Battery
By optimizing the composition of the electrolyte components and negative active materials in the battery, a porous and stable SEI membrane is formed, which solves the problem of insufficient battery performance in low and high temperature environments, and significantly improves low-temperature discharge performance and cycle stability.
Patent Information
- Application Number
- CN202410696074.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-31
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2044-05-31
AI Technical Summary
Existing batteries have insufficient discharge performance and cycle stability in low and high temperature environments, making it difficult to meet users' needs for battery life and portability.
By using specific compounds as electrolyte components in the battery, controlling the transition metal content, specific surface area, and the ratio of the total mass of the electrolyte to the discharge capacity in the negative active material, a porous and stable SEI membrane is formed to optimize the kinetic performance of the battery.
It significantly improves the low-temperature discharge performance and cycle stability of the battery, and improves the overall performance of the battery, especially in low-temperature environments.
Smart Images

Figure CN118281343B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of batteries, and in particular relates to a battery. Background Art
[0002] Resource shortage, energy crisis and environmental pollution are the severe challenges facing human production. Finding renewable and resource-saving secondary energy is one of the urgent tasks for the sustainable development of human society. Batteries have unique advantages such as high specific energy, high operating voltage, wide application temperature range, low self-discharge rate, long cycle life and good safety performance. They are now widely used in power supplies for household appliances such as mobile phones, portable computers, camcorders, cameras, etc., and have been gradually widely used in the fields of aviation, aerospace, navigation, artificial satellites, small medical instruments and military communication equipment. However, with the continuous improvement of people's requirements for battery life and portability, how to further balance and improve the comprehensive performance of batteries (such as low-temperature discharge performance, high-temperature cycle performance, etc.) has become a problem that needs to be solved urgently. Summary of the invention
[0003] The present invention aims to solve one of the technical problems in the related art at least to a certain extent. To this end, one object of the present invention is to provide a battery. The battery has excellent low-temperature discharge performance and cycle performance.
[0004] In one aspect of the present invention, the present invention provides a battery, comprising a positive electrode sheet, a negative electrode sheet and an electrolyte, wherein the electrolyte comprises a compound as shown in Formula 1, the mass percentage of the transition metal in the negative electrode active material of the negative electrode sheet is M, and the specific surface area of the negative electrode active material is Bm 2 / g, the ratio of the total mass of the electrolyte to the discharge capacity of the battery is N g / Ah, the mass percentage of the compound represented by Formula 1 in the electrolyte is C1, and satisfies the following formula: ,
[0005]
[0006] wherein m is an integer of 0 to 3, n is an integer of 0 to 3, and m and n are not both 0, p is an integer of 1 to 5, R0 is a single bond or a methylene group, R1 is hydrogen, halogen, a hydrocarbon group having 1 to 5 carbon atoms, or a halogenated hydrocarbon group having 1 to 5 carbon atoms, and R2, R3, and R4 are independently , , , , , or .
[0007] The battery of the present invention comprises a positive electrode sheet, a negative electrode sheet and an electrolyte, wherein the electrolyte comprises a compound represented by Formula 1. During the first charging and cycling of the battery, although the compound represented by Formula 1 can form a porous and stable SEI film on the surface of the negative electrode, effectively improving the kinetic performance of the battery, the inventors have found that the degree of influence of the SEI film formed above on the performance of the battery is related to the mass percentage M of the transition metal in the negative electrode active material of the negative electrode sheet, the specific surface area Bm of the negative electrode active material, and the specific surface area Bm of the negative electrode active material. 2 / g, the ratio of the total mass of the electrolyte to the discharge capacity of the battery N g / Ah, and the mass percentage C1 of the compound shown in Formula 1 in the electrolyte are closely related. The inventors found that when the above parameters satisfy the following formula: , the battery has excellent comprehensive performance, especially the battery has excellent low-temperature discharge performance and cycle stability. Therefore, the battery has excellent low-temperature discharge performance and cycle performance.
[0008] In some embodiments, R1 is hydrogen, halogen, methyl, ethyl, n-propyl, isopropyl, butyl, pentyl, hexyl, halogenated methyl, halogenated ethyl, halogenated n-propyl, halogenated isopropyl, halogenated butyl, halogenated pentyl or halogenated hexyl. Thus, the low temperature discharge performance and cycle performance of the battery can be improved.
[0009] In some embodiments, the compound represented by Formula 1 includes at least one of the following compounds:
[0010] , , , , , , , , , . Thereby, the low-temperature discharge performance and cycle performance of the battery can be improved.
[0011] In some embodiments, 0.005%≤M≤0.03%. Thus, the low-temperature discharge performance and cycle performance of the battery can be improved.
[0012] In some embodiments, the transition metal includes at least one of iron, copper, nickel, and zinc.
[0013] In some embodiments, 0.3%≤C1≤4%. Thus, the low-temperature discharge performance and cycle performance of the battery can be improved.
[0014] In some embodiments, 0.7≤B≤2.5. Thus, the low-temperature discharge performance and cycle performance of the battery can be improved.
[0015] In some embodiments, 2≤N≤4.5. Thus, the low-temperature discharge performance and cycle performance of the battery can be improved.
[0016] In some embodiments, the battery is a lithium battery, and the positive electrode active material of the positive electrode plate includes lithium iron phosphate material, nickel-cobalt-manganese ternary material, lithium cobalt oxide material, lithium manganese iron phosphate material, lithium manganese oxide material or nickel-manganese oxide lithium material. Thus, the low-temperature discharge performance and cycle performance of the battery can be improved.
[0017] In some embodiments, the battery is a sodium battery, and the positive electrode active material of the positive electrode plate includes a sodium iron phosphate material or a three-dimensional tunnel type Na 0.44 MnO2.
[0018] In some embodiments, the negative electrode active material of the negative electrode plate includes graphite or silicon-based materials, thereby improving the low-temperature discharge performance and cycle performance of the battery.
[0019] In some embodiments, the electrolyte further includes an electrolyte salt, and the electrolyte salt includes a lithium salt or a sodium salt.
[0020] In some embodiments, the mass of the electrolyte salt accounts for 10% to 20% based on the total mass of the electrolyte.
[0021] Additional aspects and advantages of the present invention will be given in part in the following description and in part will be obvious from the following description, or will be learned through practice of the present invention. DETAILED DESCRIPTION
[0022] The embodiments of the present invention are described in detail below, which are intended to explain the present invention but are not to be construed as limiting the present invention.
[0023] In one aspect of the present invention, the present invention provides a battery, comprising a positive electrode sheet, a negative electrode sheet and an electrolyte, wherein the electrolyte comprises a compound as shown in Formula 1, the mass percentage of the transition metal in the negative electrode active material of the negative electrode sheet is M, and the specific surface area of the negative electrode active material is Bm 2 / g, the ratio of the total mass of the electrolyte to the discharge capacity of the battery is N g / Ah, the mass percentage of the compound represented by Formula 1 in the electrolyte is C1, and satisfies the following formula: ,
[0024]
[0025] wherein m is an integer of 0 to 3, n is an integer of 0 to 3, and m and n are not both 0, p is an integer of 1 to 5, R0 is a single bond or a methylene group, R1 is hydrogen, halogen, a hydrocarbon group having 1 to 5 carbon atoms, or a halogenated hydrocarbon group having 1 to 5 carbon atoms, and R2, R3, and R4 are independently , , , , , or .
[0026] The battery of the present invention comprises a positive electrode sheet, a negative electrode sheet and an electrolyte, wherein the electrolyte comprises a compound represented by Formula 1. During the first charging and cycling of the battery, although the compound represented by Formula 1 can form a porous and stable SEI film on the surface of the negative electrode, effectively improving the kinetic performance of the battery, the inventors have found that the degree of influence of the SEI film formed above on the performance of the battery is related to the mass percentage M of the transition metal in the negative electrode active material of the negative electrode sheet, the specific surface area Bm of the negative electrode active material, and the specific surface area Bm of the negative electrode active material. 2 / g, the ratio of the total mass of the electrolyte to the discharge capacity of the battery N g / Ah, and the mass percentage C1 of the compound shown in Formula 1 in the electrolyte are closely related. The inventors found that when the above parameters satisfy the following formula: , the battery has excellent comprehensive performance, especially the battery has excellent low-temperature discharge performance and cycle stability. This is because N determines the total mass of the electrolyte in the battery, which can largely determine the number of molecules of the compound shown in Formula 1 retained in the battery. B and M greatly affect the number of molecules required for the compound shown in Formula 1 to form the SEI film. When the above formula relationship is satisfied between them, the number of molecules of the compound shown in Formula 1 in the battery can just form a complete SEI film without excess. As a result, the battery has excellent low-temperature discharge performance and cycle performance.
[0027] In some specific embodiments of the present invention, R1 is hydrogen, halogen, methyl, ethyl, n-propyl, isopropyl, butyl, pentyl, hexyl, halogenated methyl, halogenated ethyl, halogenated n-propyl, halogenated isopropyl, halogenated butyl, halogenated pentyl or halogenated hexyl. Thus, during the first charge and cycle of the battery, the compound shown in Formula 1 can be reduced on the negative electrode surface in priority to the electrolyte solvent to form a SEI film rich in sulfonate compounds and low in fluoride salt components. The formed SEI film has porosity, which is conducive to the rapid passage of ions during the charge and discharge process, so the impedance of the SEI film is low, and the formed SEI film has high stability, thereby effectively improving the kinetic performance of the battery, and improving the low-temperature discharge performance and cycle stability of the battery.
[0028] As an example, the compound represented by Formula 1 includes at least one of the following compounds:
[0029] , , , , , , , , , Therefore, during the first charge and cycle of the battery, the compound shown in Formula 1 can be preferentially reduced in the electrolyte solvent on the negative electrode surface to form an SEI film rich in sulfonate compounds and low in fluoride salt components. The formed SEI film has porosity, which is conducive to the rapid passage of ions during the charge and discharge process. Therefore, the impedance of the SEI film is low, and the formed SEI film has high stability, thereby effectively improving the kinetic performance of the battery, and improving the low-temperature discharge performance and cycle stability of the battery.
[0030] In some embodiments of the present invention, 0.005%≤M≤0.03%. For example, M is 0.005%, 0.007%, 0.01%, 0.015%, 0.02%, 0.025%, 0.03%, etc. The transition metal in the negative electrode active material has a strong electronic conductivity, has a stronger electrochemical activity than the negative electrode active material, and is easy to catalyze the reduction and decomposition of the compound shown in Formula 1. When the content of transition metal in the negative electrode active material is high, more molecules of the compound shown in Formula 1 will be required to form a SEI film that completely covers the negative electrode. As a result, the mass percentage of the transition metal in the negative electrode active material of the negative electrode pole piece is controlled within the above range, and a SEI film with low impedance and high stability can be formed, which improves the low-temperature discharge performance and cycle stability of the battery. It should be noted that the transition metal in the negative electrode active material is an impurity metal in the preparation process of the negative electrode active material. For example, the transition metal can be introduced into raw materials, equipment wear, and air dust.
[0031] As an example, the transition metal includes at least one of iron, copper, nickel, and zinc.
[0032] In some embodiments of the present invention, 0.3%≤C1≤4%. The inventors found that when C1 is controlled within the above range, the compound represented by Formula 1 can form a porous and stable SEI film on the surface of the negative electrode, significantly reduce the interface impedance, and effectively improve the kinetic performance of the battery.
[0033] In some embodiments of the present invention, 0.7≤B≤2.5. For example, B is 0.7, 0.9, 1.1, 1.3, 1.5, 1.7, 1.9, 2.1, 2.3, 2.5, etc. The surface of the negative electrode active material has active sites, and the compound shown in Formula 1 is reduced at the active sites on the surface of the negative electrode active material. The larger the specific surface area of the negative electrode active material, the more active sites there are, so more compounds shown in Formula 1 are needed to form a complete SEI film. The present application controls the specific surface area of the negative electrode active material within the above range to form a SEI film with low impedance and high stability, thereby improving the low-temperature discharge performance and cycle stability of the battery.
[0034] In some embodiments of the present invention, the negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer disposed on at least one side of the negative electrode current collector, wherein the negative electrode active material layer includes at least one of a first binder and a first conductive agent and a negative electrode active material.
[0035] In some embodiments of the present invention, the negative electrode active material may be a negative electrode active material for a battery known in the art. As an example, the negative electrode active material may include at least one of the following materials: graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, and lithium titanate, etc., preferably graphite or silicon-based materials, which have excellent cycle life, thereby improving the cycle performance and service life of the battery.
[0036] As an example, the silicon-based material may include at least one of simple silicon, silicon oxide, silicon carbon composite, silicon nitrogen composite, and silicon alloy. The tin-based material may include at least one of simple tin, tin oxide, and tin alloy.
[0037] In some embodiments of the present invention, the negative electrode current collector may be a metal foil or a composite current collector. For example, as the metal foil, a copper foil may be used. The composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material substrate. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), etc.).
[0038] In some embodiments of the present invention, the first binder may include at least one of sodium carboxymethyl cellulose (CMC), styrene-butadiene rubber (SBR), polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene oxide-containing polymers, polyvinyl pyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, polyamide-imide, polyvinyl alcohol, and sodium polyacrylate.
[0039] In some embodiments of the present invention, the first conductive agent may include at least one of natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fiber, and graphene.
[0040] In some embodiments of the present invention, the mass ratio of the negative electrode active material, the first conductive agent and the first binder is (90-99): (0-5): (1-10).
[0041] In some embodiments of the present invention, the positive electrode sheet includes a positive current collector and a positive active material layer disposed on at least one side of the positive current collector, wherein the positive active material layer includes at least one of a second binder and a second conductive agent and a positive active material.
[0042] In some embodiments of the present invention, the positive electrode current collector may include a metal foil or a composite positive electrode current collector. For example, the metal foil may be aluminum foil. The composite positive electrode current collector may include a polymer material base and a metal layer formed on at least one side of the polymer material base. For example, the composite negative electrode current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, etc.) on a polymer material substrate (such as polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT) and other substrates).
[0043] As an example, the positive electrode current collector has two surfaces facing each other in its thickness direction, and the positive electrode active material layer is disposed on any one or both of the two facing surfaces of the positive electrode current collector.
[0044] As an example, when the battery is a lithium-ion battery, the positive electrode active material includes but is not limited to lithium iron phosphate material, LiCoO2 material, LiNiO2, nickel-cobalt-manganese ternary material (LiNi x Co y Mn z O2 (x+y+z = 1, 0<x<1, 0<y<1, 0<z<1)), lithium-rich manganese-based materials (nLi2MnO3·(1-n)LiMO2 (0<n<1, M is one, two or three of Ni, Co, Mn)), lithium nickel manganese oxide (LiNi 0.5 Mn 1.5 O4) material, lithium iron manganese phosphate material, lithium manganese oxide material, nickel manganese oxide material, etc., preferably lithium iron phosphate material, nickel cobalt manganese ternary material, lithium cobalt oxide material, lithium manganese iron phosphate material, lithium manganese oxide material or nickel manganese oxide material, which have excellent cycle performance and high energy density, thereby improving the cycle stability of the battery.
[0045] In some embodiments of the present invention, the battery is a lithium battery, the negative electrode active material is graphite or silicon-based material, the positive electrode active material is lithium iron phosphate material, nickel-cobalt-manganese ternary material, lithium cobalt oxide material, lithium manganese iron phosphate material, lithium manganese oxide material, nickel-manganese oxide lithium material, the compound shown in formula 1 can significantly improve the kinetic performance of the battery under the above negative electrode active material and positive electrode active material, and satisfies the following formula: , the battery has excellent comprehensive performance, thereby improving the low-temperature discharge performance and cycle performance of the battery.
[0046] As an example, when the battery is a sodium ion battery, the positive electrode active material is not limited to a three-dimensional tunnel type Na 0.44 MnO2, P2 layered NaMO2 (M is one, two or three of Ni, Mn, Fe), NaFePO4, Na4Fe3(PO4)2P2O7, Na3V2(PO4)3, Na3V2(PO4)2F3, Na2Fe(CN)6, Na2MnFe(CN)6, etc., preferably sodium iron phosphate material or three-dimensional tunnel type Na 0.44 MnO2 has excellent cycle performance and high energy density, which can improve the cycle stability of the battery.
[0047] In some embodiments of the present invention, the battery is a sodium battery, the negative electrode active material is graphite or silicon-based material, and the positive electrode active material is sodium iron phosphate material or three-dimensional tunnel type Na 0.44 MnO2, the compound shown in Formula 1, can significantly improve the kinetic performance of the battery under the above-mentioned negative electrode active material and positive electrode active material, and satisfies the following formula: , the battery has excellent comprehensive performance, thereby improving the low-temperature discharge performance and cycle performance of the battery.
[0048] In some embodiments of the present invention, the second conductive agent includes at least one of carbon black, acetylene black, graphene, Ketjen black, and carbon fiber.
[0049] In some embodiments of the present invention, the second binder includes at least one of polytetrafluoroethylene, polyvinylidene fluoride (PVDF), polyvinyl fluoride, polyethylene, polypropylene, polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, ethylene oxide-containing polymers, polyvinyl pyrrolidone, and polyurethane.
[0050] In some embodiments of the present invention, the mass ratio of the positive electrode active material, the second conductive agent and the second binder is (90-99.5): (0.25-5): (0.25-5).
[0051] In some embodiments of the present invention, 2≤N≤4.5. For example, N is 2, 2.3, 2.5, 2.7, 3, 3.2, 3.5, 4, 4.5, etc. N can reflect the actual holding amount of the battery in the presence of the compound shown in Formula 1. The ratio N of the total mass of the electrolyte to the discharge capacity of the battery is controlled within the above range, which can effectively ensure that the electrolyte fully infiltrates into the gap between the positive electrode sheet and the negative electrode sheet, and can control the gap between the positive and negative electrodes to reduce the internal resistance. In this way, the low-temperature discharge performance and cycle stability of the battery can be improved. It should be noted that the test method for the discharge capacity of the battery of the present application is: the capacity obtained by discharging the battery at a current of 0.5C after the battery is fully charged at a current of 0.5C.
[0052] In some embodiments of the present invention, the electrolyte further includes an electrolyte salt, and the electrolyte salt includes a lithium salt or a sodium salt.
[0053] As an example, the lithium salt includes at least one of lithium hexafluorophosphate (LiPF6), lithium bis(fluorosulfonyl)imide salt (LiFSI), or bis(trifluoromethanesulfonyl)imide (LiTFSI).
[0054] As an example, the sodium salt includes at least one of sodium hexafluorophosphate, sodium tetrafluoroborate, sodium bis(fluorosulfonyl)imide salt (NaFSI), sodium bis(trifluoromethylsulfonyl)imide, sodium bis(oxalatoborate), sodium difluorobis(oxalatoborate), sodium difluorobis(oxalatophosphate), sodium tetrafluorooxalatophosphate, and sodium 4,5-dicyano-2-trifluoromethyl-imidazole.
[0055] In some embodiments of the present invention, the electrolyte further includes a solvent, and the solvent includes at least one of carbonates (such as cyclic carbonates, chain carbonates), carboxylates (such as cyclic carboxylates, chain carboxylates), ether compounds (such as cyclic ether compounds, chain ether compounds), phosphorus-containing compounds, sulfur-containing compounds and aromatic fluorine-containing compounds.
[0056] As an example, the solvent includes at least one of ethylene carbonate (EC), propylene carbonate (PC), diethyl carbonate (DEC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), fluoroethylene carbonate (FEC), propyl butyrate (PB), ethyl butyrate (EB), propyl propionate (PP), ethyl propionate (EP), methyl propionate (MP), propyl acetate (PA), ethyl acetate (EA), methyl acetate (MA), propyl formate (PF), ethyl formate (EF), methyl formate (MF), and γ-butyrolactone.
[0057] In some embodiments of the present invention, based on the total mass of the electrolyte, the mass proportion of the electrolyte salt is 10% to 20%. For example, the mass proportion of the electrolyte salt is 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, etc. The mass proportion of the electrolyte salt in the electrolyte is controlled within the above range to ensure that the battery has stable electrochemical properties.
[0058] In some embodiments of the present invention, the battery further comprises a separator, which includes but is not limited to glass fiber, non-woven fabric, polyethylene, polypropylene or polyvinylidene fluoride.
[0059] The present invention is described below with reference to specific embodiments. It should be noted that these embodiments are merely illustrative and do not limit the present invention in any way.
[0060] Example 1
[0061] (1) Preparation of the compound of formula 1-1
[0062] 500g of dimethyl sulfoxide and 50g of ethylene carbonate were added to a three-necked flask containing 108.1g of mannitol, and then 2g of pyridine was added as a catalyst. The three-necked flask was heated to 70°C and stirred for 6h at a negative pressure of 500Pa. 115.9g of sulfonyl fluoride was added and stirred for 6h at a negative pressure of 500Pa, and then the heating was stopped and the temperature was lowered to room temperature. 500g of methyl ethyl ether was added for recrystallization, and the mixture was filtered under reduced pressure to obtain a white solid (compound of formula 1-1).
[0063] (2) Preparation of electrolyte: In an inert atmosphere (water <0.1ppm, oxygen <1ppm), ethylene carbonate (EC), ethyl methyl carbonate (EMC) and ethyl acetoacetate (EA) were mixed at a mass ratio of EC:EMC:EA=3:3:4. After mixing evenly, lithium bis(fluorosulfonyl)imide (LiFSI) and lithium hexafluorophosphate (LiPF6) were added. The mass proportion of LiFSI in the electrolyte was 2wt%, and the mass proportion of LiPF6 in the electrolyte was 10wt%. Then, the compound of formula 1-1 was added. Based on the total mass of the electrolyte, the mass proportion of the compound of formula 1-1 was 0.6wt%.
[0064] (3) Preparation of positive electrode sheets: The positive electrode active material (lithium iron phosphate), conductive agent (acetylene black) and binder poly (vinylidene fluoride) are dispersed in N-methylpyrrolidone (NMP) solvent at a mass ratio of 96:2:2, and the mixture is fully stirred to form a uniform positive electrode slurry (the solid content in the positive electrode slurry is 60wt%). The positive electrode slurry is evenly coated on the positive electrode current collector aluminum foil, and the positive electrode sheets are obtained after drying, rolling and slitting.
[0065] (4) Preparation of negative electrode sheet: Disperse the negative electrode active material (graphite), conductive agent (acetylene black), binder (sodium carboxymethyl cellulose) and styrene-butadiene rubber (SBR) in a proper amount of deionized water at a mass ratio of 95:2:2:1, stir and mix thoroughly to form a uniform negative electrode slurry (solid content in the negative electrode slurry is 50wt%), and evenly coat the negative electrode slurry on the negative electrode current collector copper foil. After drying, rolling and slitting, a negative electrode sheet is obtained. The transition metal content M in the graphite is 0.01wt%, the transition metal is iron, and the specific surface area Bm of the graphite is 2 / g is 1.2g / cm 3 The test methods for the transition metal content in graphite and the specific surface area of graphite are given in standard GB / T 24533-2019.
[0066] (5) Preparation of battery: stack the positive electrode sheet, separator and negative electrode sheet in order, place the separator between the positive electrode sheet and the negative electrode sheet to play a role of isolation, and then wind to obtain a bare cell, and place the bare cell in an outer packaging shell. After drying, inject the electrolyte prepared in step (2), and the total mass of the electrolyte is 8g. After vacuum packaging, standing, forming, shaping and other processes, the preparation of the battery is completed, and its rated capacity is 2Ah. The ratio of the total mass of the electrolyte to the discharge capacity of the battery is 4g / Ah. Specifically, the capacity of the battery after being fully charged at a current of 0.5C and then fully discharged at a current of 0.5C is 2Ah.
[0067] in, .
[0068] Example 2
[0069] The difference between Example 2 and Example 1: The compound of Formula 1 used in Example 2 is Formula 1-2. The preparation process of the compound of Formula 1-2 is different from that of the compound of Formula 1-1 in that the amount of dimethyl carbonate added is 100 g, and the amount of sulfonyl fluoride added is 57.95 g.
[0070] Example 3
[0071] The difference between Example 3 and Example 1: The compound shown in Formula 1 used in Example 3 is Formula 1-3. The preparation process of the compound of Formula 1-3 is different from that of the compound of Formula 1-1 in that the amount and order of material addition are different. Specifically, 500g of dimethyl sulfoxide and 57.95g of sulfonyl fluoride are added to a reactor containing 108.1g of mannitol, and then 2g of pyridine is added as a catalyst, and the reactor is heated to 70°C, and stirred for 6h at a negative pressure of 500Pa. Then 50g of dimethyl carbonate and 57.95g of sulfonyl fluoride are added, and the stirring is continued for 6h at a negative pressure of 500Pa, and then the heating is stopped and the temperature is cooled to room temperature. 500g of methyl ethyl ether is added for recrystallization, and the mixture is filtered under reduced pressure to obtain a white solid (compound of Formula 1-3).
[0072] Example 4
[0073] The difference between Example 4 and Example 1: The compound of Formula 1 used in Example 4 is Formula 1-4. The preparation process of the compound of Formula 1-4 is different from that of the compound of Formula 1-2 in that this example uses 1,2,3,5,6,7-heptanhexaol instead of mannitol.
[0074] Example 5
[0075] The difference between Example 5 and Example 1: The compound of Formula 1 used in Example 5 is Formula 1-5. The preparation process of the compound of Formula 1-5 is different from that of the compound of Formula 1-2 in that 1,3,7-hydroxy-2,6-methylol-heptane is used in this example instead of mannitol. 100g of dimethyl carbonate is adjusted to 115.9g of sulfonyl fluoride.
[0076] Example 6
[0077] The difference between Example 6 and Example 1 is that the compound of Formula 1 used in Example 6 is Formula 1-6. The preparation process of the compound of Formula 1-6 is different from that of the compound of Formula 1-1 in that decanol is used in this example instead of mannitol. The amount of dimethyl carbonate added is 100 g, and the amount of sulfonyl fluoride added is 173.85 g.
[0078] Example 7
[0079] The difference between Example 7 and Example 1: The compound of Formula 1 used in Example 7 is Formula 1-7. The preparation process of the compound of Formula 1-7 is different from that of the compound of Formula 1-6 in that the amount of dimethyl carbonate added is 150 g, and the amount of sulfonyl fluoride added is 115.9 g.
[0080] Example 8
[0081] The difference between Example 8 and Example 1: The compound of Formula 1 used in Example 8 is Formula 1-8. The preparation process of the compound of Formula 1-8 is different from that of the compound of Formula 1-1 in that this example uses 1,2,3,4,5,6-heptanhexaol instead of mannitol.
[0082] Example 9
[0083] The difference between Example 9 and Example 1 is that the compound of Formula 1 used in Example 9 is Formula 1-9. The preparation process of the compound of Formula 1-9 is different from that of the compound of Formula 1-1 in that this example uses fluorohexanehexol instead of mannitol.
[0084] Example 10
[0085] The difference between Example 10 and Example 1 is that the compound of Formula 1 used in Example 10 is Formula 1-10. The preparation process of the compound of Formula 1-10 is different from that of the compound of Formula 1-1 in that this example uses butanetetracycline instead of mannitol. The amount of sulfonyl fluoride added is 57.95 g.
[0086] Embodiment 11
[0087] The difference between Example 11 and Example 1 is that the transition metal content M in the graphite of Example 11 is 0.005wt%. .
[0088] Example 12
[0089] The difference between Example 12 and Example 1 is that the transition metal content M in the graphite of Example 12 is 0.03wt%. .
[0090] Embodiment 13
[0091] The difference between Example 13 and Example 1 is that the specific surface area of the graphite in Example 13 is 0.7 g / cm 3 .in, .
[0092] Embodiment 14
[0093] The difference between Example 14 and Example 1 is that the specific surface area of the graphite in Example 14 is 2.5 g / cm 3 .in, .
[0094] Embodiment 15
[0095] The difference between Example 15 and Example 1 is that in step (2) of Example 15, based on the total mass of the electrolyte, the mass proportion C1 of the compound of Formula 1-1 is 0.3 wt %. Wherein, .
[0096] Example 16
[0097] The difference between Example 16 and Example 1 is that in step (2) of Example 16, based on the total mass of the electrolyte, the mass proportion C1 of the compound of Formula 1-1 is 4.0 wt%. Wherein, .
[0098] Embodiment 17
[0099] The difference between Example 17 and Example 1 is that in step (4) of Example 17, the specific surface area of graphite is 2.7 g / cm 3 .in, .
[0100] Embodiment 18
[0101] The difference between Example 18 and Example 1 is that in step (4) of Example 18, the specific surface area of graphite is 0.6 g / cm 3 .in, .
[0102] Embodiment 19
[0103] The difference between Example 19 and Example 1 is that the total mass of the electrolyte in Example 19 is 10 g, the discharge capacity of the battery is 2 Ah, and the ratio of the total mass of the electrolyte in Example 19 to the discharge capacity of the battery is 5. .
[0104] Embodiment 20
[0105] The difference between Example 20 and Example 1 is that the total mass of the electrolyte in Example 20 is 3.6 g, the discharge capacity of the battery is 2 Ah, and the ratio of the total mass of the electrolyte in Example 20 to the discharge capacity of the battery is 1.8. .
[0106] Embodiment 21
[0107] The difference between Example 21 and Example 1 is that the transition metal content M in the graphite of Example 21 is 0.05wt%. .
[0108] Embodiment 22
[0109] The difference between Example 22 and Example 1 is that the transition metal content M in the graphite of Example 22 is 0.004wt%. .
[0110] Embodiment 23
[0111] The difference between Example 23 and Example 1 is that in Example 23, based on the total mass of the electrolyte, the mass proportion of the compound of Formula 1-1 is 4.5wt%. .
[0112] Embodiment 24
[0113] The difference between Example 24 and Example 1 is that in Example 24, based on the total mass of the electrolyte, the mass proportion of the compound of Formula 1-1 is 0.25 wt %. .
[0114] Embodiment 25
[0115] The difference between Example 25 and Example 1 is that the total mass of the electrolyte in Example 25 is 4 g, and the discharge capacity of the battery is 2 Ah. The ratio of the total mass of the electrolyte in Example 25 to the discharge capacity of the battery is 2. .
[0116] Embodiment 26
[0117] The difference between Example 26 and Example 1 is that the total mass of the electrolyte in Example 26 is 9g, the discharge capacity of the battery is 2Ah, and the ratio of the total mass of the electrolyte in Example 26 to the discharge capacity of the battery is 4.5. .
[0118] Embodiment 27
[0119] The difference between Example 27 and Example 1 is that in Example 27, 1% of the total mass of the electrolyte is added to the electrolyte, 1,3-propane sultone (PS). .
[0120] Embodiment 28
[0121] The difference between Example 28 and Example 1: The positive electrode active material of Example 28 is LiNi 0.5 Co 0.2 Mn 0.3 O2. Among them, .
[0122] Embodiment 29
[0123] Example 29 prepares a sodium battery. The difference between Example 29 and Example 1 is that the electrolyte of Example 29 uses sodium bis(fluorosulfonyl)imide (NaFSI) and sodium hexafluorophosphate (NaPF6), and the positive electrode active material uses NaFePO4. The mass proportion of NaFSI in the electrolyte is 2wt%, and the mass proportion of NaPF6 in the electrolyte is 10wt%. Among them, .
[0124] Comparative Example 1
[0125] The difference between Comparative Example 1 and Example 1 is that the compound represented by Formula 1 is not added to the electrolyte of Comparative Example 1.
[0126] Comparative Example 2
[0127] The difference between Comparative Example 2 and Example 28: The compound represented by Formula 1 is not added to the electrolyte of Comparative Example 2.
[0128] Comparative Example 3
[0129] The difference between Comparative Example 3 and Example 1 is that in the electrolyte of Comparative Example 3, the mass of the compound of Formula 1-1 accounts for 0.3 wt % based on the total mass of the electrolyte, and the specific surface area of the graphite is 2.5 g / cm 3 .in .
[0130] Comparative Example 4
[0131] The difference between Comparative Example 4 and Example 1 is that in the electrolyte of Comparative Example 4, based on the total mass of the electrolyte, the mass proportion of the compound of Formula 1-1 is 4.0wt%, and the transition metal content M in the graphite is 0.005wt%. .
[0132] Comparative Example 5
[0133] The difference between Comparative Example 5 and Example 1 is as follows: In the electrolyte of Comparative Example 5, based on the total mass of the electrolyte, the mass percentage of the compound of Formula 1-1 is 0.6wt%, and the transition metal content M in the graphite is 0.05wt%, and the specific surface area of the graphite is 2.7g / cm 3 .in .
[0134] The electrolytes, negative electrode active materials and positive electrode active materials of Examples 1-29 and Comparative Examples 1-5 are different, as shown in Table 1.
[0135] Table 1
[0136]
[0137] The batteries prepared in Examples 1-29 and Comparative Examples 1-5 were subjected to high temperature cycle tests and low temperature discharge performance tests. The specific test conditions are as follows:
[0138] High temperature cycle test: Place the battery at 45°C and use 1.5C current for charge and discharge cycles. Record the maximum capacity of the first three times as Q, select the capacity after 2000 cycles as Q2, and calculate the capacity retention rate of the battery after high temperature cycling by the following formula: Capacity retention rate (%) = Q2 / Q×100.
[0139] Low temperature discharge performance test: Charge and discharge the battery once at room temperature with a current of 1C, and record the discharge capacity Q3. Then, fully charge the battery with a current of 1C, and then place the battery in a -20℃ constant temperature box for 4 hours, and discharge it to the lower limit voltage with a current of 0.5C, and record the discharge capacity Q4. Calculate the low temperature discharge capacity retention rate of the battery by the following formula: Low temperature discharge capacity retention rate (%) = Q4 / Q3×100.
[0140] The results of high temperature cycle tests and low temperature discharge performance tests on the batteries prepared in Examples 1-29 and Comparative Examples 1-5 are shown in Table 2.
[0141] Table 2
[0142] High temperature cycle retention rate / % Low temperature discharge retention rate / % Example 1 83.80 63.10 Example 2 82.10 62.80 Example 3 83.10 63.60 Example 4 83.40 63.40 Example 5 82.90 62.30 Example 6 83.80 62.60 Example 7 82.70 63.50 Example 8 83.30 63.20 Example 9 82.50 62.20 Example 10 82.60 62.90 Embodiment 11 84.10 60.20 Example 12 81.20 64.20 Embodiment 13 84.20 60.80 Embodiment 14 80.90 64.70 Embodiment 15 83.30 62.10 Example 16 83.80 63.30 Embodiment 17 70.20 52.70 Embodiment 18 71.60 50.90 Embodiment 19 76.10 54.10 Embodiment 20 70.80 55.60 Embodiment 21 69.70 51.60 Embodiment 22 71.90 50.20 Embodiment 23 70.50 52.20 Embodiment 24 69.80 53.30 Embodiment 25 80.40 63.30 Embodiment 26 84.80 62.50 Embodiment 27 84.90 63.00 Embodiment 28 79.20 68.30 Embodiment 29 78.3 68.8 Comparative Example 1 25.4 40.1 Comparative Example 2 30.1 40.9 Comparative Example 3 61.40 50.70 Comparative Example 4 65.50 50.10 Comparative Example 5 30.8 41.6
[0143] From the data in Table 2, it can be seen that the high temperature cycle retention rate and low temperature discharge retention rate of the battery of Examples 1-29 are much higher than those of the battery of Comparative Examples 1-2 without adding the compound of Formula 1. In particular, although the compound of Formula 1 is added in Comparative Examples 3 and 4, the The calculated value is not between 0.3 and 5.6, and the high temperature cycle retention rate and low temperature discharge retention rate of the battery are also much lower than those of Examples 1-29, indicating that not only the compound shown in Formula 1 is added to the electrolyte of the present application, but also the value calculated by the above formula is between 0.3 and 5.6, and the final battery has excellent low temperature discharge performance and cycle stability.
[0144] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.
[0145] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. A battery, characterized in that: The invention comprises a positive electrode sheet, a negative electrode sheet and an electrolyte, wherein the electrolyte comprises a compound shown in Formula 1, the mass percentage of transition metal in the negative electrode active material of the negative electrode sheet is M, and the specific surface area of the negative electrode active material is Bm 2 / g, the ratio of the total mass of the electrolyte to the discharge capacity of the battery is N g / Ah, the mass percentage of the compound represented by Formula 1 in the electrolyte is C1, and satisfies the following formula: , wherein m is an integer of 0 to 3, n is an integer of 0 to 3, and m and n are not both 0, p is an integer of 1 to 5, R0 is a single bond or a methylene group, R1 is hydrogen, halogen, a hydrocarbon group having 1 to 5 carbon atoms, or a halogenated hydrocarbon group having 1 to 5 carbon atoms, and R2, R3, and R4 are independently , , , , , or ; 0.005%≤M≤0.03%, 0.3%≤C1≤4%, 0.7≤B≤1.9, 2≤N≤4.
5.
2. The battery according to claim 1, characterized in that R1 is hydrogen, halogen, methyl, ethyl, n-propyl, isopropyl, butyl, pentyl, hexyl, halomethyl, haloethyl, halo-n-propyl, haloisopropyl, halobutyl, halopentyl or halohexyl.
3. The battery according to claim 1 or 2, characterized in that: The compound represented by Formula 1 includes at least one of the following compounds: 、 、 、 、 、 、 、 、 、 。 4. The battery according to claim 1 or 2, characterized in that The transition metal includes at least one of iron, copper, nickel and zinc.
5. The battery according to claim 1 or 2, characterized in that The battery is a lithium battery, and the positive electrode active material of the positive electrode plate includes lithium iron phosphate material, nickel-cobalt-manganese ternary material, lithium cobalt oxide material, lithium manganese iron phosphate material, lithium manganese oxide material or nickel-manganese oxide lithium material; and / or The battery is a sodium battery, and the positive electrode active material of the positive electrode plate includes sodium iron phosphate material or a three-dimensional tunnel type Na 0.44 MnO2; and / or The negative electrode active material of the negative electrode plate includes graphite or silicon-based material.
6. The battery according to claim 1 or 2, characterized in that: The electrolytic solution further includes an electrolyte salt including a lithium salt or a sodium salt.
7. The battery according to claim 6, characterized in that Based on the total mass of the electrolyte, the mass proportion of the electrolyte salt is 10% to 20%.
Citation Information
Patent Citations
Electrochemical device and electronic device
CN112151749A
Lithium ion battery
CN114122491A
Lithium secondary battery
CN115036572A
Ultralow-temperature high-energy-density sodium ion battery and preparation method thereof
CN117976978A
Electrolyte additive, electrolyte and battery
CN118040058A
Cited By
Battery
DE212025000075U1