A non-oriented electrical steel with excellent comprehensive performance and its manufacturing method
By controlling the chemical composition and process parameters of non-oriented electrical steel and optimizing the texture strength ratio, non-oriented electrical steel with low magnetic anisotropy, high magnetic induction intensity and low iron loss was prepared. This solved the problems of high-frequency iron loss and insufficient magnetic induction intensity in the existing electric vehicle drive motor, and achieved a combination of high strength and excellent electromagnetic performance.
Patent Information
- Application Number
- CN202310033304.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-10
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-01-10
AI Technical Summary
Existing non-oriented silicon steel has high iron loss and insufficient magnetic induction intensity at high frequencies, making it difficult to simultaneously meet the requirements of high strength and excellent electromagnetic performance for electric vehicle drive motors.
By controlling the content of chemical components such as Si, Al, and Mn, and combining specific hot rolling, cold rolling, and annealing processes, the texture strength ratio is optimized to prepare non-oriented electrical steel with low magnetic anisotropy, high magnetic induction intensity, and low iron loss.
It achieves comprehensive performance of high yield strength, low, medium and high frequency iron loss and high magnetic induction intensity, and is suitable for core materials of electric vehicle drive motors, high-speed motors and drones.
Smart Images

Figure BDA0004047742520000061 
Figure BDA0004047742520000071 
Figure BDA0004047742520000081
Abstract
Description
Technical Field
[0001] This invention relates to a steel plate and a method for manufacturing the same, and more particularly to a non-oriented electrical steel plate and a method for manufacturing the same. Background Technology
[0002] With the rapid development of electric vehicles, higher requirements have been placed on the non-oriented silicon steel, the magnetic core material of the drive motor, which is its core component. The non-oriented silicon steel must have sufficient strength to resist centrifugal force at high speeds to ensure that the rotor does not deform or break. At the same time, it must have excellent electromagnetic properties, especially the iron loss in the high-frequency range of 400Hz-2000Hz should be as low as possible, and the magnetic induction intensity should be high to meet the high torque requirements when the motor starts or accelerates.
[0003] Chinese patent document CN101490294A, published on July 22, 2009, entitled "High-strength Non-directional Electromagnetic Steel Sheet," discloses a non-oriented electrical steel sheet with a strength exceeding 650 MPa. Although its strength is high, the iron loss P of this electromagnetic steel sheet is... 10 / 400 It has a high electromagnetic performance of up to 70W / kg.
[0004] Chinese patent document CN112930412A, published on June 8, 2021, entitled "Non-oriented Electromagnetic Steel Sheet and Manufacturing Method Thereof, and Electric Core Thereof, and Manufacturing Method Thereof," discloses a non-oriented electrical steel sheet with excellent strength and iron loss. The main solution involves annealing a cold-rolled sheet with a Si content of 2.8-6.5% at 700-820℃, strengthening it through a partially recrystallized structure with a recrystallization area ratio of 40-95%, resulting in a yield strength exceeding 500 MPa. However, this method cannot simultaneously meet the requirements of high frequency, low iron loss, and high magnetic flux density for drive motors.
[0005] Based on this, it is desirable to obtain a non-oriented electrical steel with excellent comprehensive performance and its manufacturing method, which has both high strength and excellent electromagnetic properties. Summary of the Invention
[0006] One of the objectives of this invention is to provide a non-oriented electrical steel with excellent comprehensive performance. This non-oriented electrical steel has low magnetic anisotropy, high magnetic induction intensity, low iron loss in medium and high frequencies, and high yield strength. It can be widely used in the core materials of electric vehicle drive motors, high-speed motors, drones, etc.
[0007] To achieve the above objectives, this invention proposes a non-oriented electrical steel with excellent overall performance, which contains Fe and unavoidable impurities, and also contains the following chemical elements in the following mass percentages:
[0008] C ≤ 0.005%, Si: 3.1-4.5%, Al: 0.1-2.0%, Mn: 0.1-2.5%; and 3.75% ≤ Si + Al ≤ 5.0%;
[0009] The iron loss P of the non-oriented electrical steel 10 / 600 ≤35W / kg, magnetic induction intensity B 50 ≥1.64T, and longitudinal magnetic induction intensity B 50L With transverse magnetic induction intensity B 50C The difference ΔB does not exceed 1000 Gauss.
[0010] Accordingly, the present invention also provides a non-oriented electrical steel with excellent comprehensive performance, wherein the mass percentage content of each chemical element is as follows:
[0011] C ≤ 0.005%, Si: 3.1-4.5%, Al: 0.1-2.0%, Mn: 0.1-2.5%, balance being Fe and unavoidable impurities; and satisfying 3.75% ≤ Si + Al ≤ 5.0%;
[0012] The iron loss P of the non-oriented electrical steel 10 / 600 ≤30W / kg, magnetic induction intensity B 50 ≥1.64T, and longitudinal magnetic induction intensity B 50L With transverse magnetic induction intensity B 50C The difference ΔB does not exceed 1000 Gauss.
[0013] The non-oriented electrical steel described in this invention possesses excellent comprehensive properties, exhibiting both low iron loss and high magnetic induction. Its iron loss P under conditions of magnetic flux density 1.0T and frequency 600Hz is [insert value here]. 10 / 600 ≤35W / kg, magnetic induction intensity B 50 ≥1.64T, and longitudinal magnetic induction intensity B 50L With transverse magnetic induction intensity B 50C The difference ΔB does not exceed 1000 Gauss.
[0014] The design principles of each chemical element in the non-oriented electrical steel described in this invention are as follows:
[0015] C: In the non-oriented electrical steel described in this invention, element C is an impurity element, which is harmful to the magnetism of non-oriented silicon steel. Therefore, the content of element C must be strictly controlled to C≤0.005%.
[0016] Si: In the non-oriented electrical steel described in this invention, Si can increase the resistivity of the non-oriented electrical steel sheet, reduce iron loss, and, as a solid solution strengthening element, also improve the strength of the steel sheet. For this invention, when the Si content exceeds 4.5%, ordered phases Fe3Si or FeSi appear, causing a sharp deterioration in the material's room temperature plasticity, making large-scale industrial cold rolling impossible, and also deteriorating the magnetic induction intensity. Conversely, when the Si content is less than 3.1%, the high yield strength and high-frequency, low-iron-loss effects cannot be achieved. Therefore, the mass percentage of Si is controlled between 3.1% and 4.5%.
[0017] Al: In the non-oriented electrical steel described in this invention, Al is also an effective element for increasing resistivity and reducing iron loss. However, excessive addition is detrimental to the magnetic induction intensity of the material and will cause difficulties in steelmaking and casting, and the cold working performance of the steel plate will also deteriorate. Therefore, the addition amount is controlled to not exceed 2.0%. At the same time, considering the role of this element in improving iron loss, the addition amount is controlled to be above 0.1%.
[0018] In addition, the total content of the two alloying elements Si and Al is specifically controlled to be 3.75%-5.0% in this invention. This is because both of these elements are solid solution strengthening elements and increase the resistivity of the material. If the total content is less than 3.75%, the performance of the non-oriented silicon steel sheet of this invention cannot be achieved. If it exceeds 5.0%, it will cause difficulties in cold rolling production and reduce the magnetic induction.
[0019] Mn: In the non-oriented electrical steel described in this invention, Mn can increase resistivity and react with impurity element S to form MnS, which improves electromagnetic properties. Therefore, the addition of more than 0.1% Mn is necessary, while more than 2.0% will reduce the plasticity of the steel and lead to cold rolling strip breakage.
[0020] Furthermore, in the non-oriented electrical steel of the present invention, the C element content is preferably C≤0.003%.
[0021] Furthermore, in the non-oriented electrical steel described in this invention, the unavoidable impurities are P≤0.04%, S≤0.003%, N≤0.005%, O≤0.003%, and Nb+V+Ti≤0.005%.
[0022] Furthermore, in the non-oriented electrical steel of the present invention, the unavoidable impurities preferably contain P ≤ 0.02% and N ≤ 0.0035%.
[0023] In the non-oriented electrical steel described in this invention, P, S, N, O, Nb, V, and Ti are all impurity elements in the non-oriented electrical steel sheet. Where technical conditions permit, to obtain steel with better performance and superior quality, the content of impurity elements in the steel should be reduced as much as possible. Wherein:
[0024] P: P is a grain boundary segregating element. For the composition system of this invention with a Si content of more than 3.1%, if the phosphorus content exceeds 0.04%, it will exacerbate the brittleness of electrical steel sheets and make them difficult to roll.
[0025] S: In this invention, S is a magnetically detrimental element that combines with Mn to form fine MnS, thereby hindering grain growth during annealing and degrading the magnetic properties of the steel plate. Therefore, the mass percentage of S is controlled to be S≤0.003%.
[0026] N: In this invention, N is a magnetically detrimental element that forms fine nitrides with Al, Ti, Nb, and V, hindering grain growth. Therefore, in the non-oriented electrical steel described in this invention, the mass percentage of N is controlled to be N ≤ 0.005%.
[0027] O: In this invention, O is a harmful element. For a composition system of 3.75% ≤ Si + Al ≤ 5.0%, the cold working performance of the material is very sensitive to the segregation of oxygen at grain boundaries. Furthermore, the silicon, aluminum, and manganese oxides formed will also degrade the magnetic properties of the material. Therefore, in this invention, the mass percentage of O is controlled to be O ≤ 0.0030%.
[0028] Nb, V, and Ti combine with residual C and N in the steel to form fine carbides and nitrides, which seriously affect grain growth during the annealing process and are detrimental to the magnetic properties of the material. Therefore, this invention controls the total mass percentage of Nb, V, and Ti to be below 0.005%.
[0029] Furthermore, the non-oriented electrical steel described in this invention also contains B: 0.0003wt%-0.01wt%.
[0030] In the above technical solution of the present invention, in order to further optimize the performance of the non-oriented electrical steel of the present invention, an appropriate amount of element B may be added to the steel.
[0031] B: In the non-oriented electrical steel described in this invention, B is a grain boundary strengthening element, which can enhance the grain boundary bonding ability of the high-silicon content system, thereby improving the cold rolling performance of the material. However, when B is added in excess, it will refine the grain structure, which is detrimental to magnetic properties. Therefore, the mass percentage should not exceed 0.01%; while when the B content in the steel is less than 0.0003%, it will not play a grain boundary strengthening role.
[0032] Furthermore, the non-oriented electrical steel described in this invention also contains at least one of Sn and Sb, and the total mass percentage content of Sn is controlled at 0.005-0.3%.
[0033] Sn and Sb are both grain boundary segregation elements. On the one hand, they can hinder the diffusion of trace oxygen along the grain boundaries during the normalizing annealing process of hot-rolled plates, preventing oxidation and plastic deterioration within the steel plate. On the other hand, they can improve the magnetically favorable textures such as {100} surface texture and Goss texture during the annealing process of finished plates.
[0034] Furthermore, the non-oriented electrical steel described in this invention also contains at least one of Co, Ni, Cu, and Cr, and the total mass percentage of these elements is controlled between 0.02% and 3.0%.
[0035] Co, Ni, Cu, and Cr elements can play a role in solid solution strengthening. These elements can further improve the electromagnetic properties and strength of the material without impairing the cold working performance of the steel plate.
[0036] Furthermore, the average grain size of the non-oriented electrical steel described in this invention is 10-110 μm.
[0037] If the grain size of the finished plate is less than 10 μm, the iron loss P of this invention will not be achieved. 10 / 600 Performance requirements: If the grain size of the finished board exceeds 110μm, the yield strength will decrease, the production efficiency will be lower, the requirements for production equipment will be higher, and the cost will increase.
[0038] Furthermore, the thickness of the non-oriented electrical steel described in this invention is 0.1–0.3 mm.
[0039] Furthermore, the yield strength of the non-oriented electrical steel described in this invention is ≥430MPa.
[0040] Accordingly, another object of the present invention is to provide a manufacturing method for the above-mentioned non-oriented electrical steel, which is simple and feasible, and can obtain non-oriented electrical steel sheets with excellent comprehensive performance.
[0041] To achieve the above-mentioned objectives, this invention proposes a method for manufacturing non-oriented electrical steel, comprising the following steps:
[0042] (1) Obtain the casting billet;
[0043] (2) Hot rolling: The final rolling reduction rate of the roughing rolling is controlled to be 35%-55%. The intermediate slab obtained from the roughing rolling is kept warm for 50s-80s before entering the finishing mill. The temperature of the intermediate slab when entering the finishing mill is 960-1100℃, and the temperature difference ΔT between the head and tail of the intermediate slab is controlled to be ≤40℃.
[0044] (3) Normalizing annealing;
[0045] (4) Cold rolling;
[0046] (5) Final annealing;
[0047] (6) Insulating coating.
[0048] Furthermore, in step (2) of the manufacturing method described in this invention, the intermediate slab before entering the finishing mill has a {001} surface texture intensity at a distance of one-quarter of the slab surface thickness from the slab surface layer, which is similar to {111}. <112> Texture strength ratio I ≥ 0.55.
[0049] In this invention, the inventors optimized the chemical composition design of the steel and defined a reasonable manufacturing process. After the continuous casting billet is made according to the designed chemical composition, it is then subjected to hot rolling, normalizing annealing, cold rolling (which can be a single cold rolling or a double cold rolling including intermediate annealing), final annealing, and coating with an insulating coating to obtain non-oriented electrical steel with excellent comprehensive performance.
[0050] In the hot roughing rolling of the continuously cast slab, the final rolling reduction rate is controlled at 35-55% to obtain an intermediate slab. Before entering the hot finishing mill, the intermediate slab needs to stay on the roller table with a heat preservation cover for 50-80 seconds, or it can be re-coiled and uncoiled using the hot coil box equipment after the roughing mill to achieve a heat preservation stay of 50-80 seconds. The temperature of the intermediate slab entering the first stand of the finishing mill is controlled at 960-1100℃, and the temperature difference ΔT between the head and tail of the intermediate slab strip is ≤40℃.
[0051] The above process parameters are limited primarily to ensure sufficient recrystallization of the intermediate slab, while reducing the solid solution precipitation of second phases such as AlN, MnS, and TiC, and increasing the magnetically favorable texture components. In particular, the texture intensity of the {001} plane at a position one-quarter of the way from the surface of the intermediate slab is controlled to ensure it is compatible with the {111} plane. <112> A texture intensity ratio I ≥ 0.55 is achieved to improve the texture effect of the finished annealed plate, reduce magnetic anisotropy, and decrease the longitudinal magnetic induction intensity B. 50L With transverse magnetic induction intensity B 50C The difference ΔB does not exceed 1000 Gauss, and the magnetic induction intensity B 50 The technical effect exceeds 1.64T.
[0052] In addition, controlling the temperature difference between the head and tail of the intermediate slab strip within 40℃ can ensure the consistency of the overall performance of the strip steel product and enable constant speed and temperature rolling in the subsequent finishing mill. This significantly reduces the risk of motor overcurrent when the finishing mill produces thin-gauge high-grade non-oriented silicon steel, ensuring the stability of continuous production.
[0053] Furthermore, in step (2) of the manufacturing method described in this invention, the thickness of the intermediate slab obtained is 25-40 mm.
[0054] Furthermore, in step (5) of the manufacturing method described in this invention, the annealing temperature is 750-1000℃ and the annealing time is 11s-125s.
[0055] The final annealing process aims to achieve a target grain size of 10-110 μm for the finished non-oriented electrical steel sheet. If the annealing temperature is too low or the annealing time is too short, resulting in a grain size of less than 10 μm in the finished sheet, the iron loss P of this invention will not be achieved. 10 / 600 Performance requirements are met, but if the annealing temperature is too high or the annealing time is too long, the grain size of the finished steel plate will exceed 110μm, which will reduce the yield strength, reduce production efficiency, and increase costs.
[0056] The non-oriented electrical steel and its manufacturing method described in this invention have the following advantages and beneficial effects:
[0057] The non-oriented electrical steel described in this invention has low magnetic anisotropy, high magnetic induction intensity, low iron loss in medium and high frequencies, and high yield strength. It can be widely used in the core materials of electric vehicle drive motors, high-speed motors, drones, etc.
[0058] The non-oriented electrical steel described in this invention has a yield strength ≥430MPa and an iron loss P 10 / 600 ≤35W / kg, magnetic induction intensity B 50 ≥1.64T, and longitudinal magnetic induction intensity B 50L With transverse magnetic induction intensity B 50C The difference ΔB does not exceed 1000 Gauss. Detailed Implementation
[0059] The non-oriented electrical steel and its manufacturing method described in this invention will be further explained and described below with reference to specific embodiments. However, such explanation and description do not constitute an undue limitation on the technical solution of this invention.
[0060] Examples 1-9 and Comparative Examples 1-5
[0061] Table 1 lists the mass percentage of each chemical element in the non-oriented electrical steels of Examples 1-9 and the comparative steel plates of Comparative Examples 1-5.
[0062] Table 1. (wt%, balance Fe and unavoidable impurities other than P, S, O, N, Nb, V, and Ti)
[0063]
[0064]
[0065]
[0066] The non-oriented electrical steels of Examples 1-9 were prepared using the following steps:
[0067] (1) Prepare the billet according to the chemical composition ratio shown in Table 1.
[0068] (2) Hot rolling: The final rolling reduction rate of the roughing rolling is controlled at 35%-55% to obtain an intermediate slab with a thickness of 25-40mm; before entering the finishing mill, the intermediate slab is held at a high temperature for 50s-80s. Before entering the finishing mill, the texture strength of the {001} surface at a distance of one-quarter of the slab surface thickness is similar to that of {111}. <112> The texture strength ratio I ≥ 0.55; the temperature of the intermediate slab entering the finishing mill is 960-1100℃, and the temperature difference ΔT between the head and tail of the intermediate slab is controlled to be ≤ 40℃.
[0069] (3) Normalizing annealing: The normalizing temperature of Examples 1-4 was 1050℃, the normalizing temperature of Examples 5-7 was 920℃, the normalizing temperature of Examples 8-9 was 850℃, and the normalizing temperature of the comparative example was 920℃. The normalizing holding time was 90s.
[0070] (4) Cold rolling: The target thickness is achieved by one cold rolling process, or by one cold rolling process + intermediate annealing + two cold rolling processes to produce a sheet with a thickness of 0.1 to 0.3 mm.
[0071] (5) Final annealing: The annealing temperature is 750-1000℃ and the holding time is 11s-125s.
[0072] (6) Insulating coating.
[0073] It should be noted that although Comparative Examples 1-5 were also prepared using the above steps and procedures, their specific process parameters did not meet the control requirements of this invention.
[0074] Table 2 lists the specific process parameters and final product thickness of the non-oriented electrical steels of Examples 1-9 and the comparative steel plates of Comparative Examples 1-5 in the above manufacturing process.
[0075] Table 2.
[0076]
[0077]
[0078] Note: In Table 2, the texture strength of the {001} surface at one-quarter of the distance from the surface layer of the intermediate slab is related to that of the {111} surface. <112> The texture intensity ratio I was obtained by XRD diffraction.
[0079] Samples were taken from the final non-oriented electrical steel products of Examples 1-9 and the comparative steel plates of Comparative Examples 1-5. The iron loss P at a magnetic flux density of 1.0T and a frequency of 600Hz was tested on these non-oriented electrical steel plates. 10 / 600 The magnetic induction intensity B when magnetized in a magnetic field of 5000 A / m 50 Longitudinal magnetic induction intensity B 50L and transverse magnetic induction intensity B 50L The yield strength and other test results are listed in Table 3 below. The relevant performance testing methods are described below:
[0080] The grain size measurement of the finished plate is based on the area method of the standard "GB / T6394-2017 Method for Determination of Average Grain Size of Metals".
[0081] Iron loss P 10 / 600 The test is based on the square circle method of the standard "GB / T10129-2019 Measurement Method of Medium Frequency Magnetic Properties of Electrical Steel Strips (Sheets)".
[0082] Magnetic induction intensity is measured using the square ring method based on the standard GB / T3655-2008 "Method for Measuring the Magnetic Properties of Electrical Steel Sheets (Strips) Using the Epstein Square Ring Method", specifically testing B. 50 Longitudinal B 50L Horizontal B 50C .
[0083] The yield strength performance index is based on the standard GB / T 228.1-2010 Metallic materials, tensile testing - Part 1: Test method at room temperature.
[0084] Table 3 lists the test results of the non-oriented electrical steels of Examples 1-9 and the comparative steel plates of Comparative Examples 1-5.
[0085] Table 3.
[0086]
[0087]
[0088] As can be seen from Tables 1, 2 and 3 above, the Si content in Comparative Example 1 and Comparative Example 2 is outside the range of the present invention, which causes the grain size of the finished product of Comparative Example 1 to exceed the upper limit and its yield strength to be low. At the same time, it also causes the iron loss of Comparative Example 2 to be high.
[0089] The Si content in Comparative Example 3 does not meet the requirements of this invention, and the Si+Al content is less than 3.75%, resulting in a low yield strength.
[0090] Although Comparative Examples 4 and 5 meet the requirements of the present invention in terms of composition, their hot rolling process parameters and texture ratio I are not within the specified range. Therefore, they did not obtain the desired magnetic induction intensity and magnetic anisotropy of the finished product as desired by the present invention.
[0091] The embodiments 1-2 of the present invention employ a single cold rolling process. The chemical composition control, the reduction rate of the last pass of rough rolling, the holding time, the temperature of the intermediate slab entering the finishing mill, the temperature difference between the head and tail of the intermediate slab, and the grain size of the finished product are all within the design range of the present invention. Therefore, non-oriented silicon steel with high yield strength and excellent magnetic properties can be obtained.
[0092] Embodiment 2 of the present invention further adds Sn and Sb, which results in better strength and iron loss than Embodiment 1.
[0093] Embodiment 3 of the present invention further adds B, which has better strength and iron loss than Embodiment 1.
[0094] In embodiments 4-9 of the present invention, the performance of the finished steel plate is further improved by adding microalloying elements such as Sn, Sb, Cu, Cr, Ni, and Co, and by using a secondary cold rolling process.
[0095] It should be noted that the scope of protection of the prior art in this invention is not limited to the embodiments given in this application. All prior art that does not contradict the solution of this invention, including but not limited to prior patent documents, prior publications, prior public uses, etc., can be included in the scope of protection of this invention.
[0096] Furthermore, the combination of the technical features in this case is not limited to the combination methods described in the claims of this case or the combination methods described in the specific embodiments. All technical features described in this case can be freely combined or combined in any way, unless they contradict each other.
[0097] It should also be noted that the embodiments listed above are merely specific embodiments of the present invention. Obviously, the present invention is not limited to the above embodiments, and similar changes or modifications made thereto are those that can be directly derived or easily conceived by those skilled in the art from the content disclosed in the present invention, and should all fall within the protection scope of the present invention.
Claims
1. A non-oriented electrical steel with excellent comprehensive performance, containing Fe and unavoidable impurities, characterized in that, It also contains the following chemical elements in the following mass percentages: C ≤ 0.005%, Si: 3.1-4.5%, Al: 0.1-2.0%, Mn: 0.1-2.5%; and 3.75% ≤ Si + Al ≤ 5.0%; The iron loss P of the non-oriented electrical steel 10 / 600 ≤35W / kg, magnetic induction intensity B 50 ≥1.64T, and longitudinal magnetic induction intensity B 50L With transverse magnetic induction intensity B 50C Difference B does not exceed 1000 Gauss; During the manufacturing process of the non-oriented electrical steel, the texture strength of the {001} surface at a distance of one-quarter of the slab thickness from the surface layer of the intermediate slab before entering the finishing mill is similar to that of the {111} surface. <112> Texture strength ratio I ≥ 0.
55.
2. The non-oriented electrical steel as described in claim 1, characterized in that, Its mass percentage content of each chemical element is as follows: C ≤ 0.005%, Si: 3.1-4.5%, Al: 0.1-2.0%, Mn: 0.1-2.5%; balance is Fe and unavoidable impurities; and satisfies 3.75% ≤ Si + Al ≤ 5.0%.
3. The non-oriented electrical steel as described in claim 1 or 2, characterized in that, Where C ≤ 0.003%.
4. The non-oriented electrical steel as described in claim 1 or 2, characterized in that, Among the unavoidable impurities, P≤0.04%, S≤0.003%, N≤0.005%, O≤0.003%, and Nb+V+Ti≤0.005%.
5. The non-oriented electrical steel as described in claim 4, characterized in that, Among the unavoidable impurities, P ≤ 0.02% and N ≤ 0.0035%.
6. The non-oriented electrical steel as described in claim 1 or 2, characterized in that, It also contains B: 0.0003wt%-0.01wt%.
7. The non-oriented electrical steel as described in claim 1 or 2, characterized in that, It also contains at least one of Sn and Sb, and its total mass percentage content is controlled between 0.005 and 0.3%.
8. The non-oriented electrical steel as described in claim 1 or 2, characterized in that, It also contains at least one of Co, Ni, Cu, and Cr, and the total mass percentage of these elements is controlled between 0.02% and 3.0%.
9. The non-oriented electrical steel as described in claim 1 or 2, characterized in that, Its average grain size is 10-110µm.
10. The non-oriented electrical steel as described in claim 1 or 2, characterized in that, Its thickness is 0.1 to 0.3 mm.
11. The non-oriented electrical steel as described in claim 1 or 2, characterized in that, Its yield strength is ≥430MPa.
12. A method for manufacturing non-oriented electrical steel as described in any one of claims 1-11, characterized in that, Including the following steps: (1) Obtaining a casting billet; (2) Hot rolling: The final rolling reduction rate of the roughing rolling is controlled at 35%-55%. The intermediate slab obtained from the roughing rolling is held at a high temperature for 50-80 seconds before entering the finishing mill. The temperature of the intermediate slab when it enters the finishing mill is 960-1100℃, and the temperature difference between the head and tail of the intermediate slab is controlled. T≤40℃; (3) Normalizing annealing; (4) Cold rolling; (5) Final annealing; (6) Insulating coating.
13. The manufacturing method as described in claim 12, characterized in that, In step (2), the intermediate slab before entering the finishing mill has a {001} surface texture intensity at a distance of one-quarter of the slab surface thickness from the slab surface, which is similar to {111}. <112> Texture strength ratio I ≥ 0.
55.
14. The manufacturing method as described in claim 12, characterized in that, In step (2), the thickness of the intermediate slab obtained is 25-40 mm.
15. The manufacturing method as described in claim 12, characterized in that, In step (5), the annealing temperature is 750-1000℃ and the annealing time is 11-125s.
Citation Information
Patent Citations
Non-oriented magnetic steel sheet with high strength
CN101490294A
Non-oriented electromagnetic steel sheet and method for manufacturing same, and motor core and method for manufacturing same
CN112930412A
High-speed motor rotor non-oriented silicon steel with yield strength larger than or equal to 500 MPa and production method
CN107964631A
Non-oriented electrical steel with low iron loss and high magnetic conductivity and production method thereof
CN112921164A