Laser-ultraviolet-microwave multi-energy field coupling ultra-precision machining system and method
Through laser-ultraviolet light-microwave multi-energy field coupling technology, the plastic deformation and chemical modification of brittle photoelectric materials are regulated, and the problem of difficult to take into account the processing efficiency and quality of brittle photoelectric materials in traditional technology is solved, achieving high efficiency and low damage super-efficiency Precision processing effect.
Patent Information
- Application Number
- CN202410447047.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-15
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-04-15
AI Technical Summary
The prior art is difficult to achieve high efficiency, high precision and ultra-precision processing of brittle photoelectric materials at the same time, especially in the processing of hard and soft brittle materials, surface fragmentation, microcracks, and subsurface lattice distortion, and traditionally The control accuracy of the machining machine tool is not sufficient to meet the requirements of submicron and nanoscale.
Using laser-ultraviolet light-microwave multi-energy field coupling, the plastic deformation ability of the material is regulated through the heating effect of the laser, and the chemical modification effect of ultraviolet light and microwave initiator is used to reduce the mechanical removal of the material. Resistance, achieving efficient and near-damage-free processing of complex microstructures and surfaces.
It realizes efficient and near-destructive ultra-precision machining of complex microstructures and shapes of brittle photoelectric materials, improves processing efficiency and accuracy, reduces tool wear and subsurface damage, and meets the high quality and accuracy of materials in high-tech fields. Require.
Smart Images

Figure CN118268871B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of ultra-precision machining, and in particular to a laser-ultraviolet-microwave multi-energy field coupling high-efficiency ultra-precision composite machining system and method for brittle optoelectronic materials. Background Art
[0002] This statement merely provides background information related to the present invention and does not necessarily constitute prior art.
[0003] In recent years, due to their excellent thermal and chemical stability, hard and brittle optoelectronic materials such as single crystal silicon, silicon carbide, gallium nitride, and soft and brittle optoelectronic materials such as calcium fluoride, zinc selenide, and lithium niobate have been widely used in high-tech fields such as national defense, transportation, medical treatment, aviation, and aerospace. However, hard and brittle optoelectronic materials usually have the material characteristics of high hardness, low fracture toughness, and strong wear resistance, which makes it difficult to achieve high-efficiency and low-damage processing; although the hardness of soft and brittle optoelectronic materials is much lower than that of hard and brittle optoelectronic materials, they have the characteristics of strong anisotropy and low fracture toughness, resulting in single mechanical processing that is prone to surface scratches and relatively poor surface uniformity, and high control accuracy requirements for processing machine tools. Traditionally, chemical mechanical polishing that uses chemical reactions between polishing liquid and workpiece materials and mechanical operations between workpieces and abrasives can obtain workpieces with high surface quality, but the processing efficiency is extremely low (generally a material removal rate of several microns to tens of microns per hour). In recent years, with the rapid development of ultra-precision processing technology and equipment, ductile domain processing technology that controls processing conditions to achieve surface and sub-surface crack-free processing of brittle optoelectronic materials is considered to be a high-surface quality processing method that can replace polishing. Ductile domain processing of brittle optoelectronic materials is essentially the contact and scratching of the workpiece by the tool or grinder at the nanoscale, inducing plastic deformation of the workpiece surface material, achieving material removal and surface forming. Although ductile domain processing can increase material removal efficiency by tens to hundreds of times compared to polishing, the critical cutting depth of pure ductile domain cutting or grinding is still relatively low (between a few nanometers and tens of nanometers), and cannot simultaneously meet the processing quality and processing efficiency requirements of brittle optoelectronic materials.
[0004] Ultra-precision machining of hard and brittle optoelectronic materials (such as silicon carbide, aluminum oxide, silicon) and soft and brittle optoelectronic materials (such as calcium fluoride, zinc selenide) faces many challenges, such as surface fragmentation, microcracks, subsurface lattice distortion, etc., and it is difficult to simultaneously achieve high-efficiency and high-precision machining of hard and brittle optoelectronic materials and soft and brittle optoelectronic materials using traditional single or composite machining machine tools. For example, patent CN116921708A proposes a method for laser ultrasonic assisted turning, which efficiently couples the laser and ultrasonic energy fields to the lathe through a specially designed tool holder to achieve laser ultrasonic multi-field assisted turning of titanium alloy micro-textured surfaces. However, when the laser preheats the material, the temperature difference between the processing area and the unprocessed area is too large, which can easily cause inconsistent expansion and contraction of the material, resulting in thermal cracks on the surface of the material.
[0005] Patent CN220388961U combines grinding and ultrasonic machining to obtain a composite grinding machine, which can improve material removal efficiency on the one hand, and effectively reduce grinding force on the other hand to obtain a better grinding surface. However, the control accuracy of the ordinary grinder used is relatively low (micron-level accuracy), while the machine tool control accuracy required by general brittle optoelectronic materials is at the submicron and nanometer level, so this composite machining machine cannot achieve high-efficiency, high-quality, ultra-precision machining of brittle optoelectronic materials.
[0006] Patent CN116423302A proposes a laser-assisted ultrasonic grinding tool holder and processing method for hard and brittle materials. However, soft and brittle materials have low hardness and strong anisotropy and low fracture toughness. Abrasive particles are easily embedded in the residual workpiece surface during ultra-fine machining. At the same time, the uneven heating of the surface material during the grinding process can easily cause problems such as cracking of the machined surface, which in turn affects the machining quality and efficiency of brittle optoelectronic materials.
[0007] Patent CN 117066904A discloses a multi-energy field composite processing system for brittle materials. On the one hand, the system utilizes the efficient heating effect of nanosecond laser to quickly reduce the hardness of the surface material of the workpiece to be processed, improve the fracture toughness of the material, and improve the machinability of the brittle material. On the other hand, the system utilizes the respective processing characteristics of liquid jet, turning tool, micro-milling cutter or grinding head to realize efficient and precise processing of micro-grooves with complex curves and depths that can be controlled in real time or efficient, precise, and nearly damage-free forming processing of complex surfaces. The system is particularly suitable for forming processing of the surfaces of materials with low hardness and high brittleness or high hardness and high brittleness. The system has high surface accuracy and no sub-surface microcrack damage, and can realize economical, efficient, nearly damage-free precision and ultra-precision processing of complex microstructures and surfaces of brittle materials. However, the patent uses the mechanical force of jet, turning tool, micro-milling cutter or grinding head to form the workpiece treated by laser heating, which is essentially a "single" mechanical material removal process. Therefore, mechanical damage such as phase change, amorphization, stacking fault, dislocation, twin and nanocrystal will inevitably occur on the subsurface of the workpiece, although for most brittle material devices, the processed workpiece without crack damage on the subsurface can meet the application requirements. However, the extreme environment application scenarios of brittle optoelectronic devices lead to extremely high requirements on the processing quality of brittle workpiece materials. Not only can the subsurface not have microcracks, but also stacking fault, dislocation, nanocrystal and other crystal distortions and defects. Therefore, the use of a single laser-assisted processing cannot meet the needs of efficient ultra-precision damage-free processing of brittle optoelectronic materials. It is urgent to further chemical-mechanical composite processing of the brittle workpiece material after laser-assisted turning or grinding to achieve material removal without crystal defects near the "elastic domain". Summary of the invention
[0008] In view of the prominent contradiction between the processing efficiency and processing quality of difficult-to-process brittle optoelectronic materials, the purpose of the present invention is to provide a high-efficiency ultra-precision composite processing system and method of laser-ultraviolet-microwave multi-energy field coupling. The system comprises two interchangeable linkage modules, namely laser-ultraviolet grinding and laser-microwave turning. The heating effect of the laser is used to regulate the plastic deformation ability of the brittle optoelectronic material. At the same time, the chemical modification effect of microwaves and thermal initiators, and ultraviolet light and photoinitiators is used to reduce the mechanical removal resistance of the workpiece surface material, thereby reducing tool wear and sub-surface damage in the turning and grinding processes, and ultimately achieving high-efficiency, near-damage-free ultra-precision processing of complex microstructures and surfaces of brittle optoelectronic materials.
[0009] The present invention achieves the above-mentioned purpose through the following technical solutions:
[0010] In the first aspect, the present invention provides a multi-energy field coupling ultra-precision composite processing system for brittle optoelectronic materials, namely, a laser-ultraviolet grinding and laser-microwave turning multi-energy field composite processing system, comprising a CNC machine tool, on which a rotary table is installed that can rotate and reciprocate in the X and Y directions for clamping workpieces; a Z-axis movable platform that reciprocates in the Z direction; and a multi-energy field coupling ultra-precision composite processing unit, wherein the multi-energy field coupling ultra-precision composite processing unit comprises a laser processing unit, an ultraviolet processing unit, a microwave processing unit, a grinding processing unit, a turning processing unit and a liquid spray device;
[0011] When laser-ultraviolet ultrafine grinding is performed, the laser emitting head of the laser generating assembly of the laser processing unit is connected to the laser generator through a focusing optical path; the ultraviolet emitting head of the ultraviolet generating assembly is connected to the ultraviolet generator; the laser emitting head, the ultraviolet emitting head, and the liquid spray device are located on one side of the rotary table, and the grinding processing unit is fixed to the Z-axis movable platform; the liquid spray device is used to spray the photosensitive active lubricating liquid onto the surface of the workpiece;
[0012] When performing laser-microwave single-point turning composite processing, the laser emission head of the laser generating component of the laser processing unit is directly connected to the laser generator, and the microwave emission head of the microwave generating component is connected to the microwave generator; the laser emission head, the microwave emission head, and the liquid spray device are located on one side of the rotary table; the turning processing unit is placed on the movable platform of the Z axis of the machine tool; the liquid spray device is used to spray the thermosensitive active lubricant onto the surface of the workpiece.
[0013] As a further technical solution, the thermosensitive active lubricating fluid contains a thermosensitive initiator, and the thermosensitive initiator chemically reacts with the soft and brittle workpiece material under the action of microwaves.
[0014] As a further technical solution, the photosensitive active lubricating fluid contains a photosensitive initiator, and the photosensitive initiator chemically reacts with the hard and brittle workpiece material under the action of ultraviolet light.
[0015] As a further technical solution, the turning processing unit includes a single-point diamond turning tool, which is offset from the laser transmitter head, the microwave transmitter head and the spray device. Through the mutual cooperation of laser, microwave and the single-point diamond turning tool, the workpiece is subjected to laser and microwave assisted turning processing under the catalysis of thermosensitive lubricating fluid.
[0016] As a further technical solution, the grinding processing unit includes a diamond grinding head, which is offset from the laser emission head, the ultraviolet light emission head and the spray device. Through the mutual cooperation of laser, ultraviolet light and the diamond grinding head, the workpiece is subjected to laser and ultraviolet light assisted grinding under the catalysis of photosensitive lubricating fluid.
[0017] As a further technical solution, a multi-degree-of-freedom CCD observation microscope is also included. The CCD microscope is adsorbed on the Z-axis movable platform through a magnetic base to assist in precise tool alignment.
[0018] In a second aspect, the present invention provides a processing method of a laser-ultraviolet-microwave multi-energy field coupling ultra-precision composite processing system based on the brittle optoelectronic material, as follows:
[0019] When machining soft and brittle material workpieces:
[0020] S1: Clamp the processed soft and brittle material workpiece onto the rotary table of the machine tool;
[0021] S2: Control the Z-axis movable platform to move the laser transmitter and the focusing light path to one side of the workpiece, and determine the relative position between the laser transmitter and the workpiece surface;
[0022] S3: Turn on the laser generator to perform single pulse dot focusing, adjust the laser spot position by reciprocating and rotating the rotary table in the X direction, and adjust the laser defocus amount by reciprocating the Z-axis movable platform;
[0023] S4: Install the turning unit on the Z-axis movable platform of the machine tool, and then move the turning tool of the turning unit to the side where the laser transmitter head is located;
[0024] S5: Adjust the inclination angle of the laser beam to maintain a suitable offset distance from the turning tool, start the CNC machine tool, perform laser-assisted rough turning on the workpiece, and after the processing is completed, turn off the laser generator and retract the tool to a safe position;
[0025] S6: withdraw the laser generator to a safe position, install the microwave transmitter head on the Z-axis movable platform, control the Z-axis movable platform to move the microwave transmitter head above the soft and brittle material workpiece, and determine the relative position between the microwave transmitter head and the surface of the soft and brittle material workpiece;
[0026] S7: according to the workpiece material, a corresponding thermosensitive active lubricant is configured, and the configured thermosensitive active lubricant is evenly sprayed onto the surface of the workpiece after laser-assisted turning through a micro-lubricating spray device;
[0027] S8: Turn on the microwave generator to irradiate the processing position of the workpiece in step S6 with microwaves, induce the decomposition of the thermal decomposition initiator in the thermosensitive active lubricant, generate active free radicals, chemically modify the soft and brittle material workpiece under mechanical stress, reduce the elastic modulus of the workpiece surface material, and improve the fracture toughness of the hard and brittle material. The microwave heating position is adjusted by the reciprocating movement and rotation of the rotary table in the X direction of the CNC machine tool, and the size of the microwave irradiation area is adjusted by the reciprocating movement of the Z-axis movable platform;
[0028] S9: Adjust the tilt angle of the microwave transmitter head to maintain the set offset distance with the turning tool, start the CNC machine tool, and start microwave-assisted ultra-precision turning of the complex surface of the workpiece after rough machining by the laser-single-point diamond turning tool. After the machining is completed, retract the tool to a safe position;
[0029] When machining hard and brittle workpieces:
[0030] S10: clamping the processed hard and brittle material workpiece onto the rotary table of the machine tool;
[0031] S11: Remove the turning unit, install the grinding unit on the Z-axis movable platform, then move the grinding head to one side of the workpiece, and control the relative position between the grinding unit and the surface of the hard and brittle material through the rotary table and the Z-axis movable platform to complete the tool setting;
[0032] S12: adjusting the inclination angle of the laser beam, maintaining a set offset distance with the grinding head, setting grinding parameters and laser parameters, starting the high-precision CNC machine tool, and starting laser-assisted rough grinding of the workpiece. After the processing is completed, turning off the laser generator and retracting the tool to a safe position;
[0033] S13: withdraw the laser generator to a safe position, install the ultraviolet light emitting head on the Z-axis movable platform, control the Z-axis movable platform to move the ultraviolet light emitting head above the workpiece to be processed, and determine the relative position between the ultraviolet light emitting head and the workpiece surface;
[0034] S14: preparing a corresponding photosensitive active grinding fluid according to the processing material, and spraying the prepared photosensitive active lubricating fluid evenly onto the surface of the workpiece after the laser-assisted grinding through a micro-lubricating spray device;
[0035] S15: Turn on the UV generator, adjust the inclination angle of the UV beam, maintain the set offset distance from the grinding unit, set the UV parameters and grinding parameters, use the UV radiation energy to induce the photoinitiator in the photosensitive lubricant to crack and produce alkyl free radical activity, start the high-precision CNC machine tool, and start UV-assisted ultra-precision grinding of complex surfaces of the workpiece after laser-diamond grinding. After the processing is completed, retract the tool to a safe position.
[0036] As a further technical solution, before the workpiece to be processed is installed on the workpiece fixture, the workpiece to be processed is placed in anhydrous ethanol for ultrasonic cleaning for a set time to remove dirt on the surface of the workpiece.
[0037] As a further technical solution, the critical cutting depth d in step S6 c =λ(H / E) 1 / 2 (K c / H) 2 , where λ is about 8.7, is the brittle-plastic transition factor of the workpiece material, H is the hardness of the workpiece material after laser heating, E is the elastic modulus of the workpiece material after laser heating, and K c It is the fracture toughness of the workpiece material after laser heating.
[0038] As a further technical solution, during laser-ultraviolet superfinishing composite processing or laser-microwave single-point turning composite processing, the distance between the tool action point on the workpiece and the laser beam action point is 0.4 to 1.0 mm, the selection range of the distance between the single-point diamond turning tool action point and the offset microwave emission head is 1.0 to 10.0 cm, and the selection range of the distance between the single-point diamond consolidated abrasive action point and the offset ultraviolet light emission head is 1.0 to 10.0 cm.
[0039] The beneficial effects of the present invention are as follows:
[0040] The processing system of the present invention can detachably connect the laser-single-point turning composite processing unit, the microwave-single-point turning composite processing unit, the laser-superfine grinding composite processing unit and the ultraviolet light-superfine grinding composite processing unit, thus realizing multiple uses of one machine, that is, realizing the laser-microwave single-point turning composite processing unit and the laser-ultraviolet light superfine grinding composite processing unit at the same time, and realizing multiple composite linkage processing on the same machine tool. At the same time, when the present invention performs laser-ultraviolet superfine grinding, the heating effect of the laser is first used to regulate the plastic deformation ability of the brittle optoelectronic material, and then the chemical modification effect of ultraviolet light and the photoinitiator is used. , reduce the mechanical removal resistance of the workpiece surface material, and then reduce the abrasive wear and sub-surface damage in the grinding process, and finally achieve efficient, near-damage-free ultra-precision machining of complex microstructures and surfaces of brittle optoelectronic materials; when performing laser-microwave single-point turning composite processing, first use the heating effect of the laser to regulate the plastic deformation ability of the brittle optoelectronic material, and then use the chemical modification effect of microwaves and thermal initiators to reduce the mechanical removal resistance of the workpiece surface material, and then reduce the tool wear and sub-surface damage in the turning process, and finally achieve efficient, near-damage-free ultra-precision machining of complex microstructures and surfaces of brittle optoelectronic materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.
[0042] Figure 1 It is a schematic diagram of the overall structure of an example of the present invention;
[0043] Figure 2 It is a schematic diagram of each processing unit of the present invention;
[0044] Figure 3 This is a diagram showing the use status of the laser-ultraviolet light assisted grinding processing unit according to an embodiment of the present invention;
[0045] Figure 4 This is a diagram of the use status of the laser-microwave assisted turning processing unit according to an embodiment of the present invention;
[0046] Among them, 1-CNC machine tool, 2-high-speed air-floating spindle, 3-rotary table, 4-workpiece fixture, 5-workpiece, 6-CCD observation microscope, 7-Z-axis moving platform, 8-laser processing unit, 9-ultraviolet processing unit, 10-microwave processing unit, 11-spray device, 12-turning processing unit, 13-grinding processing unit. DETAILED DESCRIPTION
[0047] It should be noted that the following detailed descriptions are illustrative and intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used in the present invention have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.
[0048] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit the exemplary embodiments according to the present invention. As used herein, unless otherwise explicitly stated in the present invention, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "include" and / or "include" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof;
[0049] With the rapid development of the power electronics industry, optoelectronic products have put forward higher requirements on the miniaturization, complexity, processing accuracy and processing quality of devices. To meet the needs of high-quality and efficient forming processing of miniaturized and complex products, multiple processing methods need to be coordinated with each other to process the required high-performance products; therefore, this embodiment provides a high-efficiency ultra-precision composite processing system and method of laser-ultraviolet light-microwave multi-energy field coupling.
[0050] Among them, laser processing uses the high energy density of laser to process the surface to be processed, change the physical and chemical properties of the surface material, directly remove the material or improve the machinability of the material. Therefore, the heating effect of the laser is used to reduce the surface hardness of the brittle optoelectronic material and improve the plastic deformation ability of the material, thereby helping to increase the critical cutting depth d of the brittle-plastic transition removal of the brittle optoelectronic material. c It can effectively increase the cutting depth of a single feed of the tool or abrasive, while reducing the processing damage caused by mechanical stress removal, achieving high-efficiency plastic deformation removal of brittle optoelectronic materials, and ultimately obtaining a high-precision, high-quality processing surface, breaking through the difficulty of efficient, low-damage ultra-precision processing of brittle optoelectronic materials.
[0051] UV processing is to use the high energy characteristics of ultraviolet light to carry out rapid photochemical reaction or photothermal effect on the surface of materials to achieve material removal or surface modification. UV processing has the advantages of fast processing speed, small heat-affected zone, and high processing precision, especially for the processing of hard and brittle optoelectronic materials. First, ultraviolet light has high photon energy, which can directly destroy the chemical bonds on the surface of the material and achieve rapid photochemical reaction. At the same time, the rapid energy transfer reduces the thermal effect and avoids the deformation and damage of the material caused by thermal effects. Secondly, the wavelength of ultraviolet light is short. By adjusting the irradiation angle and focal length of the ultraviolet light source, specific areas on the surface of the material can be accurately selectively processed, which is of great significance for the micro-nano processing of hard and brittle optoelectronic material products with complex shapes and fine structures. Finally, compared with traditional chemical corrosion, UV processing has the advantages of energy saving, green and safety. At the same time, UV processing has good compatibility and can be combined with turning, grinding and laser processing technology to form a composite processing technology to further improve processing efficiency and precision.
[0052] Microwave heating is a non-contact heating method. Microwaves directly act on polar molecules or ions inside the material to achieve rapid heating of the material. Microwave heating can avoid material deformation and damage caused by friction or pressure in traditional contact heating, and is particularly suitable for processing soft and brittle materials with complex shapes or thin walls. Secondly, compared with traditional heating methods, microwave heating can reduce the temperature difference between the surface and the inside of the material, achieve overall uniform heating, and prevent cracking or breakage caused by local overheating. In addition, the microwave power can be precisely controlled, thereby achieving fine regulation of the surface temperature of the workpiece during the processing process. By adjusting the output power and processing time of the microwave, the degree of heating and the amount of removal of the material can be precisely controlled, and precise processing size and shape control can be achieved.
[0053] This embodiment provides a multi-energy field coupling high-efficiency ultra-precision composite processing system for brittle optoelectronic materials, such as Figure 1 , Figure 2 As shown, it includes a CNC machine tool 1, which adopts an existing high-precision CNC machine tool. The power system of the CNC machine tool 1 is connected to a high-speed air-floating spindle 2 to achieve radial and axial movement of the spindle of the high-speed air-floating spindle 2.
[0054] One end of the high-speed air-floating spindle 2 is connected to the power system of the CNC machine tool 1, and the other end is connected to the rotary table 3; the rotary table 3 is coaxial with the high-speed air-floating spindle 2, and the rotary table 3 can output a motion rotating around its own axis.
[0055] The rotary table 3 is connected to the workpiece clamp 4 and can drive the workpiece clamp 4 to move; the workpiece clamp 4 can be an existing vacuum adsorption workpiece fixture, and its specific structure is not described in detail here. The rotary table 3 can also move on the X / Y axis.
[0056] A Z-axis moving platform 7 is also installed on the bed of the numerically controlled machine tool 1 . The Z-axis moving platform 7 can output horizontal motion, and the output motion direction is perpendicular to the axial direction of the high-speed air-floating spindle 2 .
[0057] The moving part of the Z-axis moving platform 7 is connected to a platform, and the platform is detachably connected to a processing unit, and the processing unit includes a laser processing unit 8, an ultraviolet processing unit 9, a microwave processing unit 10, a spray device 11, a turning processing unit 12, and a grinding processing unit 13.
[0058] When in use, the corresponding processing unit can be installed on the mobile mechanism according to actual needs.
[0059] like Figure 2 As shown, the laser-ultraviolet light-superfine grinding composite processing unit includes a grinding processing unit 13, a laser processing unit 8, an ultraviolet light processing unit 9, and a spray device 11. The laser emission head in the laser processing unit is connected to the laser generator, and the laser beam generated by the laser generator can be emitted to the workpiece 5 to be processed through the laser emission head. The ultraviolet light emitting head in the ultraviolet processing unit 9 is connected to the ultraviolet light generator, and the ultraviolet light rays generated by the ultraviolet light generator can be emitted to the workpiece 5 to be processed through the ultraviolet light emitting head. The spray device 11 can evenly spray the photosensitive lubricating liquid required in the processing process onto the surface of the workpiece to be processed. The grinding processing unit 13 includes a grinding power system, a high-speed air-floating spindle, a grinding head fixture, etc. The grinding power system can output rotational motion. The grinding power system is connected to the high-speed air-floating spindle. A grinding head fixture is provided on the high-speed air-floating spindle. The grinding head fixture is connected to a grinding head. The grinding head adopts a diamond grinding head. The abrasive particle size of the diamond grinding head is 0.5 to 36 μm. The selection range of the distance between the action point of the laser beam and the action point of the rear diamond grinding head is 0.4 to 1.0 mm, and the laser spot diameter is 7 mm.
[0060] In this embodiment, the laser generator in the laser processing unit 8 emits nanosecond laser, with a spot diameter of 7 mm, a laser pulse width of 2.0 to 500 ns, a wavelength of 1060 to 1085 nm, an average output power greater than 100 W, a power range of 0.1 to 120 W, and a frequency of 1.0 to 4000 KHz.
[0061] In this embodiment, the ultraviolet light generator in the ultraviolet light processing unit 9 has an ultraviolet light emitting head with a power of 950 W, a wavelength of 100 to 400 nm, and a repetition frequency of 30 KHz to 150 KHz.
[0062] Based on the above processing system, a method for laser-ultraviolet light-superfinishing multi-energy field composite processing of soft and brittle material workpieces includes the following steps:
[0063] S1: Pre-process the workpiece;
[0064] S2: Clamp the processed workpiece onto the rotary table of the machine tool;
[0065] S3: Install the laser transmitter head on the Z-axis movable platform, control the Z-axis movable platform to move the laser transmitter head and the focusing light path to the right side of the workpiece to be processed, and determine the relative position of the laser transmitter head and the workpiece surface;
[0066] S4: Set laser processing parameters, turn on the laser generator for single pulse dot focusing, adjust the laser spot position through the reciprocating and rotating motion of the machine tool rotary table in the X direction, and adjust the laser defocus amount through the reciprocating motion of the Z-axis movable platform;
[0067] S5: Install the grinding unit on the Z-axis movable platform of the machine tool, then move the diamond grinding head of the grinding unit to the right of the workpiece, and control the relative position between the grinding unit and the workpiece surface through the rotary table and the Z-axis movable platform to complete the tool setting;
[0068] S6: Turn on the laser generator, adjust the inclination angle of the laser beam through the three-axis slide, maintain a suitable offset distance from the grinding head, set the grinding parameters and laser parameters, start the high-precision CNC machine tool, and start laser-assisted rough grinding of the workpiece. After the processing is completed, turn off the laser generator and retract the tool to a safe position;
[0069] S7: withdraw the laser generator to a safe position via the three-axis slide, install the UV light emitter on the three-axis slide bracket, control the Z-axis movable platform to move the UV light emitter to the top of the workpiece to be processed, and determine the relative position between the UV light emitter and the workpiece surface;
[0070] S8: preparing a corresponding photosensitive active lubricant according to the processing material, and spraying the prepared photosensitive active lubricant evenly onto the surface of the workpiece after laser-assisted grinding at a flow rate of 10 to 200 mL / h through a micro-lubricating spray device;
[0071] S9: Turn on the UV generator, adjust the inclination angle of the UV beam through the three-axis slide, maintain a suitable offset distance from the grinding unit, set the UV parameters and grinding parameters, use the UV radiation energy to induce the photoinitiator in the photosensitive lubricant to crack and produce alkyl free radical activity, start the high-precision CNC machine tool, and start UV-assisted ultra-precision grinding of complex surfaces of the workpiece after laser-diamond grinding. After the processing is completed, retract the tool to a safe position.
[0072] When performing laser-UV ultrafine grinding, the present invention first utilizes the heating effect of the laser to regulate the plastic deformation ability of the brittle optoelectronic material, and then utilizes the chemical modification effect of ultraviolet light and photoinitiator to reduce the mechanical removal resistance of the surface material of the workpiece, thereby reducing the abrasive tool wear and sub-surface damage in the grinding process, and ultimately achieving efficient, nearly damage-free ultraprecision processing of complex microstructures and surfaces of brittle optoelectronic materials.
[0073] The photosensitive active lubricant in this embodiment comprises the following components: propylene glycol, deionized water, triethanolamine, and a photosensitive initiator. The wavelength and intensity of the ultraviolet rays, as well as the grinding depth, feed rate, grinding head speed, and workpiece speed are set according to the composition and content of the initiator in the photosensitive lubricant and the flow rate of the solution, as well as the hardness, elastic modulus, fracture toughness, and interface separation strength of the photoinitiator modified layer of the workpiece material (the selection of parameters is based on the mechanical properties of the modified layer).
[0074] In some embodiments of the present invention, the photoinitiator is selected from one or more combinations of benzil dimethyl ketal.
[0075] The decomposition chemical equation of benzyl dimethyl ketal under ultraviolet irradiation is:
[0076]
[0077] The chemical equation for the reaction between hard and brittle workpiece materials and free radicals is as follows:
[0078]
[0079] Among them, B is soft and brittle workpiece material.
[0080] Ultraviolet light plays a vital role in achieving efficient application of photoactive lubricants. Ultraviolet light can stimulate the decomposition of photoactive initiators in photoactive lubricants, releasing free radicals with strong chemical reactivity, which then interact with the surface of hard and brittle optoelectronic materials to perform precise surface modification, reduce the hardness and wear resistance of the surface material, and ultimately improve the machinability of the material. In addition, through the synergistic lubrication and cooling effects of propylene glycol, glycerin and water, the contact stress and grinding heat between the diamond abrasives and the modified layer can be effectively regulated, ensuring the accuracy of the processing process and the excellent surface quality of the material.
[0081] Furthermore, the laser-microwave-single-point turning composite processing unit includes a turning processing unit 12, a laser processing unit 8, a microwave processing unit 10, and a spray device 11. The microwave rays generated by the microwave generator in the microwave processing unit 10 can be emitted to the workpiece 5 to be processed through a magnetron. The single-point turning tool adopts a single-point diamond turning tool, the tool radius of the single-point diamond turning tool is 0.5-2.5mm, the selection range of the distance between the single-point diamond turning tool action point and the offset laser beam action point is 0.4-1.0mm, and the laser spot diameter is 7mm.
[0082] In this embodiment, the microwave generator in the microwave processing unit 10 has a microwave transmitting head power of 1030 W, an output power of 100 W to 1250 W, and a frequency of 2.45 GHz.
[0083] The laser-microwave-single-point turning multi-energy field composite processing method for hard and brittle material workpieces using the above system includes the following steps:
[0084] S10: clamping the processed hard and brittle material workpiece onto the rotary table of the machine tool;
[0085] S11: Remove the turning unit, install the grinding unit on the Z-axis movable platform, then move the grinding head to one side of the workpiece, and control the relative position between the grinding unit and the surface of the hard and brittle material through the rotary table and the Z-axis movable platform to complete the tool setting;
[0086] S12: adjusting the inclination angle of the laser beam, maintaining a set offset distance with the grinding head, setting grinding parameters and laser parameters, starting the high-precision CNC machine tool, and starting laser-assisted rough grinding of the workpiece. After the processing is completed, turning off the laser generator and retracting the tool to a safe position;
[0087] S13: withdraw the laser generator to a safe position, install the ultraviolet light emitting head on the Z-axis movable platform, control the Z-axis movable platform to move the ultraviolet light emitting head above the workpiece to be processed, and determine the relative position between the ultraviolet light emitting head and the workpiece surface;
[0088] S14: preparing a corresponding photosensitive active grinding fluid according to the processing material, and spraying the prepared photosensitive active lubricating fluid evenly onto the surface of the workpiece after the laser-assisted grinding through a micro-lubricating spray device;
[0089] S15: Turn on the UV generator, adjust the inclination angle of the UV beam, maintain the set offset distance from the grinding unit, set the UV parameters and grinding parameters, use the UV radiation energy to induce the photoinitiator in the photosensitive lubricant to crack and produce alkyl free radical activity, start the high-precision CNC machine tool, and start UV-assisted ultra-precision grinding of complex surfaces of the workpiece after laser-diamond grinding. After the processing is completed, retract the tool to a safe position.
[0090] When performing laser-microwave single-point turning composite processing, the plastic deformation ability of the brittle optoelectronic material is first regulated by the heating effect of the laser, and then the chemical modification effect of microwaves and thermal initiators is used to reduce the mechanical removal resistance of the workpiece surface material, thereby reducing tool wear and sub-surface damage during the turning process, and ultimately achieving efficient, near-damage-free ultra-precision processing of complex microstructures and surfaces of brittle optoelectronic materials.
[0091] As a further technical solution, before the workpiece to be processed is installed on the workpiece fixture, the workpiece to be processed is placed in anhydrous ethanol for ultrasonic cleaning for a set time to remove dirt on the surface of the workpiece.
[0092] As a further technical solution, during laser-microwave turning composite processing or laser-ultraviolet grinding composite processing, the distance between the tool action point on the workpiece and the laser beam action point is 0.4 to 1.0 mm.
[0093] It should be particularly noted that the laser beam of this system is generally used to heat the workpiece to be processed, and the diamond turning tool, diamond grinding head and laser beam do not come into contact during the process of acting on the workpiece to be processed.
[0094] The thermosensitive active lubricant in this embodiment comprises the following components: propylene glycol, triethanolamine, thermosensitive initiator, and vegetable oil. The wavelength, intensity, cutting depth, feed rate, and workpiece speed of the microwave ray are set according to the composition, content, and flow rate of the initiator in the thermosensitive cutting fluid, as well as the hardness, elastic modulus, fracture toughness, and interface separation strength of the thermal initiator modified layer of the workpiece material (the selection of parameters is based on the mechanical properties of the modified layer).
[0095] The thermal initiator is selected from one or more combinations of hydrogen peroxide, di-p-tert-butylcyclohexyl peroxydicarbonate (TBCP) or tert-butyl peroxypivalate (BPP).
[0096] The equation for the thermal decomposition reaction of di-p-tert-butylcyclohexyl peroxydicarbonate (TBCP) is as follows:
[0097]
[0098] The equation for the thermal decomposition reaction of inorganic peroxide thermal decomposition initiator hydrogen peroxide is as follows:
[0099]
[0100] The chemical equation for the reaction between soft and brittle workpiece materials and free radicals is as follows:
[0101]
[0102] Among them, A is a soft and brittle workpiece material.
[0103] Thermosensitive initiators are a class of compounds that can generate free radicals after being heated, and then implement controllable chemical modification of soft and brittle optoelectronic materials under mechanical force. The role of microwaves is crucial to the efficient application of thermosensitive active lubricants. Microwaves can stimulate the decomposition of thermosensitive active initiators in thermosensitive active lubricants, releasing free radicals with strong chemical reaction activity, which then interact with the surface of soft and brittle optoelectronic materials to achieve rapid chemical modification. At the same time, microwaves effectively transfer heat energy to the surface of the workpiece through polar molecules adsorbed on the surface of the workpiece, increasing the plastic deformation capacity of the workpiece surface and modified layer materials. Finally, the workpiece surface material softened and modified by microwave heating is efficiently mechanically removed by the diamond turning tool. In addition, through the synergistic lubrication effect of propylene glycol and triethanolamine, the contact stress between the single-point diamond turning tool and the modified layer can be effectively regulated, ensuring the accuracy of the processing process and the excellent surface quality of the material.
[0104] In this embodiment, the two composite processing units can share a set of laser generators and laser emission heads.
[0105] In this embodiment, the moving mechanism 7 is also provided with a magnetic seat, and an image acquisition element is fixed on the top of the magnetic seat. The image acquisition element is used to acquire images of the workpiece to assist in precise tool alignment. The image acquisition element adopts a CCD observation microscope 6.
[0106] Example 1
[0107] like Figure 2 As shown, this specific embodiment provides a method for laser-ultraviolet light-superfinishing multi-energy field composite processing of gallium nitride, which specifically includes the following steps:
[0108] S1: Place the GaN wafer in anhydrous ethanol for ultrasonic cleaning for 10 minutes to obtain a clean and uncontaminated workpiece to be processed;
[0109] S2: Use a digital display heater to fix the workpiece to be processed on the aluminum alloy sample table through paraffin, start the silent oil-free vacuum pump, clamp the aluminum alloy sample table to the rotary table of the machine tool through vacuum adsorption, and adjust the spindle rotation accuracy to less than 1μm through a high-precision micrometer;
[0110] S3: Install the laser transmitter head on the three-axis slide bracket, control the Z-axis movable platform to move the laser transmitter head to the right side of the workpiece to be processed, and determine its relative position with the workpiece surface;
[0111] S4: Start the high-precision CNC machine tool 1, turn on the control system, control the moving mechanism to move the diamond grinding head to the right of the workpiece 5 processed in Example 2, adjust the CCD observation microscope, adjust the relative position of the grinding head and the workpiece surface by controlling the moving mechanism and the air-floating spindle in the observation state, and read the coordinate values of the tool machine tool coordinate system X and Z;
[0112] S5: Set the laser processing parameters, laser spot diameter 30μm, pulse width 100ns, wavelength 1080nm, power 6W, repetition frequency 50KHz, scanning speed 1mm / s. Turn on the laser generator, adjust the laser spot position through the reciprocating and rotating movement of the machine tool air-floating high-speed electric spindle in the X direction, and adjust the laser defocus through the reciprocating movement of the Z-axis movable platform;
[0113] S6: Start the high-speed air-floating spindle 2 and the air-floating spindle assembly, control the Z-axis single feed of 0.5 μm, the X-axis single grinding length of 2.7 cm, and the feed speed of 10 μm / min to perform trial grinding, then observe the morphology of the center of the sample after grinding with the help of a white light interferometer, and use a high-precision micrometer to adjust the height of the diamond grinding head 22 in the Y direction by adjusting the screw on the air-floating spindle assembly until the center of the sample after grinding is flat and has no micro-convex bodies, and the tool setting is completed;
[0114] S7: Turn on the laser generator, perform single-pulse laser dot focusing on a specific position of the workpiece, adjust the distance between the laser and the workpiece by the reciprocating motion of the Z-axis movable platform, and use a microscope to observe the platform position corresponding to the spot with good roundness and uniform energy on the workpiece surface, and finally determine the laser working focus position;
[0115] S8: Use the three-axis slide to adjust the laser beam and the diamond grinding head to a 30-degree tilt and a 0.5mm offset distance. Set the grinding parameters to workpiece speed 1000rpm, grinding head speed 3000rpm, grinding depth DOC 0.5μm, and feed speed 1μm / min. Set the laser parameters to laser spot diameter 7mm, pulse width 100ns, wavelength 1080nm, power 6W, and repetition frequency 50KHz;
[0116] S9: Start the high-precision CNC machine tool and start the laser-assisted ultra-precision grinding rough processing of the workpiece. After the processing is completed, the tool is retracted to a safe position;
[0117] S10: withdraw the laser to a safe position via the three-axis slide, install the UV light emitter on the three-axis slide bracket, control the Z-axis movable platform to move the UV light emitter to the top of the workpiece to be processed, and determine the relative position between the UV light emitter and the workpiece surface;
[0118] S11: Prepare the corresponding photosensitive active lubricant according to the processing material, and prepare the main components and contents of the lubricant: the photosensitive active lubricant contains 1.0% to 10.0% of photoinitiator, 0.5% to 5.0% of propylene glycol, 0.5% to 5.0% of triethanolamine, and the balance is the base liquid deionized water.
[0119] S12: Set the UV processing parameters, turn on the UV generator to irradiate the rough processing position of the workpiece with UV light, and spray the configured photosensitive active lubricant evenly on the surface of the workpiece after laser-assisted grinding through the micro-lubricant spray device at a flow rate of 100 ml / h, inducing the decomposition of the photoinitiator in the photosensitive active lubricant to produce alkyl free radical activity, chemically modify the workpiece under mechanical stress, reduce the elastic modulus of the workpiece surface material, and improve the fracture toughness of the brittle optoelectronic material. Adjust the UV irradiation position through the reciprocating and rotating motion of the machine tool rotary table in the X direction, and adjust the size of the UV irradiation area through the reciprocating motion of the Z-axis movable platform;
[0120] S13: Start the high-precision CNC machine tool and start ultraviolet-assisted ultra-precision grinding and finishing of the gallium nitride wafer after laser-diamond grinding. After the processing is completed, retract the tool to a safe position, and turn off the laser generator, ultraviolet generator, high-speed air-floating spindle and air-floating spindle assembly, control system, CCD observation microscope and cooling and lubrication system.
[0121] Example 2
[0122] like Figure 3 As shown, this specific embodiment provides a method for ultra-precision machining of lithium niobate wafers by laser-microwave single-point lathe, which specifically includes the following steps:
[0123] S1: Place the lithium niobate wafer in anhydrous ethanol for ultrasonic cleaning for 10 minutes to obtain a clean and uncontaminated workpiece to be processed;
[0124] S2: Use a digital display heater to fix the workpiece to be processed on the aluminum alloy sample table through paraffin, start the silent oil-free vacuum pump, clamp the aluminum alloy sample table to the rotary table of the machine tool through vacuum adsorption, and adjust the spindle rotation accuracy to less than 1μm through a high-precision micrometer;
[0125] S3: Install the laser transmitter head on the three-axis slide bracket, control the Z-axis movable platform to move the laser transmitter head to the right side of the workpiece to be processed, and determine its relative position with the workpiece surface;
[0126] S4: Start the high-precision CNC machine tool, turn on the control system, control the Z-axis movable platform to move the single-point diamond turning tool with a tool radius of 0.5 mm to the right of the workpiece, adjust the multi-degree-of-freedom CCD observation microscope, and adjust the relative position of the single-point diamond turning tool and the workpiece surface by controlling the Z-axis movable platform and the X-axis movable air-floating high-speed electric spindle in the observation state, and read the X and Z coordinate values of the tool machine tool coordinate system;
[0127] S5: Set the laser processing parameters, laser spot diameter 30μm, pulse width 100ns, wavelength 1080nm, power 6W, repetition frequency 50KHz, scanning speed 1mm / s. Turn on the laser generator, adjust the laser spot position through the reciprocating and rotating movement of the machine tool air-floating high-speed electric spindle in the X direction, and adjust the laser defocus through the reciprocating movement of the Z-axis movable platform;
[0128] S6: Start the air-floating high-speed electric spindle, control the Z-axis single feed of 0.1μm, the X-axis single cutting radius of 5.5mm, and the feed speed of 5μm / min to conduct a test cut, then use a white light interferometer to observe the shape of the micro-convex body in the center of the test cut sample, and use a high-precision micrometer to adjust the height of the single-point diamond turning tool in the Y direction by adjusting the screw on the tool holder until the center of the sample is flat and free of micro-convex bodies after the test cut, and the tool setting is completed;
[0129] S7: Turn on the laser generator, perform single-pulse laser dot focusing on a specific position of the workpiece, adjust the distance between the laser and the workpiece by the reciprocating motion of the Z-axis movable platform, and use a microscope to observe the platform position corresponding to the spot with good roundness and uniform energy on the workpiece surface, and finally determine the laser working focus position;
[0130] S8: Use a precision three-axis slide to adjust the laser beam and the diamond turning tool to a 30-degree tilt and a 0.5mm offset distance. Set the turning parameters to spindle speed 2000rpm, cutting depth DOC 50nm, and feed rate 1μm / min. Set the laser parameters to laser spot diameter 7mm, pulse width 100ns, wavelength 1080nm, power 6W, and repetition frequency 50KHz;
[0131] S9: Start the high-precision CNC machine tool and start laser-assisted ultra-precision single-point diamond turning rough machining of the workpiece. After the machining is completed, retract the tool to a safe position;
[0132] S10: withdraw the laser generator to a safe position via the three-axis slide table, install the microwave transmitter head on the three-axis slide table bracket, control the Z-axis movable platform to move the microwave transmitter head to the top of the workpiece to be processed, and determine the relative position between the microwave transmitter head and the workpiece surface;
[0133] S11: Prepare corresponding thermosensitive active lubricating liquid according to the processing material, and prepare the main components and contents of the lubricating liquid: the free radical thermosensitive initiator is benzyl dimethyl ketal, the mass percentage is 5.0%; the mass percentage of propylene glycol is 0.5%; the mass percentage of glycerol is 0.5%.
[0134] S12: Set microwave processing parameters, turn on the microwave generator to perform microwave heating on the rough processing position of the workpiece, and spray the configured thermosensitive active lubricant evenly on the surface of the workpiece after laser-assisted turning through the micro-lubrication spray device at a flow rate of 50ml / h, inducing the thermal decomposition initiator in the thermosensitive active cutting fluid to decompose and produce active free radicals to chemically modify the workpiece under mechanical stress, reduce the elastic modulus of the workpiece surface material, and improve the fracture toughness of the brittle optoelectronic material. The microwave heating position is adjusted by the reciprocating and rotating motion of the machine tool rotary table in the X direction, and the size of the microwave irradiation area is adjusted by the reciprocating motion of the Z-axis movable platform;
[0135] S13: Start the high-precision CNC machine tool and start microwave-assisted ultra-precision cutting and finishing of the lithium niobate wafer after rough machining by laser-single-point diamond turning tool. After the machining is completed, retract the tool to a safe position, and turn off the laser generator, microwave generator, high-speed air-floating spindle and air-floating spindle assembly, control system, CCD observation microscope and cooling and lubrication system.
[0136] The above description is only the preferred embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.
Claims
1. Laser-ultraviolet-microwave multi-energy field coupling ultra-precision machining system, including a CNC machine tool, on which a rotary table is installed that can rotate and reciprocate in the X and Y directions for clamping workpieces; a Z-axis movable platform can reciprocate in the Z direction; It is characterized in that It also includes a multi-energy field coupling ultra-precision composite processing unit, which includes a laser processing unit, an ultraviolet light processing unit, a microwave processing unit, a grinding processing unit, a turning processing unit and a liquid spray device; When laser-ultraviolet ultrafine grinding is performed, the laser emission head of the laser generating assembly of the laser processing unit is connected to the laser generator through a focusing optical path; the ultraviolet emission head of the ultraviolet generating assembly is connected to the ultraviolet generator; the laser emission head, the ultraviolet emission head, and the liquid spray device are located on one side of the rotary table, and the grinding processing unit is fixed to the Z-axis movable platform; the liquid spray device is used to spray a photosensitive active lubricant onto the surface of the workpiece; the photosensitive active lubricant contains a photosensitive initiator, and the photosensitive initiator reacts chemically with the hard and brittle workpiece material under the induction of ultraviolet light; the grinding processing unit includes a diamond grinding head, and the diamond grinding head is offset to the laser emission head, the ultraviolet emission head and the spray device, and through the mutual cooperation of laser, ultraviolet light and the diamond grinding head, the workpiece is subjected to laser and ultraviolet light assisted grinding under the catalysis of the photosensitive lubricant; When performing laser-microwave single-point turning composite processing, the laser emission head of the laser generating component of the laser processing unit is directly connected to the laser generator, and the microwave emission head of the microwave generating component is connected to the microwave generator; the laser emission head, the microwave emission head, and the liquid spray device are located on one side of the rotary table; the turning processing unit is placed on the movable platform of the Z-axis of the machine tool; the liquid spray device is used to spray a thermosensitive active lubricant onto the surface of the workpiece; the thermosensitive active lubricant contains a thermosensitive initiator, and the thermosensitive initiator chemically reacts with the soft and brittle workpiece material under the induction of microwaves; the turning processing unit includes a single-point diamond turning tool, and the single-point diamond turning tool is offset to the laser emission head, the microwave emission head and the spray device. Through the mutual cooperation of laser, microwave and the single-point diamond turning tool, the workpiece is subjected to laser and microwave assisted turning processing under the catalysis of the thermosensitive lubricant.
2. The laser-ultraviolet-microwave multi-energy field coupling ultra-precision machining system as claimed in claim 1, It is characterized in that It also includes a multi-degree-of-freedom CCD observation microscope, which is adsorbed on the Z-axis movable platform through a magnetic base to assist in precise tool setting.
3. A processing method of the laser-ultraviolet-microwave multi-energy field coupling ultra-precision processing system according to any one of claims 1 to 2, It is characterized in that as follows: When machining soft and brittle material workpieces: S1: Clamp the processed soft and brittle material workpiece onto the rotary table of the machine tool; S2: Control the Z-axis movable platform to move the laser transmitter and the focusing light path to one side of the workpiece, and determine the relative position between the laser transmitter and the workpiece surface; S3: Turn on the laser generator to perform single pulse dot focusing, adjust the laser spot position by reciprocating and rotating the rotary table in the X direction, and adjust the laser defocus amount by reciprocating the Z-axis movable platform; S4: Install the turning unit on the Z-axis movable platform of the machine tool, and then move the turning tool of the turning unit to the side where the laser transmitter head is located; S5: Adjust the inclination angle of the laser beam to maintain a suitable offset distance from the turning tool, start the CNC machine tool, perform laser-assisted rough turning on the workpiece, and after the processing is completed, turn off the laser generator and retract the tool to a safe position; S6: withdraw the laser generator to a safe position, install the microwave transmitter head on the Z-axis movable platform, control the Z-axis movable platform to move the microwave transmitter head above the soft and brittle material workpiece, and determine the relative position between the microwave transmitter head and the surface of the soft and brittle material workpiece; S7: according to the workpiece material, a corresponding thermosensitive active lubricant is configured, and the configured thermosensitive active lubricant is evenly sprayed onto the surface of the workpiece after laser-assisted turning through a micro-lubricating spray device; S8: Turn on the microwave generator to irradiate the processing position of the workpiece in step S6 with microwaves, induce the decomposition of the thermal decomposition initiator in the thermosensitive active lubricant, generate active free radicals, chemically modify the soft and brittle material workpiece under mechanical stress, reduce the elastic modulus of the workpiece surface material, and improve the fracture toughness of the hard and brittle material. The microwave heating position is adjusted by the reciprocating movement and rotation of the rotary table in the X direction of the CNC machine tool, and the size of the microwave irradiation area is adjusted by the reciprocating movement of the Z-axis movable platform; S9: Adjust the tilt angle of the microwave transmitter head to maintain the set offset distance with the turning tool, start the CNC machine tool, and start microwave-assisted ultra-precision turning of the complex surface of the workpiece after rough machining by the laser-single-point diamond turning tool. After the machining is completed, retract the tool to a safe position; When machining hard and brittle workpieces: S10: clamping the processed hard and brittle material workpiece onto the rotary table of the machine tool; S11: Remove the turning unit, install the grinding unit on the Z-axis movable platform, then move the grinding head to one side of the workpiece, and control the relative position between the grinding unit and the surface of the hard and brittle material through the rotary table and the Z-axis movable platform to complete the tool setting; S12: adjusting the inclination angle of the laser beam, maintaining a set offset distance with the grinding head, setting grinding parameters and laser parameters, starting the high-precision CNC machine tool, and starting laser-assisted rough grinding of the workpiece. After the processing is completed, turning off the laser generator and retracting the tool to a safe position; S13: withdraw the laser generator to a safe position, install the ultraviolet light emitting head on the Z-axis movable platform, control the Z-axis movable platform to move the ultraviolet light emitting head above the workpiece to be processed, and determine the relative position between the ultraviolet light emitting head and the workpiece surface; S14: preparing a corresponding photosensitive active grinding fluid according to the processing material, and spraying the prepared photosensitive active lubricating fluid evenly onto the surface of the workpiece after the laser-assisted grinding through a micro-lubricating spray device; S15: Turn on the UV generator, adjust the inclination angle of the UV beam, maintain the set offset distance from the grinding unit, set the UV parameters and grinding parameters, use the UV radiation energy to induce the photoinitiator in the photosensitive lubricant to crack and produce alkyl free radical activity, start the high-precision CNC machine tool, and start UV-assisted ultra-precision grinding of complex surfaces of the workpiece after laser-diamond grinding. After the processing is completed, retract the tool to a safe position.
4. The processing method of the laser-ultraviolet-microwave multi-energy field coupling ultra-precision processing system as claimed in claim 3, It is characterized in that Before the workpiece to be processed is mounted on the workpiece fixture, the workpiece to be processed is placed in anhydrous ethanol for ultrasonic cleaning for a set time to remove dirt on the surface of the workpiece.
5. The processing method of the laser-ultraviolet-microwave multi-energy field coupling ultra-precision processing system as claimed in claim 3, It is characterized in that Critical cutting depth in step S6 d c = λ ( H / E ) 1 / 2 ( K c / H) 2 , where λ is the brittle-to-ductile transition factor of the workpiece material, H is the hardness of the workpiece material after laser heating, E is the elastic modulus of the workpiece material after laser heating, K c It is the fracture toughness of the workpiece material after laser heating.
6. The processing method of the laser-ultraviolet-microwave multi-energy field coupling ultra-precision processing system as claimed in claim 5, It is characterized in that During laser-ultraviolet superfinishing composite processing or laser-microwave single-point turning composite processing, the distance between the tool action point on the workpiece and the laser beam action point is 0.4~1.0 mm, the distance between the single-point diamond turning tool action point and the offset microwave transmitter head is selected in the range of 1.0~10.0 cm, and the distance between the single-point diamond fixed abrasive action point and the offset ultraviolet transmitter head is selected in the range of 1.0~10.0 cm.
Citation Information
Patent Citations
Laser-assisted ultrasonic grinding knife handle for hard and brittle materials and machining method
CN116423302A
Laser ultrasonic multi-field assisted turning titanium alloy micro-texture surface preparation method
CN116921708A
Multi-energy-field combined machining system and method for fragile materials
CN117066904A
Grinding machine with ultrasonic machining function
CN220388961U
Process of precision grinding of transparent materials by using laser assistance
CN109551335A
Cited By
Machining method for multi-stage laser composite modified auxiliary grinding
CN121135476A