A water-saving polyester-cotton printing and dyeing process

By combining the one-bath one-step method and high-temperature alkaline dyeing liquor with composite disperse dyes, the problem of water and electricity consumption in the traditional polyester-cotton printing and dyeing process has been solved, a highly efficient water-saving and energy-saving dyeing effect has been achieved, and the color fastness and color fastness of polyester-cotton printing and dyeing have been improved. color depth.

CN118308893BActive Publication Date: 2024-10-25SHAOXING GAOWEN PRINTING & DYEING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410494280.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-23
Publication Date
2024-10-25
Estimated Expiration
2044-04-23

AI Technical Summary

Technical Problem

The traditional polyester-cotton printing and dyeing process consumes a lot of water, electricity, and steam, and the sewage standards have increased, so it is necessary to develop water-saving and energy-saving processes.

Method used

Dyeing is carried out using a one-bath and one-step method, using high-temperature alkaline dye liquor and composite disperse dyes, and using eutectic additives to improve the alkali resistance and level dyeing of disperse dyes and shorten the dyeing process.

Benefits of technology

It is possible to improve the color depth and fastness of polyester and cotton printing and dyeing at low water and electricity consumption, reduce sewage discharge, and reduce production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118308893B_ABST
    Figure CN118308893B_ABST
Patent Text Reader

Abstract

The invention discloses a water-saving polyester-cotton printing and dyeing process. A dye liquor component prepared by a composite disperse dye with high temperature alkali resistance and a reactive dye is used to realize one-bath one-step dyeing of polyester-cotton under high temperature alkaline conditions. The composite disperse dye is a eutectic complex of a disperse dye with a specific structure and 2,4,6-triiodobenzene-1,3,5-tricarboxylic acid. The 2,4,6-triiodobenzene-1,3,5-tricarboxylic acid improves the alkali resistance of the disperse dye, and the eutectic has a flaky submicron single crystal structure, so that the eutectic has a higher dyeing rate and leveling property. Therefore, a dyed fabric with good color depth and high fastness is obtained at a lower dyeing temperature and a lower bath ratio.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of polyester-cotton printing and dyeing, and in particular relates to a water-saving polyester-cotton printing and dyeing process. Background Art

[0002] Polyester-cotton knitted fabrics have both the hygroscopic properties of cotton fibers and the good wear resistance, iron-free performance and quick-drying performance of polyester fibers. They occupy an important position in knitted clothing fabrics, but the printing and dyeing of polyester-cotton blends has always been a difficult point. Because polyester has a highly compact crystalline structure and hydrophobicity, and there are no active groups that can be dyed, disperse dyes are often used to dye it. The dyeing process is that the disperse dye enters the amorphous area of ​​the polyester fiber for recrystallization, so high temperature and acidic conditions are often used, which is conducive to the expansion of the fiber and the diffusion of the disperse dye. In addition, there are a large number of hydroxyl groups on the surface of cotton fibers, and active dyes are often used to react with them under alkaline conditions, thereby chemically bonding to the fiber surface, usually under low temperature conditions. Due to the large differences in the dyeing conditions of the two fabrics, including pH and temperature, predecessors have made a lot of efforts to develop efficient and energy-saving polyester-cotton printing and dyeing processes. The traditional two-bath dyeing process includes pre-treatment, dyeing and washing, reduction cleaning, water washing, cotton dyeing, and water washing. After multiple washing steps, a large amount of printing and dyeing wastewater is generated, which increases the burden of sewage treatment. The process also consumes a lot of water, electricity, steam and other resources.

[0003] With the increase in pollution discharge standards, the pressure on enterprises to treat three wastes increases. And with the gradual implementation of carbon neutrality policies, the printing and dyeing industry, which is characterized by heavy pollution and high energy consumption, needs to develop a water-saving and energy-saving polyester-cotton printing and dyeing process. Summary of the invention

[0004] The purpose of the present invention is to provide a water-saving polyester-cotton printing and dyeing process. The technical solution is to dye the polyester-cotton fabric using a one-bath one-step method, shorten the dyeing process, reduce the need for dyeing the polyester-cotton separately under a step method or a separate bath method and perform multiple steps of washing, thereby achieving a water-saving effect.

[0005] In order to realize dyeing by disperse / reactive one-bath one-step method, the present invention adopts the dyeing process of high temperature alkaline dye solution, so it is necessary to improve the alkali resistance of disperse dyes and improve their dyeing rate under alkaline conditions.

[0006] The present invention is achieved through the following technical solutions:

[0007] A water-saving polyester-cotton printing and dyeing process comprises the following steps:

[0008] (3) preparing dye solution components to obtain a dye bath;

[0009] (4) Immerse the fabric in a dye bath, raise the temperature to 80-90°C at a rate of 1-2°C / min, keep the temperature for 15-25min, then raise the temperature to 100-130°C at a rate of 2°C / min, keep the temperature for 20-30min, and then cool the fabric to 60°C. After dyeing, wash and dry the fabric to obtain a printed and dyed fabric.

[0010] The dye solution has the following components: 1-2% (o.wf) of active dye, 1-2% (o.wf) of composite disperse dye, 30-60g / L of sodium sulfate, 0.1mol / L of pH buffer (pH is 9.6-11), and 0.5-1g / L of high-temperature leveling agent.

[0011] The bath ratio is (1:10) ~ (1:20).

[0012] The pH buffer is a sodium carbonate-sodium hydroxide buffer, and the concentrations of sodium carbonate and sodium hydroxide are adjusted according to the required pH value.

[0013] The composite disperse dye is a composite of a disperse dye and a eutectic additive, and the disperse dye has the following general formula:

[0014]

[0015] The following are some of the structures of disperse dyes that have been disclosed in the prior art and satisfy the general formula (I):

[0016] Formula I-1: A is R1 is CH3, R2 is CN, R3 is CH3, R4 is C2H4OC2H4OH; the dye is disperse yellow.

[0017] Formula I-2: A is R1 is CH3, R2 is CN, R3 is CH3, R4 is C2H4OC2H4OH; the dye is disperse orange.

[0018] Formula I-3: A is R1 is CH3, R2 is CN, R3 is CH3, R4 is C2H4OC2H4OH; the dye is disperse violet.

[0019] According to the verified interaction principle between disperse dyes and eutectic additives, disperse dyes with general formula (I) can form multi-dentate interaction forces with 2,4,6-triiodobenzene-1,3,5-tricarboxylic acid to self-assemble into eutectic complexes, and the interaction forces are stable in alkaline aqueous solutions. Therefore, compounding with eutectic additives can effectively improve the high-temperature alkali resistance of disperse dyes conforming to general formula (I).

[0020] The eutectic aid is 2,4,6-triiodobenzene-1,3,5-tricarboxylic acid.

[0021] The preparation method of the composite disperse dye is as follows: weigh the disperse dye and the eutectic auxiliary agent, dissolve them in a solvent, heat them to 60° C., stir them until they are completely dissolved, obtain a recrystallization solution, cool them, seal them, let them stand at room temperature for crystallization, filter and dry the precipitated crystals, and obtain the composite disperse dye.

[0022] In one implementation method of the present invention, the molar ratio of the disperse dye to the eutectic additive is 2.5-2.95:1.

[0023] In one implementation method of the present invention, the solvent is a mixed solution of acetonitrile and chloroform.

[0024] The composite disperse dye provided by the present invention has good high temperature alkali resistance, and a flaky crystal is obtained by adding a eutectic auxiliary and co-crystallizing with the disperse dye molecules. Since the eutectic auxiliary and the group with poor alkali resistance, such as amide, have a multi-tooth interaction force, and the interaction force is stable in an alkaline aqueous solution, the amide is prevented from being hydrolyzed by alkali during the dyeing process, thereby improving the temperature resistance of the disperse dye. On the other hand, since the introduction of the eutectic auxiliary changes the crystal structure of the disperse dye, the eutectic complex single crystal particles present a submicron-level flaky structure, so that the dispersibility of the composite disperse dye in the dye solution is greatly improved, thereby improving the level dyeing and dyeing rate; further, due to the interaction between the disperse dye and the eutectic auxiliary, its light absorption changes, resulting in color difference, but the color depth of the fabric is improved.

[0025] The present invention has the following advantages and beneficial effects:

[0026] The present invention prepares a composite disperse dye, wherein a eutectic auxiliary agent and a specific disperse dye are independently assembled into a eutectic, the alkali resistance of the disperse dye is improved, and the eutectic has a flaky submicron single crystal structure, so that the eutectic has a higher dyeing rate and levelness, so that a dyed fabric with good color depth and high fastness can be obtained at a lower dyeing temperature and a lower bath ratio. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is the X-ray diffraction scanning pattern XRD of the disperse yellow dye and the composite disperse dye of Example 1 and the composite disperse dye prepared in Comparative Example 1.

[0028] Figure 2 This is the X-ray diffraction scanning pattern XRD of the composite disperse dye prepared in Example 2 and Example 3.

[0029] Figure 3 FT-IR images of the disperse yellow, eutectic additive and composite disperse dye of Example 1.

[0030] Figure 4 Schematic diagram of the interaction force between the disperse dye of formula I and the eutectic additive.

[0031] Figure 5 This is a scanning electron microscope (SEM) image of the composite disperse dye of Example 1.

[0032] Figure 6 This is the curve of dyeing rate changing with time and temperature. DETAILED DESCRIPTION

[0033] The present invention is further described in detail below in conjunction with specific examples, but the examples do not limit the present invention in any form. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.

[0034] The raw materials used in the specific implementation manner are described: dyes were purchased from Zhejiang Yutai Dyeing Technology Co., Ltd.; polyester plain woven bleached cloth (250g / m2) and polyester-cotton blended plain woven bleached cloth were purchased from Suzhou Yibi Textile Co., Ltd.; high temperature leveling agent SE was purchased from Linyi Guoli Chemical Co., Ltd.

[0035] Example 1

[0036] Preparation of composite disperse dyes.

[0037] Weigh disperse yellow and 2,4,6-triiodobenzene-1,3,5-tricarboxylic acid and dissolve them in a mixed solution of acetonitrile and chloroform in a volume ratio of 1:3, heat to 60°C and stir until completely dissolved to obtain a recrystallization solution, seal it after cooling, stand it at room temperature for crystallization, filter the precipitated crystals after one week, and vacuum dry it at 80°C to obtain a composite disperse dye. The molar ratio of disperse yellow to eutectic additive is 2.7:1.

[0038] Example 2

[0039] The difference from Example 1 is that disperse orange is used instead of disperse yellow to prepare the composite disperse dye.

[0040] Example 3

[0041] The difference from Example 1 is that disperse violet is used instead of disperse yellow to prepare the composite disperse dye.

[0042] Comparative Example 1

[0043] The difference from Example 1 is that trimesic acid is used instead of 2,4,6-triiodobenzene-1,3,5-tricarboxylic acid as the eutectic auxiliary to prepare the composite disperse dye.

[0044] The XRD patterns of the composite disperse dyes prepared in Examples 1 to 3 and Comparative Example 1 are shown in the attached Figure 1 and 2 ,Depend on Figure 1It can be seen that disperse yellow, i.e., the composite disperse dye obtained by combining disperse yellow with 2,4,6-triiodobenzene-1,3,5-tricarboxylic acid, has an ordered crystalline structure, and the diffraction peak of the crystal has undergone a significant change, indicating that a new crystal is obtained after the composite; in comparative example 1, since there is no N---I interaction force, the obtained crystal is similar to disperse yellow, indicating that N---I is the key to forming a multi-dentate interaction force, thereby driving the self-assembly of the two.

[0045] In order to study the interaction type between disperse dyes and eutectic additives, the disperse yellow, eutectic additives and composite disperse dyes of Example 1 were tested by Fourier infrared spectroscopy (KBr tablet method). The results are shown in the attached Figure 3 The characteristic peaks of disperse yellow dye include: 2251cm -1 It is the characteristic absorption peak of C=N, 1741cm -1 is the stretching vibration of amide C=O, 1618 cm -1 It is the characteristic absorption peak of benzene ring C=C, 1595cm -1 The absorption peak of the ring deformation vibration in the pyridine plane is 1574 cm -1 It is the characteristic absorption peak of N=N; the characteristic peaks of eutectic additives include: 1751em -1 Carboxylic acid C=O stretching vibration absorption peak, 760cm -1 The antisymmetric stretch absorption peak of CI is shown in Figure 2. From the infrared absorption peak of the composite disperse dye, the C=O of the amide and carboxylic acid have shifted to varying degrees, indicating that there is an interaction force between the disperse dye and the eutectic additive. In addition, the antisymmetric stretch absorption peak of CI shifts from 760cm -1 Displacement to 756cm -1 , and the vibration peak of pyridine from 1595cm -1 Displacement to 1603cm -1 , indicating that after the interaction between the two, the CI bond is weakened and the interaction force of the N---I halogen bond is multiplied.

[0046] The high temperature alkali resistance test of the dyes of Examples 1 to 3 and Comparative Example 1 and Disperse Yellow was performed, and the test method was as follows: the polyester was dyed with the above dyes in an alkaline dyeing solution, and the K / S and color difference (ΔE) of the dyed fabric samples were measured. The dyeing solution formula was: 2% owf of the dye, 2 g / L of the high temperature leveling agent SE, and the pH was adjusted to 4.5, 7, 10, 12 with acetic acid or sodium hydroxide, and the bath ratio was 30:1; dyeing process: the fabric was added to the dye bath, heated to 130°C at 2°C / min, kept warm for 30 minutes, and then cooled to 60°C, and the dyeing was completed. The fabric samples dyed under acidic conditions were subjected to cold water washing (10 min) → reduction cleaning (70°C, 10 min) → water washing (60°C, 10 min) → drying, and the fabric samples dyed under alkaline conditions were subjected to cold water washing (10 min) → soap washing (98°C, 10 min) → water washing (60°C, 10 min) → drying; reduction cleaning formula: NaOH 2g / L, insurance powder 2g / L, bath ratio 1:50; soap washing formula: 0.6g / L soaping agent HK-8235, bath ratio 1:50; the results are listed in Table 1.

[0047] Table 1

[0048]

[0049] It can be seen from the above data that the composite disperse dye prepared in the embodiment of the present invention has little color difference when dyeing under acidic and alkaline conditions, while the color difference between comparative example 1 and disperse yellow is large, indicating that the high temperature alkali resistance of the disperse dye after compounding with the eutectic auxiliary is greatly improved; in addition, there is a certain color difference between Example 1 and disperse yellow when dyeing at pH = 4.5, indicating that after the composite eutectic, the absorption wavelength of the disperse dye changes, causing the color light to change, thus producing color difference, but the K / S of Example 1 is increased compared with disperse yellow, indicating that the dyeing rate is improved, thanks to the improved dispersibility of the composite disperse dye compared with the disperse dye.

[0050] In order to investigate the difference in dyeing rate between composite disperse dye and disperse dye, a dye solution was prepared: Example 1 composite disperse dye or disperse yellow 2% o.wf, high temperature leveling agent SE 2g / L, pH adjusted to 10 with sodium hydroxide, bath ratio of 30:1; dyeing process: add the fabric to the dye bath, heat it to 70, 90, 110, 130°C at 2°C / min, and keep it warm for 15min, 30min, 45min, 60min, take out the corresponding dye cup, measure the absorbance of the dyeing residual liquid, and calculate the dyeing rate (F%) by the following formula:

[0051] Where A0 and A1 are the absorbance of the dye solution before and after staining, respectively, and n0 and n1 are the dilution multiples of the dye solution before and after staining, respectively.

[0052] Example 1 The variation curve of the dyeing rate of the composite disperse dye or disperse yellow over time is shown in Figure 6 As can be seen from the figure, under the same temperature and time, the dyeing rate of the composite disperse dye is greater than that of disperse yellow, indicating that the dyeing rate of the composite disperse dye is higher. This is because the introduction of the eutectic additive changes the crystal structure of the disperse dye, making the eutectic composite single crystal particles present a submicron-level flake structure (see Appendix Figure 5 ), which greatly improves the dispersibility of the composite disperse dye in the dye solution, thereby increasing the dye uptake rate.

[0053] Example 4

[0054] The difference from Example 1 is that the molar ratio of the disperse yellow and the eutectic additive is 2.5:1.

[0055] Example 5

[0056] The difference from Example 1 is that the molar ratio of the disperse yellow to the eutectic additive is 2.95:1.

[0057] Example 6

[0058] A water-saving polyester-cotton printing and dyeing process comprises the following steps:

[0059] (1) Prepare dyeing liquid components to obtain a dye bath. First, prepare a sodium carbonate-sodium hydroxide buffer solution with a pH of 10, and use it as a solvent to prepare a dyeing liquid with the following components: 1.5% (owf) of active yellow brown RE-ZY, 1.5% (owf) of the composite disperse dye of Example 1, 45 gIL of sodium sulfate, and 0.7 gIL of high-temperature leveling agent SE. Sodium carbonate or sodium hydroxide is added in an appropriate amount to maintain the pH at 10 to obtain a dyeing bath; the bath ratio is 1:15.

[0060] (2) The fabric is immersed in a dye bath, and the temperature is raised to 80°C at a rate of 1°C / min, and then kept at that temperature for 20 min. The temperature is then raised to 110°C at a rate of 2°C / min, and then kept at that temperature for 20 min. The fabric is then cooled to 60°C, and the dyeing is completed. The fabric is then washed with water at 60°C for 20 min and dried to obtain a printed and dyed fabric.

[0061] Example 7

[0062] The difference from Example 1 is that the composite disperse dye of Example 2 is used to replace the composite disperse dye of Example 1, and the reactive yellow brown RE-ZY is replaced by reactive orange K-GN.

[0063] Example 8

[0064] The difference from Example 1 is that the composite disperse dye of Example 3 is used to replace the composite disperse dye of Example 1, and the reactive violet K-3R is used to replace the reactive yellow brown RE-ZY.

[0065] Example 9

[0066] A water-saving polyester-cotton printing and dyeing process comprises the following steps:

[0067] (1) Prepare dyeing liquid components to obtain a dye bath. First, prepare a sodium carbonate-sodium hydroxide buffer solution with a pH of 9.6, and use it as a solvent to prepare a dyeing liquid with the following components: 1% (owf) of active yellow brown RE-ZY, 1% (owf) of the composite disperse dye of Example 4, 30 g / L of sodium sulfate, and 0.5 g / L of high-temperature leveling agent SE. Sodium carbonate or sodium hydroxide is added in an appropriate amount to maintain the pH at 9.6 to obtain a dyeing bath; the bath ratio is 1:20.

[0068] (2) The fabric is immersed in a dye bath, and the temperature is raised to 90°C at a rate of 2°C / min, and then kept at this temperature for 25 min. The temperature is then raised to 120°C at a rate of 2°C / min, and then kept at this temperature for 30 min. The fabric is then cooled to 60°C, and the dyeing is completed. The fabric is then washed with water at 60°C for 20 min and dried to obtain a printed and dyed fabric.

[0069] Example 10

[0070] A water-saving polyester-cotton printing and dyeing process comprises the following steps:

[0071] (1) Prepare dyeing liquid components to obtain a dyeing bath. First, prepare a sodium carbonate-sodium hydroxide buffer solution with a pH of 11, and use it as a solvent to prepare a dyeing liquid with the following components: 2% (owf) of active yellow brown RE-ZY, 2% (owf) of the composite disperse dye of Example 5, 60 g / L of sodium sulfate, and 1 g / L of high-temperature leveling agent SE. Sodium carbonate or sodium hydroxide is added in an appropriate amount to maintain the pH at 11 to obtain a dyeing bath; the bath ratio is 1:10.

[0072] (2) The fabric is immersed in a dye bath, and the temperature is raised to 90°C at a rate of 2°C / min, and then kept at this temperature for 15 min. The temperature is then raised to 100°C at a rate of 2°C / min, and then kept at this temperature for 30 min. The fabric is then cooled to 60°C, and the dyeing is completed. The fabric is then washed with water at 60°C for 20 min and dried to obtain a printed and dyed fabric.

[0073] Embodiment 11

[0074] The difference from Example 1 is that in step (2), the temperature is raised to 80°C at 1°C / min and then kept warm for 20 minutes, then raised to 130°C at 2°C / min and then kept warm for 20 minutes, and then cooled to 60°C. After dyeing is completed, the fabric is washed with water at 60°C for 20 minutes and dried to obtain a printed and dyed fabric.

[0075] Comparative Example 2

[0076] The difference from Example 1 is that disperse yellow is used to replace the composite disperse dye in Example 1.

[0077] Comparative Example 3

[0078] The difference from Example 1 is that in step (2), the temperature is raised to 80°C at 1°C / min and then kept warm for 20 minutes, then raised to 90°C at 2°C / min and kept warm for 30 minutes, and then cooled to 60°C. After dyeing is completed, the fabric is washed with water at 60°C for 20 minutes and dried to obtain a printed and dyed fabric.

[0079] The dyed fabrics prepared in Examples 6 to 10 and Comparative Examples 2 to 4 were subjected to the following tests, and the results are listed in Table 2:

[0080] (1) The apparent color depth K / S value was measured using a Datacolor 650 colorimeter, using a D65 light source and a 10° viewing angle to measure the K / S value at the wavelength of maximum absorption of the dyed fabric. Ten points were randomly selected for each sample and the average value was calculated. The average value is taken as the K / S value of the fabric, and the standard deviation Sr is used to evaluate the levelness of dyeing. The calculation formula of the standard deviation Sr is as follows, n = 10:

[0081]

[0082] (2) Fastness test

[0083] Test the color fastness of dyed fabrics to washing with soap according to GB / T 3921-2008 "Textiles - Tests for color fastness - Color fastness to washing with soap";

[0084] Test the color fastness to rubbing of dyed fabrics according to GB / T 3920-2008 "Textiles - Tests for color fastness - Color fastness to rubbing";

[0085] Test the sublimation fastness of dyes according to GB / T 5718-1997 "Textiles - Tests for colour fastness - Colour fastness to hot pressing";

[0086] The color fastness of dyes to sunlight is tested in accordance with GB / T 8427-2008 Textiles - Tests for color fastness to artificial light: Xenon arc fading lamp.

[0087] Table 2

[0088]

[0089] From the data in the table, it can be seen that Example 6 has a lower Sr than Comparative Example 2, indicating that the composite disperse dye has a better dye uptake rate than the disperse dye, thanks to its better dispersibility, and is easier to diffuse into the fiber. In addition, the higher the temperature, the lower the Sr, indicating that high temperature is conducive to the diffusion of disperse dyes into the fiber. Compared with Example 6, the K / S of Example 11 decreases, indicating that K / S increases first and then decreases with increasing temperature, indicating that too high a temperature will reduce the dye uptake rate of the composite disperse dye. The possible reason is that too high a temperature causes the interaction force to dissociate, so that the disperse dye is easily hydrolyzed, resulting in dyeing failure.

[0090] The above contents are further detailed descriptions of the present invention in combination with specific preferred technical solutions, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For professionals and technicians in the technical field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the concept of the present invention, which should be regarded as belonging to the protection scope of the present invention.

Claims

1. A water-saving polyester-cotton printing and dyeing process, characterized in that: The following steps are involved: (1) preparing dye solution components to obtain a dye bath; (2) immersing the fabric in a dye bath, heating the fabric to 80-90°C at a rate of 1-2°C / min, and then keeping the temperature for 15-25min, then heating the fabric to 100-130°C at a rate of 2°C / min, and then keeping the temperature for 20-30min, and then cooling the fabric to 60°C. After dyeing, the fabric is washed and dried to obtain a printed and dyed fabric. The dye solution components include: 1-2% owf reactive dye, 1-2% owf composite disperse dye, 30-60 g / L sodium sulfate, pH buffer, and 0.5-1 g / L high temperature leveling agent; The composite disperse dye is a composite of a disperse dye and 2,4,6-triiodobenzene-1,3,5-tricarboxylic acid, and the disperse dye has the following general formula: In the general formula (I): when A is R1 is CH3, R2 is CN, R3 is CH3, R4 is C2H4OC2H4OH, and the disperse dye is disperse yellow; when A is R1 is CH3, R2 is CN, R3 is CH3, R4 is C2H4OC2H4OH, and the disperse dye is disperse orange; when A is R1 is CH3, R2 is CN, R3 is CH3, R4 is C2H4OC2H4OH, and the disperse dye is disperse violet.

2. A water-saving polyester-cotton printing and dyeing process according to claim 1, characterized in that: The bath ratio of the dye bath is (1:10) to (1:20).

3. A water-saving polyester-cotton printing and dyeing process according to claim 1, characterized in that: The pH buffer is sodium carbonate-sodium hydroxide buffer.

4. A water-saving polyester-cotton printing and dyeing process according to claim 1, characterized in that: The pH of the dye bath is 9.6-11.

5. A water-saving polyester-cotton printing and dyeing process according to claim 1, characterized in that: The preparation method of the composite disperse dye is as follows: weigh the disperse dye and 2,4,6-triiodobenzene-1,3,5-tricarboxylic acid, dissolve them in a solvent, heat to 60°C and stir until completely dissolved to obtain a recrystallization solution, seal it after cooling, let it stand at room temperature for crystallization, and obtain the composite disperse dye after filtering and drying the precipitated crystals.

6. A water-saving polyester-cotton printing and dyeing process according to claim 1, characterized in that: The molar ratio of the disperse dye to 2,4,6-triiodobenzene-1,3,5-tricarboxylic acid is 2.5-2.95:

1.

7. A water-saving polyester-cotton printing and dyeing process according to claim 5, characterized in that: The solvent is a mixed solution of acetonitrile and chloroform.