A kind of porous manganese dioxide and its preparation method and application

Through the mixed electrolysis method of manganese sulfate acidic electrolyte, coconut oil and natural surfactants, the problem of complex and high cost preparation process of porous manganese dioxide is solved, the preparation of uniform porous structure and high purity manganese dioxide is achieved, and the process is simplified And has environmentally friendly properties.

CN118223043BActive Publication Date: 2024-10-18CHANGSHA UNIVERSITY
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410319721.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-20
Publication Date
2024-10-18
Estimated Expiration
2044-03-20

AI Technical Summary

Technical Problem

The existing preparation methods for porous manganese dioxide are complex, costly and have uneven pores, making it difficult to meet the diverse performance requirements of manganese dioxide for high-performance batteries.

Method used

Using a mixed electrolysis method of manganese sulfate acidic electrolyte, coconut oil and natural surfactants (saponin, soapberry extract, betaine), hydrogen gas is used to form a fine foam structure, and uniform porous manganese dioxide is formed in one step, simplifying the process and Reduce costs.

Benefits of technology

It achieves the preparation of uniform porous structure and high-purity manganese dioxide, simplifies the process, reduces production costs, and avoids the irritating and corrosive damage to the skin caused by traditional chemical products, and has environmentally friendly properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118223043B_ABST
    Figure CN118223043B_ABST
Patent Text Reader

Abstract

The present invention provides a porous manganese dioxide and a preparation method and application thereof, belonging to the technical field of battery materials. The present invention adds a foaming agent and coconut oil to a manganese sulfate acid electrolyte. Since coconut oil is insoluble in water, the negative electrode continuously generates hydrogen during electrolysis. The coconut oil distributed on the surface of the manganese sulfate acid electrolyte forms a heat-insulating layer with a foam structure under the action of hydrogen to cover the surface of the electrolyte. On the one hand, the temperature of the electrolyte can be stabilized within a suitable range. On the other hand, the presence of the heat-insulating layer can reduce the escape of hydrogen, so that the foaming agent distributed in the electrolyte continuously forms fine foam at the anode under the action of hydrogen. In the deposition and crystallization process of manganese dioxide electrolyzed on the surface of the anode plate, tiny bubbles are mixed under the action of fine foam, thereby forming loose porous manganese dioxide deposited on the anode plate in one step, and obtaining uniform porous manganese dioxide.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of battery materials, and in particular to porous manganese dioxide and a preparation method and application thereof. Background Art

[0002] With the vigorous development of the environmentally friendly new energy battery industry, high-performance batteries such as lithium manganese oxide and lithium iron manganese phosphate have more diverse performance requirements for key raw material manganese dioxide. The internal pore space of porous manganese dioxide can effectively alleviate the structural stress generated by the insertion / extraction of lithium ions in the electrode material during repeated charging and discharging, thereby maintaining the stability of the electrode, and the porous structure has a large specific surface area, which helps to increase the electrochemical active area and improve the capacity and charge and discharge efficiency of the electrode. At present, the preparation method of porous manganese dioxide is mostly post-processing pore formation of finished manganese dioxide. For example, the Chinese patent application with publication number CN114956186A adopts high-temperature reduction and roasting of the finished manganese dioxide, and then disproportionation by sulfuric acid, reset oxidation, continuous bubble impact in the reaction solution, and separation and drying to prepare porous manganese dioxide. This treatment method is not only complex in process and high in cost, but also the surface and internal pores of the prepared porous manganese dioxide are uneven, which is difficult to meet the technical requirements.

[0003] Therefore, providing a preparation method of manganese dioxide with simple process and uniform pores has become a technical problem to be solved urgently in this field. Summary of the invention

[0004] The object of the present invention is to provide a porous manganese dioxide and a preparation method and application thereof. The manganese dioxide prepared by the preparation method provided by the present invention has a uniform porous microstructure, and the manganese dioxide has high purity and a simple preparation process.

[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0006] The present invention provides a method for preparing porous manganese dioxide, comprising the following steps:

[0007] The manganese sulfate acid electrolyte, coconut oil and a foaming agent are mixed and then electrolyzed to obtain porous manganese dioxide;

[0008] The foaming agent comprises saponin, soapberry extract, betaine and water;

[0009] The mass ratio of the manganese sulfate acid electrolyte, coconut oil and foaming agent is 1: (0.03-0.07): (0.02-0.06);

[0010] The current density of the positive and negative electrodes during electrolysis is independently 60 to 100 A / m 2 .

[0011] Preferably, the method for preparing the manganese sulfate acidic electrolyte comprises the following steps:

[0012] (1) mixing pyrolusite and pyrite with ball milling to obtain mixed ore powder;

[0013] (2) mixing the mixed ore powder obtained in step (1) with dilute sulfuric acid to carry out a leaching reaction, and filtering to obtain a crude manganese sulfate solution;

[0014] (3) adding lime milk to the crude manganese sulfate solution obtained in step (2) to carry out a neutralization reaction, then filtering, then adding sodium dimethylaminosulfonate and BaS impurity remover to carry out a chelating reaction, and finally filtering to obtain a refined manganese sulfate solution;

[0015] (4) Mixing the refined manganese sulfate solution obtained in step (3) with sulfuric acid to obtain a manganese sulfate acidic electrolyte.

[0016] Preferably, the concentration of sulfuric acid in the manganese sulfate acidic electrolyte is 25-45 g / L.

[0017] Preferably, the total amount of sodium dimethylaminosulfonate and BaS impurity remover in step (3) is 4-8% of the mass of the mixed mineral powder in step (1).

[0018] Preferably, the foaming agent comprises 20-50 wt.% of saponin, ≤20 wt.% of soapberry extract, 10-30 wt.% of betaine and 40-60 wt.% of water.

[0019] Preferably, the mass ratio of the manganese sulfate acidic electrolyte, coconut oil and foaming agent is 1: (0.03-0.06): (0.03-0.05).

[0020] Preferably, the electrolysis temperature is 90-100°C.

[0021] Preferably, the current density of the positive and negative electrodes during electrolysis is independently 80 to 100 A / m 2 .

[0022] The present invention provides porous manganese dioxide prepared by the preparation method described in the above technical solution.

[0023] The present invention provides the application of the porous manganese dioxide described in the above technical solution in a battery.

[0024] The invention provides a method for preparing porous manganese dioxide, comprising the following steps: mixing manganese sulfate acid electrolyte, coconut oil and a foaming agent and then electrolyzing to obtain porous manganese dioxide; the foaming agent comprises saponin, soapberry extract, betaine and water; the mass ratio of the manganese sulfate acid electrolyte, coconut oil and foaming agent is 1: (0.03-0.07): (0.02-0.06); the current density of the positive and negative electrodes during the electrolysis is independently 60-100A / m 2 The present invention adds a foaming agent and coconut oil to the manganese sulfate acid electrolyte. Since coconut oil is insoluble in water, the negative electrode continuously generates hydrogen during the electrolysis process. The coconut oil distributed on the surface of the manganese sulfate acid electrolyte forms a heat-insulating layer with a foam structure under the action of hydrogen and covers the surface of the electrolyte. On the one hand, the temperature of the electrolyte can be stabilized within a suitable range. On the other hand, the presence of the heat-insulating layer can reduce the escape of hydrogen, so that the foaming agent distributed in the electrolyte continuously forms fine foam at the anode under the action of hydrogen. In the deposition and crystallization process of manganese dioxide electrolyzed on the surface of the anode plate, the manganese dioxide is deposited on the surface of the anode plate. Under the action of dense foam, tiny bubbles are mixed, so that loose porous manganese dioxide is formed in one step and deposited on the anode plate to obtain uniform and porous manganese dioxide, and there is no need to perform subsequent treatment on the pore structure of manganese dioxide, thereby reducing production costs; in addition, by using three different surfactants of saponin, betaine and soapberry extract as foaming substances, there is interaction between molecules after mixing, which can play a role of compounding and synergizing, so that the bubbles produced are more dense and stable, which is conducive to obtaining a uniform porous structure, and the natural surfactant used at the same time avoids the irritation and corrosive damage of traditional chemical products to the skin and eyes, which is green and environmentally friendly. The results of the embodiment show that the manganese dioxide prepared by the preparation method provided by the present invention has a uniform and porous microstructure, and the purity of manganese dioxide is high. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is a SEM image of the porous manganese dioxide prepared in Example 1 of the present invention;

[0026] Figure 2 This is the XRD pattern of the porous manganese dioxide prepared in Example 1 of the present invention;

[0027] Figure 3 This is a SEM image of the porous manganese dioxide prepared in Comparative Example 1;

[0028] Figure 4 This is the SEM image of the porous manganese dioxide prepared in Comparative Example 2. DETAILED DESCRIPTION

[0029] The present invention provides a method for preparing porous manganese dioxide, comprising the following steps:

[0030] Manganese sulfate acid electrolyte, coconut oil and a foaming agent are mixed and then electrolyzed to obtain porous manganese dioxide.

[0031] In the present invention, unless otherwise specified, the raw materials used are commercially available products well known to those skilled in the art.

[0032] In the present invention, the method for preparing the manganese sulfate acidic electrolyte preferably comprises the following steps:

[0033] (1) mixing pyrolusite and pyrite with ball milling to obtain mixed ore powder;

[0034] (2) mixing the mixed ore powder obtained in step (1) with dilute sulfuric acid to carry out a leaching reaction, and filtering to obtain a crude manganese sulfate solution;

[0035] (3) adding lime milk to the crude manganese sulfate solution obtained in step (2) to carry out a neutralization reaction, then filtering, then adding sodium dimethylaminosulfonate and BaS impurity remover to carry out a chelating reaction, and finally filtering to obtain a refined manganese sulfate solution;

[0036] (4) Mixing the refined manganese sulfate solution obtained in step (3) with sulfuric acid to obtain a manganese sulfate acidic electrolyte.

[0037] In the present invention, preferably, pyrolusite and pyrite are mixed and ball-milled to obtain mixed ore powder.

[0038] In the present invention, the mass ratio of the pyrolusite to the pyrite is preferably 1:(0.2-0.35), and more preferably 1:(0.25-0.3).

[0039] The present invention has no special limitation on the specific operation of the ball milling, and the ball milling process well known to those skilled in the art can be used.

[0040] The present invention has no particular limitation on the particle size of the mixed mineral powder, which can be determined based on the technical common sense of those skilled in the art.

[0041] After obtaining the mixed ore powder, the present invention preferably mixes the mixed ore powder with dilute sulfuric acid and performs a leaching reaction, and obtains a crude manganese sulfate solution after filtering.

[0042] The present invention preferably detects the mass fraction of manganese in the mixed ore powder before mixing. In the present invention, the detection method is preferably to use the potentiometric titration method in the national standard GB / T 1506-2016. The present invention can better control the amount of mixed ore powder and dilute sulfuric acid added by detecting the mass fraction of manganese.

[0043] In the present invention, the concentration of the dilute sulfuric acid is preferably 80 to 100 g / L, more preferably 90 to 100 g / L. The present invention uses dilute sulfuric acid to avoid the solution temperature from rising during mixing and to better control the amount of sulfuric acid added.

[0044] In the present invention, the molar ratio of manganese in the mixed ore powder to sulfuric acid in dilute sulfuric acid is preferably 1: (0.8-1.2), more preferably 1: (0.9-1.1), and further preferably 1: 1. The present invention can fully carry out the reaction and avoid the waste of raw materials by controlling the dosage relationship of manganese and sulfuric acid.

[0045] In the present invention, the leaching reaction is preferably carried out in a continuous leaching tank; the temperature of the leaching reaction is preferably 90-95°C; the time of the leaching reaction is preferably 4-5 hours. The present invention can promote the further progress of the reaction by controlling the reaction parameters.

[0046] In the present invention, the filtering method is preferably filter pressing. The present invention has no special limitation on the specific operation of the filter pressing, and the filter pressing operation well known to those skilled in the art can be used. The present invention can remove solid impurities through filter pressing.

[0047] After obtaining the crude manganese sulfate solution, the present invention preferably adds lime milk to the crude manganese sulfate solution for neutralization reaction, then filters it, then adds sodium dimethylaminosulfonate and BaS impurity remover for chelating reaction, and finally filters it to obtain a refined manganese sulfate solution.

[0048] The present invention has no particular limitation on the amount of the lime milk, as long as the pH value of the solution is 6 to 8. In the present invention, the neutralization reaction time is preferably 3 to 4 hours. By controlling the neutralization reaction time, the present invention can ensure complete reaction and precipitation of solid impurities, thereby facilitating subsequent filtration to remove solid impurities.

[0049] In the present invention, the total amount of the sodium dimethylaminosulfonate and BaS impurity remover is preferably 4-8% of the mass of the mixed ore powder, more preferably 5-7%, and further preferably 6%; the mass ratio of the sodium dimethylaminosulfonate and BaS impurity remover is preferably 1: 1. The present invention can form a water-insoluble chelate with metal ions such as mercury, silver, copper, nickel, cobalt, platinum, calcium, titanium, tin, zinc, etc. in the solution by adding sodium dimethylaminosulfonate and BaS impurity removers and controlling their dosage, thereby removing impurities.

[0050] In the present invention, the chelation reaction time is preferably 24 to 32 hours. The present invention can further remove impure metal elements by controlling the chelation reaction time.

[0051] In the present invention, the filtering method is preferably filter pressing. The present invention has no special limitation on the specific operation of the filter pressing, and the filter pressing operation well known to those skilled in the art can be used. The present invention can remove solid impurities through filter pressing.

[0052] After obtaining the refined manganese sulfate solution, the present invention preferably mixes the refined manganese sulfate solution with sulfuric acid to obtain a manganese sulfate acidic electrolyte.

[0053] In the present invention, the concentration of sulfuric acid in the manganese sulfate acid electrolyte is preferably 25-45 g / L, more preferably 30-40 g / L, and further preferably 35 g / L. The present invention can achieve better electrolysis by controlling the concentration of sulfuric acid in the manganese sulfate acid electrolyte.

[0054] In the present invention, the foaming agent comprises saponin, soapberry extract, betaine and water, preferably 20-50wt.% of saponin, ≤20wt.% of soapberry extract, 10-30wt.% of betaine and 40-60wt.% of water, more preferably 20-40wt.% of saponin, 5-20wt.% of soapberry extract, 10-25wt.% of betaine and 40-60wt.% of water, further preferably 25-35wt.% of saponin, 5-15wt.% of soapberry extract, 15-20wt.% of betaine and 40-55wt.% of water. The present invention adopts three different surfactants, namely saponin, betaine and soapberry extract, as foaming substances. After mixing, the molecules interact with each other, which can play a role of compounding and enhancing, so that the bubbles generated by them are finer and more stable, which is conducive to obtaining a uniform porous structure; by controlling the content of each component in the foaming agent, a better foaming effect can be achieved, and the cost of the foaming agent can be avoided to be too high.

[0055] In the present invention, the method for preparing the foaming agent preferably comprises the following steps: mixing saponin, soapberry extract, betaine and water in a batching tank to obtain the foaming agent. The present invention has no particular limitation on the stirring method and stirring time during the mixing, which can be determined according to the technical common sense of those skilled in the art, as long as the components can be mixed evenly.

[0056] In the present invention, the mass ratio of the manganese sulfate acid electrolyte, coconut oil and foaming agent is 1: (0.03-0.07): (0.02-0.06), preferably 1: (0.04-0.06): (0.03-0.05), and more preferably 1: 0.05: 0.04. In the present invention, the density of coconut oil is smaller than that of the electrolyte, and it can float on the surface of the electrolyte to form a heat preservation layer. By controlling the amount of coconut oil, it can be avoided that the electrolyte cannot be completely covered by too little coconut oil, and the cost increase caused by too much coconut oil can be avoided; the foaming agent can be dissolved in the electrolyte, and fine bubbles are generated at the electrode plate during electrolysis to facilitate the deposition of porous manganese dioxide. By controlling the amount of the foaming agent, sufficient fine bubbles can be formed and the cost can be avoided.

[0057] The present invention has no particular limitation on the specific manner of mixing the manganese sulfate acid electrolyte, coconut oil and foaming agent, which can be determined according to the technical common sense of those skilled in the art.

[0058] In the present invention, the electrolysis is preferably carried out in an electrolytic cell. In the present invention, the anode used in the electrolysis is preferably an anode plate. The present invention uses an anode plate, which has a large area and is convenient for the attachment of porous manganese dioxide.

[0059] In the present invention, the electrolysis temperature is preferably 90-100°C, more preferably 95-100°C; the current density of the positive and negative electrodes during the electrolysis is independently 60-100A / m 2 , preferably 70 to 100 A / m 2 , more preferably 80 to 100 A / m 2 The present invention can further improve the density of bubbles generated during electrolysis by controlling the temperature and current density during electrolysis, thereby improving the uniformity of the pores of manganese dioxide.

[0060] After the electrolysis is completed, the present invention preferably sequentially strips, crushes, rinses, neutralizes and dries the product of the anode plate during electrolysis to obtain porous manganese dioxide. The present invention has no particular limitation on the specific operations of the stripping, crushing, rinsing, neutralizing and drying processes, and the stripping, crushing, rinsing, neutralizing and drying processes well known to those skilled in the art can be used. The present invention can remove impurities in the porous manganese dioxide through the above-mentioned treatment to improve the purity of the manganese dioxide.

[0061] The invention adds a foaming agent and coconut oil to a manganese sulfate acid electrolyte. Since the coconut oil is insoluble in water, the negative electrode continuously generates hydrogen during the electrolysis process. The coconut oil distributed on the surface of the manganese sulfate acid electrolyte forms a heat-insulating layer with a foam structure under the action of hydrogen and covers the surface of the electrolyte. On the one hand, the temperature of the electrolyte can be stabilized within a suitable range. On the other hand, the existence of the heat-insulating layer can reduce the escape of hydrogen, so that the foaming agent distributed in the electrolyte continuously forms fine foam at the anode under the action of hydrogen. In the deposition and crystallization process of manganese dioxide electrolyzed on the surface of the anode plate, the manganese dioxide is formed on the surface of the anode plate. Under the action of dense foam, tiny bubbles are mixed in, so that loose porous manganese dioxide is formed in one step and deposited on the anode plate, so as to obtain uniform porous manganese dioxide. There is no need to carry out subsequent treatment on the pore structure of manganese dioxide, thereby reducing production costs. In addition, by using three different surfactants, namely saponin, betaine and soapberry extract, as foaming substances, there is interaction between the molecules after mixing, which can play a role of compounding and enhancing, so that the bubbles generated are more fine and stable, which is conducive to obtaining a uniform porous structure. At the same time, the natural surfactants used avoid the irritation and corrosive damage to the skin and eyes caused by traditional chemical products, which is green and environmentally friendly.

[0062] The present invention provides porous manganese dioxide prepared by the preparation method described in the above technical solution. The manganese dioxide prepared by the present invention has a uniform porous microstructure.

[0063] The present invention provides the application of the porous manganese dioxide described in the above technical solution in a battery.

[0064] In the present invention, the battery is preferably a lithium manganese oxide battery or a lithium iron manganese phosphate battery. The present invention has no special limitation on the specific application of the porous manganese dioxide in the battery, and the application method familiar to those skilled in the art can be used.

[0065] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0066] Example 1

[0067] A method for preparing porous manganese dioxide, comprising the following steps:

[0068] A manganese sulfate acid electrolyte, coconut oil and a foaming agent are mixed in an electrolytic cell and then electrolyzed, wherein the anode is an anode plate during the electrolysis, and then the product of the anode plate is sequentially stripped, crushed, rinsed, neutralized and dried to obtain porous manganese dioxide;

[0069] The concentration of sulfuric acid in the manganese sulfate acidic electrolyte is 35 g / L;

[0070] The foaming agent is composed of: 30wt.% of saponin, 5wt.% of soapberry extract, 20wt.% of betaine and 45wt.% of water;

[0071] The preparation method of the foaming agent comprises: mixing saponin, soapberry extract, betaine and water in a mixing tank to obtain the foaming agent;

[0072] The mass ratio of the manganese sulfate acid electrolyte, coconut oil and foaming agent is 1:0.03:0.05;

[0073] The electrolysis temperature is 95°C, and the current density of the positive and negative electrodes during electrolysis is independently 90A / m 2 ;

[0074] The preparation method of the manganese sulfate acidic electrolyte is specifically the following steps:

[0075] (1) mixing pyrolusite and pyrite in a mass ratio of 1:0.25 and ball-milling to obtain mixed ore powder;

[0076] (2) The mass fraction of manganese in the mixed ore powder obtained in step (1) is detected by the potentiometric titration method in the national standard GB / T 1506-2016, and then the mixed ore powder and dilute sulfuric acid are mixed in a continuous leaching tank for leaching reaction, and a crude manganese sulfate solution is obtained after filter pressing; the concentration of the dilute sulfuric acid is 90 g / L; the molar ratio of manganese in the mixed ore powder to sulfuric acid in the dilute sulfuric acid is 1:1; the temperature of the leaching reaction is 95° C., and the time of the leaching reaction is 5 h;

[0077] (3) adding lime milk to the crude manganese sulfate solution obtained in step (2) to carry out neutralization reaction for 4 hours, so that the pH value of the solution is 6.5, then filtering, then adding sodium dimethylaminosulfonate and BaS impurity remover to carry out chelating reaction, and finally filtering to obtain a refined manganese sulfate solution; the total amount of sodium dimethylaminosulfonate and BaS impurity remover is 6% of the mass of the mixed ore powder; the mass ratio of sodium dimethylaminosulfonate to BaS impurity remover is 1:1; the chelating reaction time is 32 hours;

[0078] (4) The refined manganese sulfate solution obtained in step (3) is mixed with sulfuric acid to obtain a manganese sulfate acid electrolyte having a sulfuric acid concentration of 35 g / L.

[0079] The SEM image of the porous manganese dioxide prepared in Example 1 is as follows: Figure 1 As shown. Figure 1 It can be seen that the manganese dioxide prepared in Example 1 has a uniform porous microstructure.

[0080] The XRD pattern of the porous manganese dioxide prepared in Example 1 is as follows: Figure 2 As shown. Figure 2 It can be seen that the manganese dioxide prepared in Example 1 has high purity.

[0081] Comparative Example 1

[0082] A method for preparing porous manganese dioxide, comprising the following steps:

[0083] A manganese sulfate acid electrolyte, coconut oil and a foaming agent are mixed in an electrolytic cell and then electrolyzed, wherein the anode is an anode plate during the electrolysis, and then the product of the anode plate is sequentially stripped, crushed, rinsed, neutralized and dried to obtain porous manganese dioxide;

[0084] The concentration of sulfuric acid in the manganese sulfate acidic electrolyte is 35 g / L;

[0085] The foaming agent is composed of: 20wt.% of saponin, 15wt.% of soapberry extract, 10wt.% of betaine and 55wt.% of water;

[0086] The preparation method of the foaming agent is as follows: saponin, soapberry extract, betaine and water are directly mixed in a mixing tank to obtain the foaming agent;

[0087] The mass ratio of the manganese sulfate acid electrolyte, coconut oil and foaming agent is 1:0.03:0.04;

[0088] The electrolysis temperature is 95°C, and the current density of the positive and negative electrodes during electrolysis is independently 110A / m 2 ;

[0089] The preparation method of the manganese sulfate acidic electrolyte is specifically the following steps:

[0090] (1) mixing pyrolusite and pyrite in a mass ratio of 1:0.25 and ball-milling to obtain mixed ore powder;

[0091] (2) The mass fraction of manganese in the mixed ore powder obtained in step (1) is detected by the potentiometric titration method in the national standard GB / T 1506-2016, and then the mixed ore powder and dilute sulfuric acid are mixed in a continuous leaching tank for leaching reaction, and a crude manganese sulfate solution is obtained after filter pressing; the concentration of the dilute sulfuric acid is 90 g / L; the molar ratio of manganese in the mixed ore powder to sulfuric acid in the dilute sulfuric acid is 1:1; the temperature of the leaching reaction is 95° C., and the time of the leaching reaction is 5 h;

[0092] (3) adding lime milk to the crude manganese sulfate solution obtained in step (2) to carry out neutralization reaction for 4 hours, so that the pH value of the solution is 6.5, then filtering, then adding sodium dimethylaminosulfonate and BaS impurity remover to carry out chelating reaction, and finally filtering to obtain a refined manganese sulfate solution; the total amount of sodium dimethylaminosulfonate and BaS impurity remover is 6% of the mass of the mixed ore powder; the mass ratio of sodium dimethylaminosulfonate to BaS impurity remover is 1:1; the chelating reaction time is 32 hours;

[0093] (4) The refined manganese sulfate solution obtained in step (3) is mixed with sulfuric acid to obtain a manganese sulfate acid electrolyte having a sulfuric acid concentration of 35 g / L.

[0094] The SEM image of the porous manganese dioxide prepared in Comparative Example 1 is as follows: Figure 3 As shown. Figure 3 It can be seen that the manganese dioxide prepared in Comparative Example 1 has a dense structure and does not achieve the purpose of porous structure design. Figure 1 and Figure 3 It can be seen from the comparison that when the current density during electrolysis is too large, the structure of manganese dioxide will become dense and the porosity will decrease.

[0095] Comparative Example 2

[0096] A method for preparing porous manganese dioxide, comprising the following steps:

[0097] A manganese sulfate acid electrolyte, coconut oil and a foaming agent are mixed in an electrolytic cell and then electrolyzed, wherein the anode is an anode plate during the electrolysis, and then the product of the anode plate is sequentially stripped, crushed, rinsed, neutralized and dried to obtain porous manganese dioxide;

[0098] The concentration of sulfuric acid in the manganese sulfate acidic electrolyte is 35 g / L;

[0099] The foaming agent is composed of: 25wt.% of saponin, 10wt.% of soapberry extract, 25wt.% of betaine and 40wt.% of water;

[0100] The preparation method of the foaming agent is as follows: saponin, soapberry extract, betaine and water are directly mixed in a mixing tank to obtain the foaming agent;

[0101] The mass ratio of the manganese sulfate acid electrolyte, coconut oil and foaming agent is 1:0.02:0.06;

[0102] The electrolysis temperature is 95°C, and the current density of the positive and negative electrodes during electrolysis is independently 60A / m 2 ;

[0103] The preparation method of the manganese sulfate acidic electrolyte is specifically the following steps:

[0104] (1) mixing pyrolusite and pyrite in a mass ratio of 1:0.25 and ball-milling to obtain mixed ore powder;

[0105] (2) The mass fraction of manganese in the mixed ore powder obtained in step (1) is detected by the potentiometric titration method in the national standard GB / T 1506-2016, and then the mixed ore powder and dilute sulfuric acid are mixed in a continuous leaching tank for leaching reaction, and a crude manganese sulfate solution is obtained after filter pressing; the concentration of the dilute sulfuric acid is 90 g / L; the molar ratio of manganese in the mixed ore powder to sulfuric acid in the dilute sulfuric acid is 1:1; the temperature of the leaching reaction is 95° C., and the time of the leaching reaction is 5 h;

[0106] (3) adding lime milk to the crude manganese sulfate solution obtained in step (2) to carry out neutralization reaction for 4 hours, so that the pH value of the solution is 6.5, then filtering, then adding sodium dimethylaminosulfonate and BaS impurity remover to carry out chelating reaction, and finally filtering to obtain a refined manganese sulfate solution; the total amount of sodium dimethylaminosulfonate and BaS impurity remover is 6% of the mass of the mixed ore powder; the mass ratio of sodium dimethylaminosulfonate to BaS impurity remover is 1:1; the chelating reaction time is 32 hours;

[0107] (4) The refined manganese sulfate solution obtained in step (3) is mixed with sulfuric acid to obtain a manganese sulfate acid electrolyte having a sulfuric acid concentration of 35 g / L.

[0108] The SEM image of the porous manganese dioxide prepared in Comparative Example 2 is as follows: Figure 4 As shown. Figure 4 It can be seen that the manganese dioxide prepared in Comparative Example 2 has a loose structure and uneven pores. Figure 1 and Figure 4 It can be seen from the comparison that when the amount of coconut oil added is too little, the coconut oil will not be able to completely cover the thermal insulation layer on the surface of the electrolyte, resulting in unstable temperature during electrolysis. At the same time, hydrogen is easy to escape, resulting in insufficient hydrogen for the foaming agent to form fine foam, which leads to a loose structure of manganese dioxide and uneven pores.

[0109] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing porous manganese dioxide, comprising the following steps: The manganese sulfate acid electrolyte, coconut oil and a foaming agent are mixed and then electrolyzed to obtain porous manganese dioxide; The foaming agent comprises 20-50 wt.% of saponin, ≤20 wt.% of soapberry extract, 10-30 wt.% of betaine and 40-60 wt.% of water; The mass ratio of the manganese sulfate acid electrolyte, coconut oil and foaming agent is 1: (0.03-0.07): (0.02-0.06); The current density of the positive and negative electrodes during electrolysis is independently 60 to 100 A / m 2 .

2. The preparation method according to claim 1, It is characterized in that The preparation method of the manganese sulfate acidic electrolyte comprises the following steps: (1) mixing pyrolusite and pyrite with ball milling to obtain mixed ore powder; (2) mixing the mixed ore powder obtained in step (1) with dilute sulfuric acid to carry out a leaching reaction, and filtering to obtain a crude manganese sulfate solution; (3) adding lime milk to the crude manganese sulfate solution obtained in step (2) to carry out a neutralization reaction, then filtering, then adding sodium dimethylaminosulfonate and BaS impurity remover to carry out a chelating reaction, and finally filtering to obtain a refined manganese sulfate solution; (4) Mixing the refined manganese sulfate solution obtained in step (3) with sulfuric acid to obtain a manganese sulfate acidic electrolyte.

3. The preparation method according to claim 1 or 2, It is characterized in that The concentration of sulfuric acid in the manganese sulfate acidic electrolyte is 25-45 g / L.

4. The preparation method according to claim 2, It is characterized in that The total amount of sodium dimethylaminosulfonate and BaS impurity remover in step (3) is 4-8% of the mass of the mixed ore powder in step (1).

5. The preparation method according to claim 1, It is characterized in that The mass ratio of the manganese sulfate acid electrolyte, coconut oil and foaming agent is 1: (0.03-0.06): (0.03-0.05).

6. The preparation method according to claim 1, It is characterized in that The electrolysis temperature is 90-100°C.

7. The preparation method according to claim 1, It is characterized in that The current density of the positive and negative electrodes during electrolysis is independently 80 to 100 A / m 2 .

8. The porous manganese dioxide prepared by the preparation method according to any one of claims 1 to 7.

9. Use of the porous manganese dioxide according to claim 8 in a battery.

Citation Information

Patent Citations

  • Porous manganese dioxide and preparation method thereof

    CN114956186A

  • Method for synthesizing anatase titanium dioxide and manganese dioxide nanocomposite through surfactant assisted electrodeposition and application of method

    CN106283099A