Rapid Detection Method for Hydration Resistance of Aluminum Electrolytic Capacitors
The method of sealing and preserving the anode foil and the cathode foil at high temperature can quickly detect the hydration resistance of the aluminum electrolytic capacitor, which solves the problems of long detection cycle and high cost in the existing technology, and enables timely judgment and evaluation of the matching between the aluminum foil and the electrolyte. Accurate prediction of capacitor performance.
Patent Information
- Application Number
- CN202410662002.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-27
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-05-27
AI Technical Summary
In the existing technology, the hydration resistance performance testing cycle of aluminum electrolytic capacitors is long and the cost is high, making it difficult to timely judge the matching of aluminum foil and electrolyte during the product production process.
By placing the anode foil and cathode foil in high-temperature sealed storage in the electrolyte, observing the surface characteristics and changes in electrical parameters, calculating the rate of increase in voltage increase time, rate of decrease in capacity and rate of decrease in withstand voltage, and judging whether the hydration resistance is qualified. .
It realizes the rapid detection of the hydration resistance of aluminum electrolytic capacitors, reduces production costs and time costs, reduces the defective rate of capacitor products, and improves product quality and efficiency.
Smart Images

Figure CN118226338B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of electrolytic capacitor detection, and in particular to a rapid detection method for the hydration resistance of an aluminum electrolytic capacitor. Background Art
[0002] Aluminum electrolytic capacitors are assembled from raw materials such as anode foil, cathode foil, electrolyte, and electrolytic paper. Among them, the electrolyte is the real cathode of the aluminum electrolytic capacitor. It not only plays a conductive role, but also plays a role in repairing the aluminum oxide dielectric layer on the surface of the anode foil, giving the aluminum electrolytic capacitor self-healing properties. Therefore, in order to improve the conductivity of the electrolyte, reduce ESR, and improve the repair efficiency of the aluminum oxide dielectric layer, aluminum electrolytic capacitor manufacturers usually add water to the electrolyte. However, as the use time of the capacitor gradually increases, the oxide film on the surface of the anode foil and cathode foil will react with the water in the electrolyte to hydrate, reduce the crystallinity of aluminum oxide, and form amorphous hydrated aluminum oxide, resulting in increased capacitance loss, increased leakage current, and large capacity attenuation, which seriously affects the service life of the capacitor.
[0003] At present, the high-temperature storage experiment is usually used to verify the hydration resistance of aluminum electrolytic capacitors. After assembling the raw materials such as anode foil, cathode foil, and electrolytic paper into capacitors, they are placed in an oven at 105-150°C and stored until the target life of the aluminum electrolytic capacitor (usually 500-3000 hours). During this period, the capacitors are taken out and tested for electrical properties, including leakage current, capacity, loss, impedance, etc. The capacitors are then disassembled to observe whether there is obvious degeneration on the surface of the anode foil and cathode foil (such as CN117330870A). However, the methods in the prior art are not only time-consuming, but also easy to miss the best production and application cycle of the product. In addition, the finished capacitors need to be made to determine whether the aluminum foil used matches the electrolyte in terms of hydration resistance, and the material cost and testing cost are high. Therefore, it is of great significance to achieve rapid judgment of the hydration resistance of aluminum electrolytic capacitors. Summary of the invention
[0004] In view of the long detection cycle and high detection cost of the above-mentioned aluminum electrolytic capacitor hydration resistance performance, a rapid detection method for the hydration resistance performance of aluminum electrolytic capacitors is provided. The present invention quickly determines the hydration resistance performance of the aluminum electrolytic capacitor constructed by the anode foil, cathode foil and electrolyte under high temperature conditions by judging the compatibility of the anode foil, cathode foil and electrolyte under high temperature conditions. The method of the present invention can provide an accurate prediction of whether the capacitor will fail due to hydration.
[0005] In order to achieve the above objectives, the present invention is implemented by the following technical solutions:
[0006] A quick test method for the hydration resistance of aluminum electrolytic capacitors includes the following steps:
[0007] The initial electrical parameters of the samples of anode foil and cathode foil are tested respectively, and then they are immersed in electrolyte respectively, and sealed and stored for no more than 350 hours at at least 100°C. After the test, their surface characteristics are observed. If the surface characteristics of both do not meet the standards, the hydration resistance of the corresponding aluminum electrolytic capacitor composed of such anode foil, cathode foil, and electrolyte is judged to be unqualified;
[0008] If the surface characteristics of both or one of them meet the standards, it is necessary to further test the electrical parameters after immersion and calculate the increase or decrease rate of the electrical parameters;
[0009] The calculated value of the increase rate or decrease rate of the electrical parameter is compared with the judgment value. If the calculated value of the increase rate or decrease rate of the electrical parameter exceeds the judgment value, it is determined that the hydration resistance of the corresponding aluminum electrolytic capacitor composed of the anode foil, cathode foil, and electrolyte is unqualified. The unqualified hydration resistance means that the hydration resistance of the corresponding aluminum electrolytic capacitor composed of the anode foil, cathode foil, and electrolyte is poor, and the aluminum electrolytic capacitor will fail due to hydration during its life cycle. On the contrary, if it does not exceed the judgment value, it is determined that the hydration resistance of the corresponding aluminum electrolytic capacitor composed of the anode foil, cathode foil, and electrolyte is qualified. The qualified hydration resistance means that the hydration resistance of the corresponding aluminum electrolytic capacitor composed of the anode foil, cathode foil, and electrolyte is good, and the aluminum electrolytic capacitor will not fail due to hydration during its life cycle.
[0010] Furthermore, the electrical parameters include: boost time, capacity, and withstand voltage; based on the initial electrical parameters and the electrical parameters after immersion detected, the boost time increase rate, capacity reduction rate, and withstand voltage reduction rate are calculated respectively, and the boost time increase rate is represented by T; the capacity reduction rate is represented by C; and the withstand voltage reduction rate is represented by V;
[0011] For example, T0 represents the value of the initial boost time, C0 represents the value of the initial capacity, and V0 represents the initial withstand voltage value;
[0012] T1 represents the value of the pressure rise time after immersion, C1 represents the value of the capacity after immersion, and V1 represents the withstand voltage value after immersion;
[0013] The increase rate of boost time can be calculated according to the formula: T=[|(T1- T0)| / T0]×100%;
[0014] The capacity reduction rate can be calculated according to the formula: C=[|(C1- C0)| / C0]×100%;
[0015] The voltage reduction rate can be calculated according to the formula: V=[|(V1- V0)| / V0]×100%.
[0016] According to the degradation trend of the electrical parameters of conventional capacitors, after running for a period of time, the capacity will inevitably decrease compared to the initial value, the withstand voltage will inevitably decrease compared to the initial value, and the boost time will inevitably increase compared to the initial value.
[0017] Furthermore, the judgment value corresponding to the capacity reduction rate C is 5%; the judgment value corresponding to the boost time increase rate T is 50%; the judgment value corresponding to the withstand voltage reduction rate V is 10%;
[0018] If at least one of the following conditions occurs: C>5%, T>50%, and V>10%, the hydration resistance of the corresponding aluminum electrolytic capacitor composed of the anode foil, cathode foil, and electrolyte is determined to be unqualified;
[0019] If C≤5%, T≤50%, and V≤10% are satisfied at the same time, it is determined that the hydration resistance of the corresponding aluminum electrolytic capacitor composed of the anode foil, cathode foil, and electrolyte is qualified.
[0020] Furthermore, the temperature of the sealed storage test is 105°C-150°C and the time is 168 hours-336 hours.
[0021] Furthermore, the number of samples of anode foil and cathode foil to be tested is at least 3 pieces respectively, the size of the samples is 1cm×5cm~1cm×10cm, and the amount of electrolyte used is sufficient to completely immerse the samples. The samples can be completely impregnated with this amount of electrolyte.
[0022] Furthermore, the surface characteristics not meeting the standards means that black spots and / or black irregular stripes can be observed, which indicates obvious degradation; the surface characteristics meeting the standards means that black spots and / or black irregular stripes cannot be clearly observed, which indicates no obvious abnormality or no obvious degradation.
[0023] Beneficial technical effects:
[0024] The essential reason for the hydration failure of the capacitor is that, on the one hand, the water in the electrolyte reacts with the anode foil, causing the aluminum oxide on the surface of the anode foil to become hydrated aluminum oxide, increasing loss and leakage; on the other hand, the water in the electrolyte reacts with the thinner aluminum oxide on the surface of the cathode foil or even the aluminum inside, causing the electrode foil to denature; therefore, the present invention directly seals the anode foil and the cathode foil in the electrolyte and places them in a high-temperature environment, wherein the volume of the electrolyte used for storage is much larger than the volume of the electrolyte in the actual aluminum electrolytic capacitor, so the volume of water content in the electrolyte that the aluminum foil contacts is much larger than that in the actual capacitor; at the same time, the storage temperature of the anode foil and the cathode foil in the present invention is much higher than the actual use temperature of the capacitor, and the above two items indicate that the storage environment of the aluminum foil is more severe than the environment in the actual capacitor, thereby amplifying the possibility of its hydration reaction; the present invention can quickly verify and determine the hydration resistance of the corresponding capacitor by respectively testing the electrical parameters of the anode foil and the cathode foil after being sealed and stored at high temperature in the corresponding electrolyte, without the need to assemble the layer core package for testing, so the judgment method of the present invention can provide an accurate prediction of whether the capacitor will fail due to hydration;
[0025] The present invention is based on the essential reaction of hydration reaction, and can examine the compatibility of aluminum foil and electrolyte without going through the preparation process of the capacitor (such as rolling aluminum foil and electrolytic paper into a core package and then immersing it in electrolyte for impregnation, then assembling it in an aluminum shell, then performing aging testing, and then storing it at high temperature). The present invention reduces the material cost and time cost of production. The method of the present invention can play an effective role in the research and development of electrolyte formulas, and can also greatly reduce the defective rate of capacitor products, reduce cost output, and improve efficiency and product quality. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 The present invention is a flowchart of a method for quickly detecting the hydration resistance of aluminum electrolytic capacitors. DETAILED DESCRIPTION
[0027] The technical solutions in the embodiments of the present invention will be described clearly and completely below in combination with the embodiments of the present invention and the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its application or use. All other embodiments obtained by ordinary technicians in this field without creative work based on the embodiments of the present invention are within the scope of protection of the present invention.
[0028] Unless otherwise specifically stated, the numerical value set forth in these embodiments does not limit the scope of the present invention. The technology and method known to those of ordinary skill in the relevant art may not be discussed in detail, but in appropriate cases, the technology and method should be considered as a part of the specification. In all examples shown and discussed here, any specific value should be interpreted as being merely exemplary, rather than as a limitation. Therefore, other examples of exemplary embodiments may have different values.
[0029] The experimental methods in the following examples without specifying specific conditions are usually measured in accordance with national standards; if there is no corresponding national standard, the method is carried out in accordance with the general standard requirements or general methods.
[0030] Example 1
[0031] A rapid test method for the hydration resistance of aluminum electrolytic capacitors with a model of 550V 470μF and a target life cycle of 3000 hours at 105℃ is as follows: Figure 1 As shown, no pre-assembly is required, and the specific steps include the following:
[0032] S1. Take the anode foil (820VF, borated) and cathode foil (2.5VF, aluminum purity 98%) used for this type of capacitor, cut them into test samples with a size of 1 cm × 10 cm, take three anode foil test samples and three cathode foil test samples to test their initial electrical parameters respectively. The electrical parameters include: boost time, capacity, and withstand voltage. T0 represents the value of the initial boost time, C0 represents the value of the initial capacity, and V0 represents the initial withstand voltage. Then rinse the anode foil test samples and cathode foil test samples with deionized water, dry them naturally, and set aside.
[0033] S2. Prepare two containers, each containing 200 mL of electrolyte A used for this type of capacitor. The water content of electrolyte A is 5.6 wt%, the main solvent is ethylene glycol, the main solute is C14~C22 branched carboxylic acid, the conductivity is 750 μS / cm, and the pH is 6.6.
[0034] The anode foil test sample is immersed in the electrolyte A in a container and subjected to a high temperature sealed storage test at 105 degrees Celsius for 168 hours;
[0035] The cathode foil test sample is immersed in the electrolyte A in another container and subjected to a high temperature sealed storage test at 105 degrees Celsius for 168 hours;
[0036] S3. Take out the anode foil test sample and the cathode foil test sample in step S2, clean the surface of the aluminum foil with deionized water, and dry it naturally. It is observed that the surface of the anode foil test sample in this case is normal, which indicates no obvious degradation (i.e., the surface characteristics meet the standard), but the surface of the cathode foil test sample is obviously degraded, with local black spots, which indicates obvious degradation (i.e., the surface characteristics do not meet the standard);
[0037] It can be preliminarily determined that under the electrolyte A, the anode foil has no hydration phenomenon, while the cathode foil has hydration. Therefore, the aluminum electrolytic capacitor constructed with the electrolyte A, cathode foil and anode foil is very likely to have poor hydration resistance and is prone to hydration failure during its life cycle.
[0038] S4. In order to further verify the reliability of the preliminary determination, the electrical parameters of the test samples observed in S3 are tested respectively, with T1 representing the value of the voltage rise time after immersion, C1 representing the value of the capacity after immersion, and V1 representing the withstand voltage value after immersion;
[0039] The increase rate of boost time can be calculated according to the formula: T=[|(T1- T0)| / T0]×100%;
[0040] The capacity reduction rate can be calculated according to the formula: C=[|(C1- C0)| / C0]×100%;
[0041] The voltage resistance reduction rate can be calculated according to the formula: V=[|(V1- V0)| / V0]×100%;
[0042] The test results are: the capacity reduction rate of the anode foil test sample is C=1.2% (C≤5%), the increase rate of the voltage rise time is T=0.8% (T≤50%), and the increase rate of the withstand voltage is V=1.1% (V≤10%); the capacity reduction rate of the cathode foil test sample is C=43.8% (C>5%), the increase rate of the voltage rise time is T=70% (T>50%), and the voltage resistance value reduction rate is V=50% (V>10%);
[0043] If the anode foil satisfies the three conditions of C≤5%, T≤50%, and V≤10% at the same time, but the cathode foil satisfies the three conditions of C>5%, T>50%, and V>10% at the same time, then it can be determined that the hydration resistance of the aluminum electrolytic capacitor constructed with the electrolyte A, cathode foil, and anode foil is unqualified, which means that the aluminum electrolytic capacitor constructed with the electrolyte A, cathode foil, and anode foil has poor hydration resistance and will experience hydration failure during its life cycle.
[0044] In order to further verify the reliability of the overall solution of this case, the following control test was conducted.
[0045] Comparative Example 1
[0046] The hydration resistance of an aluminum electrolytic capacitor with a model of 550V 470μF and a target life cycle of 3000 hours at 105°C was tested by a conventional method. The cathode foil, anode foil, and electrolyte A used below are the same as those in Example 1. The specific method is as follows:
[0047] S1. After cutting the anode foil and cathode foil used for the capacitor of this model, the anode foil-electrolytic paper-cathode foil-electrolytic paper are stacked and wound in the order of anode foil-electrolytic paper-cathode foil-electrolytic paper to form a core package of the capacitor. The core package is immersed in the electrolyte A used for the capacitor of this model and assembled into an aluminum shell to obtain a 550V 470μF aluminum electrolytic capacitor. After the capacitor is pressurized at 575V and aged for 2 hours, 50 capacitors are randomly selected and numbered and tested, and the average leakage current is 0.26 mA, and the average loss is 5.0%;
[0048] S2, the 50 capacitors in S1 were placed in a 105℃ oven for a 3000h high temperature durability life test; after the test, the capacitors were taken out and returned to room temperature, and the leakage current and loss after the test were tested. Compared with the original measured data in S1, the average leakage current increase rate of the 50 capacitors after the high temperature durability life test was 267%, the average loss increase rate was 188%, and the average capacity attenuation rate was 23%;
[0049] S3. After the high temperature durability life test in step S2, the capacitors were dissected and the surface of the aluminum foil was observed. It was found that there was no abnormality on the surface of the anode foil, but 32 of the 50 capacitors had local black spots on the surface of the cathode foil, which indicated that the cathode foil had hydration reaction, thus causing the capacitor leakage current and loss to increase sharply, thus causing the capacitor to fail. The failure rate of the aluminum electrolytic capacitor constructed with the electrolyte A, cathode foil and anode foil in comparative example 1 reached 64%.
[0050] The test results of control example 1 are consistent with the test results of embodiment 1 of the present invention. The judgment method of the present invention can provide an accurate prediction of whether the capacitor will fail due to hydration. Under the premise of realizing the rapid judgment of the hydration resistance of aluminum electrolytic capacitors, the present invention can also quickly verify the compatibility of electrode foil and electrolyte without assembling them into capacitors and performing high-temperature sealing storage tests on anode foil and cathode foil respectively, and the matching results have good reliability. The method of the present invention can play an effective role in the research and development of electrolyte formulas, and can also greatly reduce the defective rate of capacitor products, reduce cost output, and improve efficiency and product quality.
[0051] Example 2
[0052] A rapid test method for the hydration resistance of aluminum electrolytic capacitors with a model of 450V 390μF and a target life cycle of 5000 hours at 105℃ is as follows: Figure 1 As shown, no pre-assembly is required, and the specific steps include the following:
[0053] S1. Take the anode foil (660VF, inorganic acid) and cathode foil (3VF, aluminum purity 99.4%) used for this type of capacitor, cut them into test samples with a size of 1 cm × 10 cm, take three anode foil test samples and three cathode foil test samples to test the initial electrical parameters, the electrical parameters include: boost time, capacity, withstand voltage value, T0 represents the value of the initial boost time, C0 represents the value of the initial capacity, and V0 represents the initial withstand voltage value. After the test, rinse the anode foil test samples and cathode foil test samples with deionized water and dry them naturally;
[0054] S2. Prepare two containers, each containing 200 mL of electrolyte B used for this type of capacitor. The water content of electrolyte B is 2.2%, the main solvent is ethylene glycol, the main solute is C10~C16 straight chain + branched carboxylic acid, the conductivity is 1250 μS / cm, and the pH is 6.35;
[0055] The anode foil test sample is immersed in the electrolyte B in a container and subjected to a high temperature sealed storage test at 150 degrees Celsius for 240 hours;
[0056] The cathode foil test sample is immersed in the electrolyte B in another container and subjected to a high temperature sealed storage test at 150 degrees Celsius for 240 hours;
[0057] S3, taking out the anode foil test sample and the cathode foil test sample in step S2, cleaning the surface of the aluminum foil with deionized water, and drying naturally, and observing that the surfaces of the anode foil test sample and the cathode foil test sample in this case are normal;
[0058] It can be preliminarily determined that under the electrolyte B, there is no abnormality on the surface of the anode foil and the cathode foil, which means that there is no obvious deterioration (i.e., the surface characteristics meet the standards), but no abnormality on the surface does not mean no hydration, so further judgment is needed;
[0059] S4, respectively test the electrical parameters of the test samples after observation in S3, with T1 representing the value of the voltage rise time after immersion, C1 representing the value of the capacity after immersion, and V1 representing the withstand voltage value after immersion;
[0060] The increase rate of boost time can be calculated according to the formula: T=[|(T1- T0)| / T0]×100%;
[0061] The capacity reduction rate can be calculated according to the formula: C=[|(C1- C0)| / C0]×100%;
[0062] The voltage resistance reduction rate can be calculated according to the formula: V=[|(V1- V0)| / V0]×100%;
[0063] The test results are: the capacity reduction rate of the anode foil test sample is 0.31% (C≤5%), the increase rate of the voltage rise time is 20% (T≤50%), and the increase rate of the withstand voltage value is 0.28% (V≤10%); the capacity reduction rate of the cathode foil test sample is 0.33% (C≤5%), the increase rate of the voltage rise time is 16% (T≤50%), and the decrease rate of the withstand voltage value is 0.38% (V≤10%);
[0064] If the anode foil satisfies the three conditions of C≤5%, T≤50%, and V≤10% at the same time, and the cathode foil satisfies the three conditions of C≤5%, T≤50%, and V≤10% at the same time, it can be determined that the hydration resistance of the aluminum electrolytic capacitor constructed with the electrolyte B, cathode foil and anode foil is qualified, which means that the aluminum electrolytic capacitor constructed with the electrolyte A, cathode foil and anode foil has good hydration resistance and will not fail due to hydration during its life cycle.
[0065] In order to further verify the reliability of the overall solution of this case, the following control test was conducted.
[0066] Comparative Example 2
[0067] The hydration resistance of an aluminum electrolytic capacitor with a model of 450V 390μF and a target life cycle of 5000 hours at 105°C was tested by a conventional method. The cathode foil, anode foil, and electrolyte B used below are the same as those in Example 2. The specific method is as follows:
[0068] S1. After cutting the anode foil and cathode foil used for the capacitor of this model, the anode foil-electrolytic paper-cathode foil-electrolytic paper are stacked and wound in the order of anode foil-electrolytic paper-cathode foil-electrolytic paper to form a core package of the capacitor. The core package is immersed in the electrolyte B used for the capacitor of this model and assembled into an aluminum shell to obtain a 450V 390μF aluminum electrolytic capacitor. After the capacitor is pressurized at 475V and aged for 2 hours, 50 capacitors are randomly selected and numbered and tested, and the average leakage current is 0.13 mA, and the average loss is 4.3%;
[0069] S2. The 50 capacitors in S1 were placed in a 105°C oven for a 5000h high temperature durability life test. After the test, the capacitors were taken out and returned to room temperature. The leakage current and loss after the test were tested. Compared with the original data measured in S1, the average leakage current increase rate of the 50 capacitors after the high temperature durability life test was 2.7%, the average loss increase rate was 120%, and the average capacity attenuation rate was 5.6%.
[0070] S3. After the high temperature durability life test in step S2, the capacitor was dissected and the surface of the aluminum foil was observed. It was found that there was no abnormality on the surface of the anode foil and the cathode foil, which indicated that the anode foil and the cathode foil had good hydration resistance. The aluminum electrolytic capacitor constructed with the electrolyte B, cathode foil and anode foil in comparative example 2 would not suffer from hydration failure during its life cycle.
[0071] The test results of control example 2 are consistent with the test results of embodiment 2 of the present invention. The judgment method of the present invention can provide an accurate prediction of whether the capacitor will fail due to hydration. Under the premise of realizing the rapid judgment of the hydration resistance of aluminum electrolytic capacitors, the present invention can also quickly verify the compatibility of electrode foil and electrolyte without assembling them into capacitors and performing high-temperature sealing storage tests on anode foil and cathode foil respectively, and the matching results have good reliability. The method of the present invention can play an effective role in the research and development of electrolyte formulas, and can also greatly reduce the defective rate of capacitor products, reduce cost output, and improve efficiency and product quality.
[0072] Example 3
[0073] A rapid test method for the hydration resistance of aluminum electrolytic capacitors with a model of 410V 940μF and a target life cycle of 5000 hours at 105℃ is as follows: Figure 1 As shown, no pre-assembly is required, and the specific steps include the following:
[0074] S1. Take the anode foil (610VF, borated) and cathode foil (4VF, aluminum purity 99.4%) used for this type of capacitor, cut them into test samples with a size of 1 cm × 10 cm, take three anode foil test samples and three cathode foil test samples to test the initial electrical parameters, the electrical parameters include: boost time, capacity, withstand voltage value, T0 represents the value of the initial boost time, C0 represents the value of the initial capacity, and V0 represents the initial withstand voltage value. After the test, rinse the anode foil test samples and cathode foil test samples with deionized water and dry them naturally;
[0075] S2. Prepare two containers, each containing 200 mL of electrolyte C used for this type of capacitor. The water content of electrolyte C is 2.9%, the main solvent is ethylene glycol, the main solute is C10~C16 straight-chain carboxylic acid, the conductivity is 1750 μS / cm, and the pH is 6.4;
[0076] The anode foil test sample is immersed in the electrolyte C in a container and subjected to a high temperature sealed storage test at 105 degrees Celsius for 168 hours;
[0077] The cathode foil test sample is immersed in the electrolyte C in another container and subjected to a high temperature sealed storage test at 105 degrees Celsius for 168 hours;
[0078] S3, taking out the anode foil test sample and the cathode foil test sample in step S2, cleaning the surface of the aluminum foil with deionized water, and drying naturally, and observing that the surfaces of the anode foil test sample and the cathode foil test sample in this case are normal;
[0079] It can be preliminarily determined that under the electrolyte C, there is no abnormality on the surface of both the anode foil and the cathode foil, which means that there is no obvious deterioration (i.e., the surface characteristics meet the standards), but no abnormality on the surface does not mean no hydration, so further judgment is needed;
[0080] S4, respectively test the electrical parameters of the test samples after observation in S3, with T1 representing the value of the voltage rise time after immersion, C1 representing the value of the capacity after immersion, and V1 representing the withstand voltage value after immersion;
[0081] The increase rate of boost time can be calculated according to the formula: T=[|(T1- T0)| / T0]×100%;
[0082] The capacity reduction rate can be calculated according to the formula: C=[|(C1- C0)| / C0]×100%;
[0083] The voltage resistance reduction rate can be calculated according to the formula: V=[|(V1- V0)| / V0]×100%;
[0084] The test results are: the capacity reduction rate of the anode foil test sample is 1.0% (C≤5%), the increase rate of the voltage rise time is 6% (T≤50%), and the increase rate of the withstand voltage value is 0.93% (V≤10%); the capacity reduction rate of the cathode foil test sample is 77.2% (C>5%), the increase rate of the voltage rise time is 300% (T>50%), and the voltage withstand value reduction rate is 53% (V>10%);
[0085] If the anode foil satisfies the three conditions of C≤5%, T≤50%, and V≤10% at the same time, but the cathode meets the three conditions of C>5%, T>50%, and V>10% at the same time, it can be determined that the aluminum electrolytic capacitor constructed with the electrolyte C, cathode foil, and anode foil has unqualified hydration resistance, which means that the aluminum electrolytic capacitor constructed with the electrolyte A, cathode foil, and anode foil has poor hydration resistance and will fail due to hydration during its life cycle. Therefore, after initially determining that there is no hydration phenomenon in the anode foil and cathode foil (that is, there is no obvious abnormality or obvious degradation in the surface characteristics), the next step of electrical parameter testing must be carried out to obtain reliable inspection results.
[0086] In order to further verify the reliability of the overall solution of this case, the following control test was conducted.
[0087] Comparative Example 3
[0088] The hydration resistance of an aluminum electrolytic capacitor with a model of 410V 940μF and a target life cycle of 105°C 5000 hours was tested by a conventional method. The cathode foil, anode foil, and electrolyte C used below were the same as those in Example 3. The specific method is as follows:
[0089] S1. After cutting the anode foil and cathode foil used for the capacitor of this model, the anode foil-electrolytic paper-cathode foil-electrolytic paper are stacked and wound in the order of anode foil-electrolytic paper-cathode foil-electrolytic paper to form a core package of the capacitor. The core package is immersed in the electrolyte C used for the capacitor of this model and then assembled into an aluminum shell to obtain a 410V 940μF aluminum electrolytic capacitor. After the capacitor is pressurized at 435V and aged for 2 hours, 50 capacitors are randomly selected and numbered and tested, and the average leakage current is 0.27 mA and the average loss is 5.8%;
[0090] S2. The 50 capacitors in S1 were placed in a 105°C oven for a 5000h high temperature durability life test. After the test, the capacitors were taken out and returned to room temperature. The leakage current and loss after the test were tested. Compared with the original data measured in S1, the average leakage current increase rate of the 50 capacitors after the high temperature durability life test was 331%, the average loss increase rate was 209%, and the average capacity attenuation rate was 31%.
[0091] S3. After the high temperature durability life test in step S2, the capacitors were dissected and the surface of the aluminum foil was observed. It was found that there was no abnormality on the surface of the anode foil, but black spots appeared on the surface of the cathode foil of 18 of the 50 capacitors, indicating that the cathode foil had hydration reaction, which led to increased leakage current and loss of the capacitor, thus causing the capacitor to fail. The failure rate of the aluminum electrolytic capacitor constructed with the electrolyte C, cathode foil and anode foil in Comparative Example 3 was 36%.
[0092] The test results of control example 3 are consistent with the test results of embodiment 3 of the present invention. The judgment method of the present invention can provide an accurate prediction of whether the capacitor will fail due to hydration. Under the premise of realizing the rapid judgment of the hydration resistance of aluminum electrolytic capacitors, the present invention can also quickly verify the compatibility of electrode foil and electrolyte without assembling them into capacitors and performing high-temperature sealing storage tests on anode foil and cathode foil respectively, and the matching results have good reliability. The method of the present invention can play an effective role in the research and development of electrolyte formulas, and can also greatly reduce the defective rate of capacitor products, reduce cost output, and improve efficiency and product quality.
[0093] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A rapid detection method for the hydration resistance of aluminum electrolytic capacitors, characterized in that: The steps include: The initial electrical parameters of the samples of anode foil and cathode foil were tested respectively, and then they were immersed in electrolyte respectively, and sealed and stored for no more than 350 hours at at least 100°C. After the test, their surface characteristics were observed. If the surface characteristics of both do not meet the standards, the corresponding aluminum electrolytic capacitor composed of the anode foil, cathode foil, and electrolyte is judged to be unqualified in terms of hydration resistance; If the surface characteristics of both or one of them meet the standards, it is necessary to further test the electrical parameters after immersion and calculate the increase or decrease rate of the electrical parameters; The calculated value of the increase rate or decrease rate of the electrical parameter is compared with the judgment value. If the calculated value of the increase rate or decrease rate of the electrical parameter exceeds the judgment value, it is determined that the hydration resistance of the corresponding aluminum electrolytic capacitor composed of the anode foil, cathode foil, and electrolyte is unqualified; otherwise, if it does not exceed the judgment value, it is determined that the hydration resistance of the corresponding aluminum electrolytic capacitor composed of the anode foil, cathode foil, and electrolyte is qualified. The electrical parameters include: boost time, capacity, and withstand voltage value; based on the initial electrical parameters and the electrical parameters after immersion detected, the boost time increase rate, capacity reduction rate, and withstand voltage value reduction rate are calculated respectively, and the boost time increase rate is represented by T; the capacity reduction rate is represented by C; and the withstand voltage value reduction rate is represented by V; The judgment value corresponding to the capacity reduction rate C is 5%; the judgment value corresponding to the boost time increase rate T is 50%; the judgment value corresponding to the withstand voltage reduction rate V is 10%; If the anode foil and / or cathode foil have at least one of the following conditions: C>5%, T>50%, V>10%, then the corresponding aluminum electrolytic capacitor composed of such anode foil, cathode foil, and electrolyte is judged to be unqualified in hydration resistance; If the anode foil and the cathode foil simultaneously satisfy the following three conditions: C≤5%, T≤50%, and V≤10%, then the hydration resistance of the corresponding aluminum electrolytic capacitor composed of the anode foil, cathode foil, and electrolyte is determined to be qualified.
2. The rapid detection method for the hydration resistance of aluminum electrolytic capacitors according to claim 1 is characterized in that: The temperature of the sealed storage test is 105° C.-150° C., and the time is 168 hours-336 hours.
3. The rapid detection method for the hydration resistance of aluminum electrolytic capacitors according to claim 1 or 2, characterized in that: The number of samples of anode foil and cathode foil to be tested is at least 3 pieces respectively, the size of the samples is 1cm×5cm~1cm×10cm, and the amount of electrolyte used is sufficient to completely immerse the samples.
4. The rapid detection method for the hydration resistance of aluminum electrolytic capacitors according to claim 1 or 2, characterized in that: The surface characteristics not meeting the standards means that black spots and / or black irregular stripes can be observed; the surface characteristics meeting the standards means that black spots and / or black irregular stripes cannot be clearly observed.
Citation Information
Patent Citations
Test method for rapidly verifying waterproof capacity of low-voltage aluminum electrolytic capacitor
CN117330870A
Inspection method for inhibiting treatment process for reacting electrolytic capacitor aluminum foil oxidation film with water
CN101452768A
Method for manufacturing anodic foil of aluminum electrolytic capacitor
CN101707141A
Formation method for anode foil of intermediate-voltage aluminum electrolytic capacitor
CN102709059A
Method for improving specific volume and hydration resistance of low-voltage anode formed foil of aluminum electrolytic capacitor
CN112582176A