136] Compared with Example 1, the only difference is that the prepared product of this comparative example is used as the adsorption material, and the other conditions are the same as Example 1.
[0137] In this comparative example, after 4 h of adsorption, the prepared product was Li + The adsorption amount is <0.1mg / g.
[0138] Comparative Example 3
[0139] 1. Preparation of adsorption materials:
[0140] Compared with Example 1, the only difference is that in the process of obtaining the diaspore sol, the solid content of the boehmite powder is adjusted to 9% (that is, the mass percentage of the boehmite powder and pure water is 9%), and the other conditions are the same as Example 1.
[0141] The prepared product of this comparative example is as follows Figure 8 As shown in the figure, it can be seen that the fiber surface is hardened; in this comparative example, the specific surface area of the prepared product is measured to be 76cm 2 / g.
[0142] 2. Static adsorption of lithium ions:
[0143] Compared with Example 1, the only difference is that the prepared product of this comparative example is used as the adsorption material, and the other conditions are the same as Example 1.
[0144] In this comparative example, after 4 h of adsorption, the prepared product was Li + The adsorption amount is 1.58 mg / g.
[0145] Comparative Example 4
[0146] 1. Preparation of adsorption materials:
[0147] Compared with Example 1, the only difference is that in the process of obtaining the diaspore sol, the heating and stirring time after the dropwise addition of the nitric acid solution is adjusted to 2 hours, and the other conditions are the same as in Example 1.
[0148] In this comparative example, the specific surface area of the prepared product was measured to be 104 cm 2 / g.
[0149] 2. Static adsorption of lithium ions:
[0150] Compared with Example 1, the only difference is that the prepared product of this comparative example is used as the adsorption material, and the other conditions are the same as Example 1.
[0151] In this comparative example, after 4 h of adsorption, the prepared product was Li + The adsorption amount is 0.13 mg / g.
[0152] Comparative Example 5
[0153] 1. Preparation of adsorption materials:
[0154] Compared with Example 1, the only difference is that in the process of obtaining the aluminum-based lithium adsorption fiber, the reaction time in the reactor is adjusted to 12 hours, and the other conditions are the same as Example 1.
[0155] In this comparative example, the specific surface area of the prepared product was measured to be 97 cm 2 / g.
[0156] 2. Static adsorption of lithium ions:
[0157] Compared with Example 1, the only difference is that the prepared product of this comparative example is used as the adsorption material, and the other conditions are the same as Example 1.
[0158] In this comparative example, after 4 h of adsorption, the prepared product was Li + The adsorption amount is 0.24 mg / g.
[0159] Comparative Example 6
[0160] 1. Preparation of adsorption materials:
[0161] Compared with Example 1, the only difference is that in the process of obtaining the lithium-aluminum mixed solution, the temperature of the ion mixed solution is adjusted from 70° C. to room temperature, and the other conditions are the same as Example 1.
[0162] In this comparative example, the specific surface area of the prepared product was measured to be 94 cm 2 / g.
[0163] 2. Static adsorption of lithium ions:
[0164] Compared with Example 1, the only difference is that the prepared product of this comparative example is used as the adsorption material, and the other conditions are the same as Example 1.
[0165] In this comparative example, after 4 h of adsorption, the prepared product was Li + The adsorption capacity is <0.1 mg / g.
[0166] The above technical solutions of the present invention are only preferred embodiments of the present invention, and are not intended to limit the patent scope of the present invention. All equivalent structural changes made using the contents of the present invention specification under the technical concept of the present invention, or directly / indirectly applied in other related technical fields, are included in the patent protection scope of the present invention.
Claims
1. A method for preparing aluminum-based lithium adsorption fiber, characterized in that: include: The fiber material is immersed in diaspore sol to obtain a precursor material; The precursor material and the lithium aluminum mixed solution are reacted at 80-90° C. for 18-30 hours to obtain an intermediate material; the intermediate material is subjected to an aging treatment to obtain the aluminum-based lithium adsorption fiber; The mass volume ratio of the precursor material to the lithium aluminum mixed solution is 0.1-0.5 g: 50-150 mL, and the molar ratio of lithium ions to aluminum ions in the lithium aluminum mixed solution is 1: 1-1.3; The fiber material includes one or more of polyacrylonitrile fiber, polyvinyl chloride fiber, and polyvinylidene fluoride fiber; The method for obtaining the diaspore sol comprises: mixing diaspore powder and a dispersant at 60-80° C. for 0.5-2 hours to obtain a pretreatment liquid, wherein the dispersant comprises water; dropping a nitric acid solution into the pretreatment liquid, and mixing the nitric acid solution and the pretreatment liquid at 60-80° C. for 3-6 hours to obtain the diaspore sol; the mass percentage of the diaspore powder and the dispersant is 5-8%, the concentration of nitric acid in the nitric acid solution is 1.5-2.5 mol / L, and the molar ratio of the nitric acid to the aluminum ion in the diaspore is 0.4-0.6:1; The method for obtaining the lithium aluminum mixed solution comprises: + and Al 3+ An alkaline solution is added dropwise to the ion mixed solution until the pH of the ion mixed solution is 5.3-5.8 to obtain the lithium aluminum mixed solution; during the process of adding the alkaline solution dropwise, the temperature of the ion mixed solution is maintained at 60-80°C.
2. An aluminum-based lithium adsorption fiber, characterized in that: The preparation is carried out by the preparation method as claimed in claim 1.
3. Use of the aluminum-based lithium adsorption fiber as claimed in claim 2 in extracting lithium.
4. A method for selectively extracting lithium, characterized in that: Includes steps: S1, obtaining a liquid to be extracted, wherein the liquid to be extracted contains Li + ; S2, performing lithium extraction treatment on the liquid to be extracted; The lithium extraction process comprises: mixing aluminum-based lithium adsorbing fibers into the solution to be extracted to obtain a first treatment solution; then, mixing the first treatment solution to remove Li + Adsorbing into the aluminum-based lithium adsorption fiber to obtain a lithium extraction product; The preparation process of the aluminum-based lithium adsorption fiber includes: soaking the fiber material in diaspore sol to obtain a precursor material; reacting the precursor material with a lithium-aluminum mixed solution at 80-90° C. for 18-30 hours to obtain an intermediate material; aging the intermediate material to obtain the aluminum-based lithium adsorption fiber; wherein the mass volume ratio of the precursor material to the lithium-aluminum mixed solution is 0.1-0.5 g: 50-150 mL, and the molar ratio of lithium ions to aluminum ions in the lithium-aluminum mixed solution is 1: 1-1.3; The fiber material includes one or more of polyacrylonitrile fiber, polyvinyl chloride fiber, and polyvinylidene fluoride fiber; The method for obtaining the diaspore sol comprises: mixing diaspore powder and a dispersant at 60-80° C. for 0.5-2 hours to obtain a pretreatment liquid, wherein the dispersant comprises water; dropping a nitric acid solution into the pretreatment liquid, and mixing the nitric acid solution and the pretreatment liquid at 60-80° C. for 3-6 hours to obtain the diaspore sol; the mass percentage of the diaspore powder and the dispersant is 5-8%, the concentration of nitric acid in the nitric acid solution is 1.5-2.5 mol / L, and the molar ratio of the nitric acid to the aluminum ion in the diaspore is 0.4-0.6:1; The method for obtaining the lithium aluminum mixed solution comprises: + and Al 3+ Adding an alkaline solution dropwise to the ion mixed solution until the pH of the ion mixed solution is 5.3-5.8, thereby obtaining the lithium aluminum mixed solution; in the process of adding the alkaline solution dropwise, maintaining the temperature of the ion mixed solution at 60-80° C.; S3, delithiation treatment of the lithium extraction product in a neutral solution to obtain a lithium-rich solution.
5. The method for selectively extracting lithium according to claim 4, characterized in that: The Li in the solution to be extracted + The concentration of Mg is 0.2-60mmol / L, the pH of the extract is 5.5-8; the extract also contains Mg 2+ , Ca 2+ 、Na + , K + , B 3+ One or more of .
6. The method for selectively extracting lithium according to claim 4, characterized in that: When the first treatment liquid is mixed, the rotation speed is 50-200 rpm and the duration is 1-5 hours.
7. The method for selectively extracting lithium according to claim 4, characterized in that: The neutral solution includes water or lithium chloride solution, and the concentration of lithium ions in the lithium chloride solution is not higher than 0.5 mmol / L; The lithium removal treatment includes: mixing the lithium extraction product into the neutral solution to obtain a second treatment liquid; then performing a mixing operation on the second treatment liquid at a rotation speed of 50-200 rpm for a time of 0.5-1.5 hours to remove the lithium element in the lithium extraction product.