Lithium-rich manganese-based oxide positive electrode material, precursor and preparation method thereof, lithium-ion battery and electrical equipment
By preparing lithium-rich manganese-based oxide cathode materials with specific crystal structures, the resource and safety issues of cobalt-based or nickel-based materials in lithium-ion batteries are solved, and high capacity and cycle performance improvement under high voltage are achieved, which is suitable for large-scale applications. .
Patent Information
- Application Number
- CN202410790231.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-19
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-06-19
AI Technical Summary
Cobalt-based or nickel-based cathode materials in existing lithium-ion batteries have limited their large-scale application due to limited resources and safety issues. Moreover, lithium-rich manganese-based cathode materials have low battery capacity performance and poor cycle performance, making it difficult to meet the requirements of high performance and low battery life. cost requirements.
A lithium-rich manganese-based oxide cathode material is used. In its X-ray diffraction pattern, the diffraction peak at the diffraction angle 2θ is 20.0°-24.5° and is a single peak with a half-peak width of 0.3°-0.6°. Through co-precipitation The method prepares nickel manganese oxide, and then performs two-stage sintering with a lithium source to form a lithium-rich manganese-based oxide cathode material with a specific crystal structure.
This material significantly improves the capacity performance and cycle performance of the battery at high voltage, is suitable for large-scale industrial production, and provides excellent electrochemical performance.
Smart Images

Figure CN118367136B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of lithium-ion batteries, and in particular to a lithium-rich manganese-based oxide positive electrode material and its precursor and preparation method, a lithium-ion battery and electrical equipment. Background Art
[0002] With the rapid development of new energy electric vehicles and large-scale energy storage, the demand for high-performance and low-cost lithium-ion batteries has prompted extensive research on new battery cathode materials. How to develop a cathode material that can meet both high performance and low cost is a challenging topic. Especially in electric vehicles and large-scale energy storage, commonly used cobalt-based or nickel-based cathode materials are plagued by relatively limited resources and safety issues, which greatly restricts their large-scale application. Lithium-rich manganese-based cathode materials are promising alternatives, but they still face problems such as low battery capacity performance and poor cycle performance.
[0003] Therefore, it is particularly important to develop a relatively low-cost lithium-manganese-rich based positive electrode material with high battery capacity performance and good cycle performance under high voltage. Summary of the invention
[0004] The purpose of the present application is to provide a lithium-rich manganese-based oxide positive electrode material and its precursor and preparation method, a lithium-ion battery and electrical equipment to solve the above problems.
[0005] To achieve the above objectives, this application adopts the following technical solutions:
[0006] A lithium-rich manganese-based oxide positive electrode material, wherein in an X-ray diffraction pattern of the lithium-rich manganese-based oxide positive electrode material, a diffraction peak within a diffraction angle 2θ range of 20.0°-24.5° is a single peak, the single peak is recorded as diffraction peak A, and the half-peak width FWHM (A) of the diffraction peak A is 0.3°-0.6°.
[0007] Optionally, the lithium-rich manganese-based oxide positive electrode material meets one or more of the following conditions:
[0008] A. The diffraction angle 2θ of the lithium-rich manganese-based oxide positive electrode material corresponding to the peak position of the diffraction peak A is 20.0°-21.0°;
[0009] B. The half-peak width FWHM (A) of the diffraction peak A of the lithium-rich manganese-based oxide positive electrode material is 0.4°-0.5°;
[0010] C. The number of crystal plane sheets N corresponding to the diffraction peak A of the lithium-rich manganese-based oxide positive electrode material (A) 20-70;
[0011] D. Peak intensity I of diffraction peak A of the lithium-rich manganese-based oxide positive electrode material(A) The peak intensity I of the diffraction peak in the diffraction angle 2θ range of 44.0°-45.0° (104) The ratio I (A) / I (104) is 0.07-0.12; optionally, I (A) / I (104) 0.075-0.090;
[0012] E. Peak intensity I of diffraction peak A of the lithium-rich manganese-based oxide positive electrode material (A) The peak intensity I of the diffraction peak in the diffraction angle 2θ range of 18.1°-19.1° (003) The ratio I (A) / I (003) is 0.07-0.12; optionally, I (A) / I (003) It is 0.075-0.11.
[0013] Optionally, the lithium-rich manganese-based oxide positive electrode material satisfies one or more of the following conditions:
[0014] (1) The lithium-rich manganese-based oxide positive electrode material has at least four diffraction peaks within a diffraction angle 2θ range of 55°-70°;
[0015] (2) The peak intensity I of the diffraction peak of the lithium-rich manganese-based oxide positive electrode material in the diffraction angle 2θ range of 59.1°-64.5° (018) The peak intensity I of the diffraction peak in the diffraction angle 2θ range of 64.6°-65.2° (110) The ratio I (018) / I (110) 0.9-1.2;
[0016] (3) The peak position of the diffraction peak of the lithium-rich manganese-based oxide positive electrode material in the diffraction angle 2θ range of 64.6°-65.2° (110) The peak position of the diffraction peak in the range of diffraction angle 2θ of 59.1°-64.5° (018) The difference 2θ (110) -2θ (018) It is 0.7°-0.8°.
[0017] Optionally, the lithium-rich manganese-based oxide positive electrode material satisfies one or more of the following conditions:
[0018] (1) The lithium-rich manganese-based oxide positive electrode material has at least three diffraction peaks within a diffraction angle 2θ range of 35°-40°;
[0019] (2) The grain size D(006) of the crystal plane of the lithium-rich manganese-based oxide positive electrode material corresponding to the diffraction peak in the diffraction angle 2θ range of 37.5°-38.1° is 480-850Å; optionally, D(006) is 480-720Å.
[0020] Optionally, the lithium-rich manganese-based oxide positive electrode material meets one or more of the following conditions:
[0021] a. The secondary particles of the lithium-rich manganese-based oxide positive electrode material include a plurality of plate-like primary particles;
[0022] b. The average particle size D50 of the lithium-rich manganese-based oxide positive electrode material is 2-6 μm;
[0023] c. The chemical formula of the lithium-rich manganese-based oxide positive electrode material is Li x Ni y Mn z O 2+δ , among which, 1.1≤x≤1.5, 0.1≤y≤0.4, 0.6≤z≤0.9, 0.15≤δ≤0.65.
[0024] The present application also provides a precursor of a lithium-rich manganese-based oxide positive electrode material, which satisfies one or more of the following conditions:
[0025] (1) The chemical formula of the precursor of the lithium-rich manganese-based oxide positive electrode material is Ni a Mn b (OH)2, 0.5≤b<1, a+b≤1;
[0026] (2) The average particle size D50 of the precursor of the lithium-rich manganese-based oxide positive electrode material is 2-6 μm;
[0027] (3) The Span of the secondary particles of the lithium-rich manganese-based oxide positive electrode material precursor is (D90-D10) / D50 of 0.5-0.7;
[0028] (4) The tap density of the lithium-rich manganese-based oxide positive electrode material precursor is 1.1-1.3 g / cm³;
[0029] (5) The specific surface area of the precursor of the lithium-rich manganese-based oxide positive electrode material is 10-20m 2 / g;
[0030] (6) The precursor secondary particles of the lithium-rich manganese-based oxide positive electrode material include a plurality of plate-shaped primary particles.
[0031] The present application also provides a method for preparing the lithium-rich manganese-based oxide positive electrode material, comprising:
[0032] A metal salt solution including manganese salt and nickel salt, a precipitant and a complexing agent are introduced into the bottom liquid to perform a coprecipitation reaction to obtain a precursor; during the coprecipitation reaction, the mother liquid is discharged, and the discharge rate of the mother liquid is consistent with the total liquid feeding rate;
[0033] The precursor is subjected to a first sintering to obtain nickel manganese oxide;
[0034] The nickel-manganese oxide is cooled and mixed with a lithium source, and subjected to a second sintering to obtain the lithium-rich manganese-based oxide positive electrode material.
[0035] Optionally, the preparation method of the lithium-rich manganese-based oxide positive electrode material meets one or more of the following conditions:
[0036] (1) The precipitant includes sodium hydroxide, and the mass fraction of the precipitant is 10-30wt%;
[0037] (2) The complexing agent includes one or more of ammonia water, ammonium sulfate or ammonium chloride, and the mass fraction of the complexing agent is 10-30wt%;
[0038] (3) The base liquid includes one or more of water, the precipitant and the complexing agent;
[0039] (4) The total metal content in the metal salt solution is 1-8 mol / L;
[0040] (5) The pH value of the base liquid is 10.4-12.8, and the ammonia concentration in the base liquid is 3-8 g / L;
[0041] (6) The temperature of the coprecipitation reaction is 60-80°C;
[0042] (7) The flow rate of the metal salt solution is 0.5-2.0% / h of the volume of the reaction container, the pH value during the coprecipitation reaction is 9.4-11.6, and the ammonia concentration during the coprecipitation reaction is 4.2-8.6 g / L;
[0043] (8) The coprecipitation reaction is carried out under stirring conditions at a stirring speed of 450-800 rpm;
[0044] (9) After the coprecipitation reaction is completed, the method further comprises: solid-liquid separation, and then washing and drying the solid;
[0045] (10) The atmospheres of the first sintering and the second sintering are independently air or oxygen atmospheres;
[0046] (11) The first sintering includes a first sintering heating stage and a first sintering heat preservation stage. The temperature in the first sintering heating stage is raised to 425-675°C. The heating rate in the first sintering heating stage is 2-4°C / min. The heat preservation time in the first sintering heat preservation stage is 6-10h.
[0047] (12) The second sintering includes a second sintering heating stage and a second sintering keeping stage. The temperature in the second sintering heating stage is raised to 875-1025°C. The heating rate in the second sintering heating stage is 20-30°C / min. The keeping time in the second sintering keeping stage is 6-10h.
[0048] The present application also provides a lithium-ion battery, comprising the lithium-rich manganese-based oxide positive electrode material.
[0049] The present application also provides an electrical device, including the lithium-ion battery.
[0050] Compared with the prior art, the beneficial effects of this application include:
[0051] The lithium-rich manganese-based oxide positive electrode material provided in the present application has a single peak in the diffraction angle 2θ range of 20.0°-24.5°, and its half-peak width FWHM(A) is 0.3°-0.6°. The position of the strongest diffraction peak of the lithium-rich manganese-based oxide positive electrode material provided in the present application in the diffraction angle 2θ range of 20.0°-24.5° is slightly shifted to a low angle, and the XRD spectrum shows that the original multiple diffraction peaks are optimized to a single diffraction peak (i.e., a single peak), and the width of the diffraction peak is significantly larger, indicating that the crystal structure of the positive electrode material has changed, forming a better lithium-rich manganese phase Li2MnO3, which can improve the Li + The migration channels can be expanded and the electrochemical reactions can be better participated in, so the capacity and cycle performance can be improved when used in batteries.
[0052] The preparation method of the lithium-rich manganese-based oxide positive electrode material provided in the present application is to first prepare nickel manganese hydroxide by a coprecipitation method, and then obtain the lithium-rich manganese-based oxide positive electrode material by two-stage sintering with a lithium source; the process can be applied to large-scale industrial production. The nickel manganese hydroxide prepared in the present application has a narrow span value, good secondary particle consistency, and moderate specific surface area and tap density; the secondary particles of the prepared lithium-rich manganese-based oxide positive electrode material include a plurality of plate-like primary particles, and the C2 / m monoclinic structure Li2MnO3 and the Rm rhombohedral structure LiMnO2 in the positive electrode material are arranged in a certain proportion and manner, and have a specific crystal structure, which can improve the battery capacity performance and cycle performance under high voltage.
[0053] The lithium-ion battery and electrical equipment provided in this application have excellent electrical performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0054] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope of the present application.
[0055] Figure 1 This is a surface SEM photo of the precursor prepared in Example 1;
[0056] Figure 2 for Figure 1 A partial enlarged photo of
[0057] Figure 3 This is a SEM photo of the positive electrode material prepared in Example 1;
[0058] Figure 4 This is a SEM photo of the positive electrode material prepared in Comparative Example 1;
[0059] Figure 5 This is the XRD pattern of the positive electrode material prepared in Comparative Example 6;
[0060] Figure 6 This is the XRD pattern of the positive electrode material prepared in Comparative Example 7;
[0061] Figure 7 XRD comparison diagram of the lithium-rich manganese-based oxide positive electrode materials prepared in Example 1-2 and Comparative Example 1-7 within the diffraction angle range of 2θ=20°-30°;
[0062] Figure 8 XRD comparison diagram of the lithium-rich manganese-based oxide positive electrode materials prepared in Example 1-2 and Comparative Example 1-7 within the diffraction angle range of 2θ=55°-70°;
[0063] Fig. 9 This is an XRD comparison diagram of the lithium-rich manganese-based oxide positive electrode materials prepared in Example 1-2 and Comparative Example 1-7 within the diffraction angle 2θ range of 35°-40°. DETAILED DESCRIPTION
[0064] In order to better explain the technical solution provided by this application, before the embodiments, the technical solution is first described as a whole, as follows:
[0065] The XRD data of the lithium-rich manganese-based oxide positive electrode material prepared in the present application is tested and calculated by the following method: the XRD raw data of the sample is obtained by testing with a Bruker D8A A25X instrument under Cu-Kα radiation, and then the data is refined and calculated using the X-ray powder diffraction comprehensive analysis software PDXL (manufactured by Rigaku Corporation) to obtain the grain size corresponding to each crystal plane, the diffraction peak intensity corresponding to each diffraction peak, the half-peak width and other data, and finally the peak intensity ratio of the two specified diffraction peaks, the grain size of the crystal plane corresponding to the diffraction peak and the number of crystal plane layers are calculated.
[0066] In an X-ray diffraction pattern of a lithium-rich manganese-based oxide positive electrode material, a diffraction peak within a diffraction angle 2θ range of 20.0°-24.5° is a single peak, which is recorded as diffraction peak A. The half-peak width FWHM (A) of diffraction peak A is 0.3°-0.6°.
[0067] Optionally, the half-peak width FWHM (A) of the diffraction peak of the lithium-rich manganese-based oxide positive electrode material in the diffraction angle 2θ range of 20.0°-24.5° can be 0.3°, 0.31°, 0.32°, 0.33°, 0.34°, 0.35°, 0.36°, 0.37°, 0.38°, 0.39°, 0.4°, 0.41°, 0.42°, 0.43°, 0.44°, 0.45°, 0.46°, 0.47°, 0.48°, 0.49°, 0.5°, 0.51°, 0.52°, 0.53°, 0.54°, 0.55°, 0.56°, 0.57°, 0.58°, 0.59°, 0.60°, 0.61°, 0.62°, 0.63°, 0.64°, 0.65°, 0.66°, 0.67°, 0.68°, 0.69°, 0.70°, 0.71°, 0.72°, 0.73°, 0.74°, 0.75°, 0.76°, 0.77°, 0.78°, 0.79°, 0.80°, 0.81°, 0.82°, 0.83°, 0.84°, .53°, 0.54°, 0.55°, 0.56°, 0.57°, 0.58°, 0.59°, 0.6° or any value between 0.3°-0.6° or any interval within the above range such as 0.3°-0.4°, 0.4°-0.5°, 0.5°-0.6°, 0.3°-0.5°, 0.4°-0.6°, 0.34°-0.44°, etc.;
[0068] Mn 4+ Ionic radius: 0.54Å, Ni 2+ Ionic radius: 0.69Å, Ni has a larger ionic radius than Mn. Ni replaces Mn to form a Li-O-Li structure, causing the diffraction peak to shift toward the low-angle side. Due to the increase in the Li-O-Li structure, more oxygen ions participate in the redox reaction to provide additional capacity. In addition, the covalent bond between the replacement element Ni and O is enhanced, which can also reduce the detachment of oxygen from the lattice accompanying the oxidation of the transition metal, thereby inhibiting the generation of oxygen and reducing oxygen defects in the crystal structure, making the crystal structure more stable to prevent particle breakage, that is, further inhibiting the dissolution of Mn during charge and discharge, and using it in batteries can improve capacity performance and cycle performance at high voltages.
[0069] The diffraction angle 2θ at 20.0°-24.5° corresponds to the Li2MnO3 superlattice diffraction peak. In the XRD spectrum, multiple peaks are optimized to a single peak, and the width of the strongest diffraction peak is significantly larger. Its crystal structure has changed, forming a better lithium-rich manganese phase Li2MnO3, which can improve the Li + The migration channel can be better participated in the electrochemical reaction, showing the improvement of capacity performance and cycle performance.
[0070] In an optional embodiment, the X-ray diffraction pattern of the lithium-rich manganese-based oxide positive electrode material satisfies one or more of the following conditions:
[0071] A. The diffraction angle 2θ corresponding to the peak position of diffraction peak A of the lithium-rich manganese-based oxide positive electrode material is 20.0°-21.0°;
[0072] The lithium-rich manganese-based oxide positive electrode material provided in the present application has a strongest diffraction peak position in the diffraction angle 2θ range of 20.0°-24.5° (diffraction angle 2θ is near 21.5°) that is slightly shifted to a lower angle (diffraction angle 2θ is near 20.5°), indicating that more Mn is replaced by Ni and solid-dissolved in the positive electrode material, the structure is more stable, and the dissolution of Mn is inhibited. When used in batteries, it can improve the capacity performance and cycle performance at high voltage.
[0073] B. The half-peak width FWHM(A) of the diffraction peak A of the lithium-rich manganese-based oxide positive electrode material is 0.4°-0.5°;
[0074] C. The number of crystal planes N corresponding to the diffraction peak A of the lithium-rich manganese-based oxide positive electrode material (A) 20-70;
[0075] Li + The transmission path and deintercalation speed of the lithium-rich manganese-based oxide positive electrode material prepared in this application has a small number of crystal planes corresponding to the diffraction peak A in the range of 20.0°-21.0°. + The transmission path on the crystal plane is shorter, which is beneficial to the utilization of capacity; however, when the number of crystal facets on the positive electrode material corresponding to the diffraction peak A in the range of 2θ of 20.0°-21.0° is too small, the crystal tends to grow on other crystal planes, which in turn affects the transmission of lithium ions on the corresponding crystal plane and is not conducive to the utilization of capacity.
[0076] Optionally, the number of crystal plane sheets N of the crystal plane corresponding to the diffraction peak A of the lithium-rich manganese-based oxide positive electrode material (A)40, 45, 46, 47, 48, 49, 50, 51, 52, 53, 54, 55, 56, 57, 58, 59, 60, 61, 62, 63, 64, 65, 66, 67, 68, 69, 70 or any value between 20 and 70, or any interval within the above range such as 20-30, 30-40, 40-50, 50-60, 60-70, 20-60, 35-70, 30-60, etc.;
[0077] D. Peak intensity I of diffraction peak A of lithium-rich manganese-based oxide positive electrode material (A) The peak intensity I of the diffraction peak in the diffraction angle 2θ range of 44.0°-45.0° (104) The ratio I (A) / I (104) is 0.07-0.12; optionally, I (A) / I (104) is 0.075-0.090; wherein, the diffraction peak of the lithium-rich manganese-based oxide positive electrode material in the diffraction angle 2θ range of 20.0°-21.0° corresponds to the (104) crystal plane, the same below;
[0078] Optionally, the peak intensity I of the diffraction peak A of the lithium-rich manganese-based oxide positive electrode material is (A) The peak intensity I of the diffraction peak in the diffraction angle 2θ range of 44.0°-45.0° (104) The ratio I (A) / I (104) It can be 0.07, 0.075, 0.080, 0.085, 0.090, 0.095, 0.10, 0.105, 0.11, 0.115, 0.12 or any value between 0.07 and 0.12 or any interval within the above range such as 0.08-0.10, 0.075-0.090, 0.90-0.12, 0.075-0.11, 0.081-0.088, etc.;
[0079] E. Peak intensity I of diffraction peak A of lithium-rich manganese-based oxide positive electrode material (A) The peak intensity I of the diffraction peak in the diffraction angle 2θ range of 18.1°-19.1° (003) The ratio I (A) / I (003) is 0.07-0.12; optionally, I (A) / I (003) It is 0.075-0.11.
[0080] Optionally, the peak intensity I of the diffraction peak A of the lithium-rich manganese-based oxide positive electrode material is (A) The peak intensity I of the diffraction peak with a diffraction angle 2θ in the range of 18.1°-19.1° (003) The ratio I (A) / I (003) It can be 0.07, 0.08, 0.09, 0.10, 0.11, 0.12 or any value between 0.07-0.12 or any interval within the above range such as 0.08-0.10, 0.075-0.10, 0.075-0.11, 0.080-0.090, 0.084-0.088, etc.
[0081] The lithium-rich manganese-based cathode material is equivalent to the C2 / m monoclinic structure (first phase) of Li2MnO3 and the R of LiMO2 (M=Ni, Mn). In order to make the lithium secondary battery prepared by lithium-rich manganese-based positive electrode materials show high capacity at high voltage, it is necessary to maintain the stable structure of LiMO2 under high voltage and activate Li2MnO3 under high voltage, so as to improve the capacity performance and cycle performance under high voltage.
[0082] The (003) diffraction peak reflects the R m rhombohedral structure, (104) diffraction peak reflects the mixed phase of R m rhombohedral structure LiMO2 and C2 / m monoclinic structure Li2MnO3; the diffraction peak in the range of diffraction angle 2θ of 20.0°-21.0° reflects the C2 / m monoclinic structure Li2MnO3. I (A) / I (003) ,I (A) / I (104) The ratio of C2 / m monoclinic structure and R in the crystal of lithium-rich manganese-based positive electrode material can be within a certain range. The m rhombohedral structure is arranged in a certain proportion and in a specific way, and has a special crystal structure.
[0083] In an optional embodiment, the X-ray diffraction pattern of the lithium-rich manganese-based oxide positive electrode material satisfies one or more of the following conditions:
[0084] (1) The lithium-rich manganese-based oxide positive electrode material has at least four diffraction peaks within the diffraction angle 2θ range of 55°-70°;
[0085] (2) The peak intensity I of the diffraction peak of the lithium-rich manganese-based oxide positive electrode material in the diffraction angle 2θ range of 59.1°-64.5° (018) The peak intensity I of the diffraction peak in the diffraction angle 2θ range of 64.6°-65.2° (110) The ratio I (018) / I (110) 0.9-1.2;
[0086] Optionally, the peak intensity I of the diffraction peak of the lithium-rich manganese-based oxide positive electrode material in the diffraction angle 2θ range of 59.1°-64.5° (018) The peak intensity I of the diffraction peak in the diffraction angle 2θ range of 64.6°-65.2° (110) The ratio I (018) / I (110) It can be 0.9, 0.91, 0.92, 0.94, 0.96, 0.98, 1.0, 1.02, 1.04, 1.06, 1.08, 1.1, 1.12, 1.14, 1.16, 1.18, 1.2 or any value between 0.9 and 1.2 or any interval within the above range such as 0.97-1.03, 0.9-1.05, 1.1-1.2, 0.97-1.03, etc.;
[0087] The peak intensity ratios of (018) and (110) are close, the degree of double peak splitting is good, Ni is doped into the lattice, the rhombohedral structure of LiMO2 is obvious, which makes the crystal structure more stable, inhibits the dissolution of Mn at high voltage, and exerts the activity of lattice oxygen of Li2MnO3 phase in the positive electrode material. When used in batteries, it can improve the capacity performance and cycle performance at high voltage.
[0088] (3) Peak position of the diffraction peak of the lithium-rich manganese-based oxide positive electrode material in the diffraction angle 2θ range of 64.6°-65.2° (110) The peak position of the diffraction peak in the range of diffraction angle 2θ of 59.1°-64.5° (018) The difference 2θ (110) -2θ (018) 0.7°-0.8°;
[0089] The 2θ difference between the peaks is related to the arrangement of lithium and transition metal ions in the crystal structure of the positive electrode material, showing improved charge capacity and cycle performance. When split into two peaks, it is inferred that the positive electrode material has a Li-rich layered (OLO) structure, in which lithium excess regions and / or metal cations penetrate each other to form a solid solution material with significant preferential orientation.
[0090] Optionally, the peak position of the diffraction peak of the lithium-rich manganese-based oxide positive electrode material in the diffraction angle 2θ range of 64.6°-65.2° is (110) The peak position of the diffraction peak in the range of diffraction angle 2θ of 59.1°-64.5° (018) The difference 2θ (110) -2θ (018)It can be 0.7°, 0.71°, 0.72°, 0.73°, 0.74°, 0.75°, 0.76°, 0.77°, 0.78°, 0.79°, 0.8° or any value between 0.7° and 0.8° or any interval within the above range such as 0.77°-0.78°, 0.74°-0.78°, 0.777°-0.785°, etc.
[0091] In an optional embodiment, the X-ray diffraction pattern of the lithium-rich manganese-based oxide positive electrode material satisfies one or more of the following conditions:
[0092] (1) The lithium-rich manganese-based oxide positive electrode material has at least three diffraction peaks within the diffraction angle 2θ range of 35°-40°;
[0093] (2) The grain size D(006) of the crystal plane of the lithium-rich manganese-based oxide positive electrode material corresponding to the diffraction peak in the diffraction angle 2θ range of 37.5°-38.1° is 480-850Å; optionally, D(006) is 480-720Å.
[0094] Optionally, the grain size D(006) of the crystal plane corresponding to the diffraction peak with a diffraction angle 2θ in the range of 37.5°-38.1° of the lithium-rich manganese-based oxide positive electrode material can be 480Å, 490Å, 500Å, 510Å, 520Å, 530Å, 540Å, 550Å, 560Å, 570Å, 580Å, 590Å, 600Å, 610Å, 620Å, 630Å, 640Å, 650Å, 660Å 400Å, 750Å, 760Å, 770Å, 780Å, 790Å, 800Å, 810Å, 820Å, 830Å, 840Å, 850Å or any value between 480 and 850Å or any interval within the above range such as 480-528Å, 528-704Å, 600-704Å, etc.
[0095] Due to its special atomic arrangement and higher R The m-symmetric LiMO2 phase regulates the oxygen redox activity; thermodynamically, Li is preferentially extracted from the Li layer in the crystal structure. + Instead of Li in the Mn layer + ; In addition, at high potential, part of the Li is still retained in the Mn layer, stabilizing the structural framework of the material, thereby improving the capacity performance and cycle performance of the positive electrode material at high voltage.
[0096] During the lithium insertion process, if the temperature is too low, it will cause uneven lithium insertion, which will increase the proportion of spinel phase and cause inhomogeneity in morphology and phase structure; 2θ is a triple peak at 35°-40°, and the original LiMn2O4 spinel impurity shoulder peak disappears, showing higher capacity performance. The crystal plane corresponding to the diffraction peak in the diffraction angle 2θ range of 37.5°-38.1° of the lithium-rich manganese-based oxide positive electrode material has a larger grain size, high crystallinity, and stable crystal structure. It can be used in batteries to improve capacity performance and cycle performance at high voltage.
[0097] In an optional embodiment, the lithium-rich manganese-based oxide positive electrode material satisfies one or more of the following conditions:
[0098] a. The secondary particles of the lithium-rich manganese-based oxide positive electrode material include a plurality of plate-like primary particles;
[0099] In the partial magnified photos of the surface SEM, some primary particles are arranged vertically to the plane of the photo, and only one or more strip-shaped faces can be seen. Primary particles with this morphology are also identified as plate-like primary particles, the same below;
[0100] b. The average particle size D50 of the lithium-rich manganese-based oxide positive electrode material is 2-6 μm;
[0101] Optionally, the average particle size D50 of the lithium-rich manganese-based oxide positive electrode material can be 2 μm, 3 μm, 4 μm, 5 μm, 6 μm or any value between 2-6 μm or any interval within the above range such as 2-4 μm, 4-6 μm, 3-5 μm, etc.;
[0102] c. The chemical formula of lithium-rich manganese-based oxide positive electrode material is Li x Ni y Mn z O 2+δ , where 1.1≤x≤1.5, 0.1≤y≤0.4, 0.6≤z≤0.9, 0.15≤δ≤0.65;
[0103] Optionally, x can be 1.1, 1.12, 1.14, 1.16, 1.18, 1.2, 1.22, 1.24, 1.26, 1.28, 1.3, 1.32, 1.34, 1.36, 1.38, 1.4, 1.42, 1.44, 1.46, 1.48, 1.5 or any value between 1.1 and 1.5; y can be 0.1, 0.11, 0.12, 0.13, 0.14, 0.15, 0.16, 0.17, 0.18, 0.19, 0.2, 0.21 , 0.22, 0.23, 0.24, 0.25, 0.26, 0.27, 0.28, 0.29, 0.30, 0.31, 0.32, 0.33, 0.34, 0.35, 0.36, 0.37, 0.38, 0.39, 0.40 or any value between 0.1 and 0.4; z can be 0.6, 0.61, 0.62, 0.63, 0.64, 0.65, 0.66, 0.67, 0.68, 0.69, 0.7, 0.71, 0.72, 0.73, 0. 74, 0.75, 0.76, 0.77, 0.78, 0.79, 0.8, 0.81, 0.82, 0.83, 0.84, 0.85, 0.86, 0.87, 0.88, 0.89, 0.9 or any value between 0.6 and 0.9; δ can be 0.15, 0.16, 0.17, 0.18, 0.19, 0.20, 0.21, 0.22, 0.23, 0.24, 0.25, 0.26, 0.27, 0.28, 0.29, 0.30, 0.31, 0.32, 0.33, 0.34, 0.35, 0.36, 0.37, 0.38, 0.39, 0.40, 0.41, 0.42, 0.43, 0.44, 0.45, 0.46, 0.47, 0.48, 0.49, 0.5, 0.51, 0.52, 0.53, 0.54, 0.55, 0.56, 0.57, 0.58, 0.59, 0.6, 0.61, 0.62, 0.63, 0.64, 0.65 or any value between 0.15 and 0.65.
[0104] In an optional embodiment, the molar ratio of y to z is 3:1.
[0105] The present application also provides a precursor of a lithium-rich manganese-based oxide positive electrode material, which satisfies one or more of the following conditions:
[0106] (1) The chemical formula of the precursor of lithium-rich manganese-based oxide positive electrode material is Ni a Mn b (OH)2, 0.5≤b<1, a+b≤1;
[0107] Optionally, b can be 0.5, 0.51, 0.52, 0.53, 0.54, 0.55, 0.56, 0.57, 0.58, 0.59, 0.6, 0.61, 0.62, 0.63, 0.64, 0.65, 0.66, 0.67, 0.68, 0.69, 0.70, 0.71, 0.72, 0.73, 0.74, 0.75, 0.76, 0.77, 0.78, 0.79, 0.80, 0.81, 0.82, 0.83, 0.84, 0.85, 0.86, 0.87, 0.88, a+b can be 0.90, 0.91, 0.92, 0.93, 0.94, 0.95, 0.96, 0.97, 0.98, 0.99, or any value greater than 0.5 and less than 1, or any interval within the above range such as 0.5≤b<0.75, 0.75≤b<1, 0.6≤b<0.8, etc.; a+b can be 0.90, 0.91, 0.92, 0.93, 0.94, 0.95, 0.96, 0.97, 0.98, 0.99, 1.00, or any value greater than 0.90 and less than or equal to 1.
[0108] In an optional embodiment, the chemical formula of the precursor of the lithium-rich manganese-based oxide positive electrode material is Ni 0.25 Mn 0.75 (OH)2;
[0109] (2) The average particle size D50 of the precursor of the lithium-rich manganese-based oxide positive electrode material is 2-6 μm.
[0110] Optionally, the average particle size D50 of the precursor of the lithium-rich manganese-based oxide positive electrode material can be 2 μm, 3 μm, 4 μm, 5 μm, 6 μm or any value between 2-6 μm or any interval within the above range such as 2-4 μm, 4-6 μm, 3-6 μm, etc.;
[0111] (3) The Span of the secondary particles of the lithium-rich manganese-based oxide positive electrode material precursor is (D90-D10) / D50 is 0.5-0.7;
[0112] Optionally, the average particle size Span value of the lithium-rich manganese-based oxide positive electrode material precursor can be 0.5, 0.52, 0.54, 0.56, 0.58, 0.6, 0.62, 0.64, 0.66, 0.68, 0.7 or any value therebetween;
[0113] (4) The tap density of the lithium-rich manganese-based oxide cathode material precursor is 1.1-1.3 g / cm³;
[0114] Optionally, the tap density of the lithium-rich manganese-based oxide positive electrode material precursor may be 1.0 g / cm³, 1.02 g / cm³, 1.04 g / cm³, 1.06 g / cm³, 1.08 g / cm³, 1.1 g / cm³, 1.12 g / cm³, 1.14 g / cm³, 1.16 g / cm³, 1.18 g / cm³, 1.2 g / cm³ or any value between 1.1-1.3 g / cm³ or any interval within the above range such as 1.0-1.1 g / cm³, 1.1-1.2 g / cm³, 1.05-1.15 g / cm³, etc.;
[0115] (5) The specific surface area of the lithium-rich manganese-based oxide cathode material precursor is 10-20m 2 / g;
[0116] Optionally, the specific surface area of the lithium-rich manganese-based oxide positive electrode material precursor can be 10m 2 / g, 11m 2 / g, 12m 2 / g, 13m 2 / g, 14m 2 / g, 15m 2 / g, 16m 2 / g, 17m 2 / g, 18m 2 / g, 19m 2 / g, 20m 2 / g or 10-20m 2 Any value between / g or any interval within the above range such as 10-15m 2 / g, 15-20m 2 / g, 12-18m 2 / g, 13-17m 2 / g, 14-16m 2 / g, etc.
[0117] (6) The precursor secondary particles of the lithium-rich manganese-based oxide positive electrode material include a plurality of plate-like primary particles.
[0118] The present application also provides a method for preparing a lithium-rich manganese-based oxide positive electrode material, comprising:
[0119] A metal salt solution including manganese salt and nickel salt, a precipitant and a complexing agent are introduced into the bottom liquid to perform a coprecipitation reaction to obtain a precursor; during the coprecipitation reaction, the mother liquid is discharged, and the discharge rate of the mother liquid is consistent with the total liquid feeding rate;
[0120] The precursor is first sintered to obtain nickel manganese oxide;
[0121] The nickel manganese oxide is cooled and mixed with a lithium source, and a second sintering is performed to obtain a lithium-rich manganese-based oxide positive electrode material.
[0122] The nickel manganese hydroxide prepared in the present application has a narrow span and good consistency of secondary particles; and the specific surface area and tap density are moderate; the secondary particles of the prepared lithium-rich manganese-based oxide positive electrode material include a plurality of plate-like primary particles, in which the C2 / m monoclinic structure Li2MnO3 and the Rm rhombohedral structure LiMnO2 are arranged in a certain proportion and manner, and have a specific crystal structure, which can improve the battery capacity performance and cycle performance under high voltage.
[0123] In an optional embodiment, the preparation method of the lithium-rich manganese-based oxide positive electrode material satisfies one or more of the following conditions:
[0124] (1) The precipitant includes sodium hydroxide, and the mass fraction of the precipitant is 10-30wt%;
[0125] Optionally, the mass fraction of the precipitant may be 10wt%, 15wt%, 20wt%, 25wt%, 30wt% or any value between 10-30wt%;
[0126] (2) The complexing agent includes one or more of ammonia water, ammonium sulfate or ammonium chloride, and the mass fraction of the complexing agent is 10-30wt%;
[0127] Optionally, the mass fraction of the complexing agent may be 10wt%, 15wt%, 20wt%, 25wt%, 30wt% or any value between 10% and 30wt%;
[0128] (3) The base liquid includes one or more of water, a precipitant and a complexing agent;
[0129] (4) The total metal content in the metal salt solution is 1-8 mol / L;
[0130] Optionally, the total metal content in the metal salt solution may be 1 mol / L, 2 mol / L, 3 mol / L, 4 mol / L, 5 mol / L, 6 mol / L, 7 mol / L, 8 mol / L or any value between 1 and 8 mol / L;
[0131] (5) The pH value of the base solution is 10.4-12.8, and the ammonia concentration in the base solution is 3-8 g / L;
[0132] Optionally, the pH value of the base solution can be 10.4, 10.5, 10.6, 10.7, 10.8, 10.9, 11.0, 11.1, 11.2, 11.3, 11.4, 11.5, 11.6, 11.7, 11.8 or any value between 10.4 and 12.8; the ammonia concentration in the base solution can be 3g / L, 3.1g / L, 3.2g / L, 3.3g / L, 3.4g / L, 3.5g / L, 3.6g / L, 3.7g / L, 3.8g / L, 3.9g / L, 4g / L, 4.0g / L, 4.1g / L, 4.2g / L, 4.3g / L, 4.4g / L, 4.5g / L, 4.6g / L, 4.7g / L, 4.8g / L g / L, 4.9g / L, 5g / L, 5.1g / L, 5.2g / L, 5.3g / L, 5.4g / L, 5.5g / L, 5.6g / L, 5.7g / L, 5.8g / L, 5.9g / L, 6g / L, 6.1g / L, 6.2g / L, 6.3g / L, 6.4g / L, 6.5g / L, 6.6g / L, 6.7g / L, 6.8g / L, 6.9g / L, 7g / L, 7.1g / L, 7.2g / L, 7.3g / L, 7.4g / L, 7.5g / L, 7.6g / L, 7.7g / L, 7.8g / L, 7.9g / L, 8g / L or any value between 3-8g / L; wherein ammonia concentration refers to NH4 + The mass concentration of, the same below;
[0133] (6) The temperature of the coprecipitation reaction is 60-80°C;
[0134] Optionally, the temperature of the coprecipitation reaction can be 60°C, 65°C, 70°C, 75°C, 80°C or any value between 60-80°C;
[0135] (7) The flow rate of the metal salt solution is 0.5-2.0% / h of the volume of the reaction vessel, the pH value during the coprecipitation reaction is 9.4-11.6, and the ammonia concentration during the coprecipitation reaction is 4.2-8.6 g / L;
[0136] Optionally, the flow rate of the metal salt solution can be 0.5% / h, 0.6% / h, 0.7% / h, 0.8% / h, 0.9% / h, 1.0% / h, 1.1% / h, 1.2% / h, 1.3% / h, 1.4% / h, 1.5% / h, 1.6% / h, 1.7% / h, 1.8% / h, 1.9% / h, 2.0% / h or any value between 0.5-2.0% / h of the volume of the reaction vessel. The pH value during the reaction can be 9.4, 9.5, 9.6, 9.7, 9.8, 9.9, 10.0, 10.1, 10.2, 10.3, 10.4, 10.5, 10.6, 10.7, 10.8, 10.9, 11.0, 11.1, 11.2, 11.3, 11.4, 11.5, 11.6 or any value between 9.4 and 11.6. The ammonia concentration during the coprecipitation reaction can be 4.2 g / L, 4 .3g / L, 4.4g / L, 4.5g / L, 4.6g / L, 4.7g / L, 4.8g / L, 4.9g / L, 5g / L, 5.1g / L, 5.2g / L, 5.3g / L, 5.4g / L, 5.5g / L, 5.6g / L, 5.7g / L, 5.8g / L, 5.9g / L, 6g / L, 6.1g / L, 6.2g / L, 6.3g / L, 6.4g / L, 6.5g / L, 6. 6g / L, 6.7g / L, 6.8g / L, 6.9g / L, 7g / L, 7.1g / L, 7.2g / L, 7.3g / L, 7.4g / L, 7.5g / L, 7.6g / L, 7.7g / L, 7.8g / L, 7.9g / L, 8g / L, 8.1g / L, 8.2g / L, 8.3g / L, 8.4g / L, 8.5g / L, 8.6g / L or any value between 4.2-8.6g / L;
[0137] (8) The coprecipitation reaction is carried out under stirring conditions at a stirring speed of 450-800 rpm;
[0138] Optionally, the stirring speed may be 450 rpm, 500 rpm, 550 rpm, 600 rpm, 650 rpm, 700 rpm, 750 rpm, 800 rpm or any value between 450-800 rpm;
[0139] (9) After the coprecipitation reaction is completed, the method further includes: solid-liquid separation, and then washing and drying the solid matter;
[0140] (10) The atmospheres of the first sintering and the second sintering are independently air or oxygen atmospheres;
[0141] (11) The first sintering includes a first sintering heating stage and a first sintering heat preservation stage. The temperature in the first sintering heating stage is raised to 425-675°C. The heating rate in the first sintering heating stage is 2-4°C / min. The heat preservation time in the first sintering heat preservation stage is 6-10h.
[0142] During direct sintering, there is a large temperature range between the decomposition of lithium salt and precursor and the formation of lithium manganese oxide, indicating that the system has a large ion diffusion resistance, which is not conducive to the penetration of lithium salt. In addition, during the lithium insertion process, too low a temperature will cause uneven lithium insertion, thereby increasing the proportion of spinel phase, resulting in uneven morphology and phase structure, thereby affecting the structural stability of the positive electrode material under high voltage, and ultimately affecting the capacity performance and cycle performance of the positive electrode material under high voltage. By first sintering nickel manganese hydroxide to nickel manganese oxide at a relatively low temperature, the rapid overflow of water vapor decomposed by the violent reaction of the precursor at high temperature, resulting in the rupture of primary and secondary particles, etc., is slowed down or avoided, thereby improving the structural stability of the material; then the second sintering temperature is increased to accelerate the decomposition of lithium salt, and through the regulation of oxygen activity and lattice structure, a lithium manganese oxide positive electrode material with uniform phase distribution is obtained, which exhibits better capacity performance and cycle performance under high voltage.
[0143] Optionally, the terminal temperature of the first sintering heating stage can be 425°C, 450°C, 475°C, 500°C, 525°C, 550°C, 575°C, 600°C, 625°C, 650°C, 675°C or any value between 425-675°C or any interval within the above range such as 425-500°C, 500-600°C, 600-700°C, 500-675°C, 525-625°C, etc. The heating rate of the first sintering heating stage can be 2°C / m in, 2.5℃ / min, 3℃ / min, 3.5℃ / min, 4℃ / min or any value between 2-4℃ / min or any interval within the above range, such as 2-3℃ / min, 3-4℃ / min, 2.5-3.5℃ / min, etc. The holding time of the first sintering holding stage can be 6h, 7h, 8h, 9h, 10h or any value between 6-10h or any interval within the above range, such as 6-8h, 8-10h, 7-9h, etc.;
[0144] (12) The second sintering includes a second sintering heating stage and a second sintering heat preservation stage. The temperature in the second sintering heating stage is increased to 875-1025°C. The heating rate in the second sintering heating stage is 20-30°C / min. The heat preservation time in the second sintering heat preservation stage is 6-10h.
[0145] Optionally, the terminal temperature of the second sintering heating stage can be 875℃, 900℃, 925℃, 950℃, 975℃, 1000℃, 1025℃ or any value between 875-1025℃ or any interval within the above range such as 875-975℃, 975-1025℃, 950-1000℃, etc., the heating rate of the second sintering heating stage can be 20℃ / min, 25℃ / min, 30℃ / min or any value between 20-30℃ / min or any interval within the above range such as 20-25℃ / min, 25-30℃ / min, 18-28℃ / min, etc., the insulation time of the second sintering insulation stage can be 6h, 7h, 8h, 9h, 10h or any value between 6-10h or any interval within the above range such as 6-8h, 8-10h, 7-9h, etc.
[0146] The present application also provides a lithium-ion battery, comprising a lithium-rich manganese-based oxide positive electrode material.
[0147] The present application also provides an electrical device, including a lithium-ion battery.
[0148] The embodiments of the present application will be described in detail below in conjunction with specific examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. If specific conditions are not specified in the examples, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0149] Example 1
[0150] This embodiment provides a lithium-rich manganese-based oxide positive electrode material, and the preparation method thereof is as follows:
[0151] 1. Precursor Ni 0.25 Mn 0.75 Preparation of (OH)2
[0152] ①Preparing the solution: dissolving nickel sulfate crystals and manganese sulfate crystals to prepare a manganese-containing metal salt solution with a total metal content of 4 mol / L, and a molar ratio of Ni:Mn of 25:75; preparing ammonia water with a concentration of 16wt% and a sodium hydroxide solution with a concentration of 19.2wt%;
[0153] ② Reaction: Add water, sodium hydroxide solution and ammonia water to the reactor to prepare a bottom liquid, control the pH of the bottom liquid to 11.4-11.8, and the ammonia concentration in the bottom liquid to 5.8-6.2 g / L, raise the temperature to 70°C, and control the feed flow rate of the manganese-containing metal salt solution to 1.0-1.2% / h of the reactor container volume under the stirring action of 600 rpm, and introduce nitrogen at the same time, and control the pH of the coprecipitation reaction process to 10.4-10.6 by sodium hydroxide solution; control the ammonia concentration of the coprecipitation reaction process to 6.2-6.6 g / L by ammonia solution; discharge the mother liquor through the concentration equipment during the coprecipitation reaction, and the discharge rate of the mother liquor is consistent with the total liquid feed rate; until the target particle size D50 is 4.0±0.5 μm, stop the reaction;
[0154] ③ After the synthesis stage, the material is washed with 0.2 mol / L sodium hydroxide solution and deionized water, filtered, and a washed product is obtained;
[0155] ④ Place the washed product in a common drying oven and dry it at 105℃ for 5h to obtain a dry product; after sieving, a spherical or quasi-spherical nickel-manganese hydroxide precursor is obtained. Among them, the primary particles in the secondary particles of the precursor product are plate-shaped, with a D50 of 3.854μm, a Span of 0.62, and a specific surface area of 16.17m 2 / g, tap density is 1.17g / cm 3 .
[0156] The SEM image of the obtained precursor is shown in Figure 1 As shown, Figure 2 for Figure 1 A partial enlarged view of .
[0157] 2. Preparation of cathode materials
[0158] The precursor product prepared above was weighed and moved into a box furnace for the first sintering treatment. The atmosphere was air. The heating rate was 3° C. / min. The temperature was raised to 575° C. and kept at this temperature for 8 h to obtain nickel manganese oxide.
[0159] Nickel manganese oxide and lithium hydroxide were weighed and ground and mixed according to the molar ratio of Li:TM=1.35:1. After the mixture was evenly mixed, the second sintering was performed at a heating rate of 25°C / min to 975°C for 8h in the air atmosphere. After sintering, the lithium-rich manganese-based oxide positive electrode material Li 1.35 Ni 0.25 Mn 0.75 O 2.425 Wherein, TM is the total metal content in the precursor product, the same below.
[0160] The secondary particles of the obtained positive electrode material product include plate-like primary particles and granular primary particles, with a D50 of 3.759 μm. The SEM photo of the positive electrode material product is shown in FIG. Figure 3 shown.
[0161] Example 2
[0162] The difference from Example 1 is that the sintering atmosphere is oxygen. The primary particles of the precursor product are plate-shaped, with a D50 of 3.794 μm, a Span of 0.68, and a specific surface area of 18.67 m 2 / g, tap density is 1.15g / cm 3 .
[0163] The obtained secondary particles of the positive electrode material product include plate-like primary particles and granular primary particles, and D50 is 3.816 μm.
[0164] Example 3
[0165] 1. Precursor Ni 0.2 Mn 0.8 Preparation of (OH)2
[0166] ①Preparing the solution: dissolving nickel sulfate crystals and manganese sulfate crystals to prepare a manganese-containing metal salt solution with a total metal content of 4 mol / L and a molar ratio of Ni:Mn of 2:8; preparing an ammonia solution with a concentration of 16wt% and a sodium hydroxide solution with a concentration of 19.2wt%;
[0167] ② Reaction: Add water, sodium hydroxide solution and ammonia water to the reactor to prepare a bottom liquid, control the pH of the bottom liquid to 11.1-11.4, and the ammonia concentration in the bottom liquid to 6.2-6.6 g / L, raise the temperature to 65°C, and control the feed flow rate of the manganese-containing metal salt solution to 0.8-1.1% / h of the reactor container volume under the stirring action of 580 rpm, and introduce nitrogen at the same time, and control the pH of the coprecipitation reaction process to 10.1-10.2 by sodium hydroxide solution; control the ammonia concentration of the coprecipitation reaction process to 6.6-7.0 g / L by ammonia solution; discharge the mother liquor through the concentration equipment during the coprecipitation reaction, and the discharge rate of the mother liquor is consistent with the total liquid feed rate; until the target particle size D50 is 4.0±0.5 μm, stop the reaction;
[0168] ③ After the synthesis stage, the material is washed with 0.2 mol / L sodium hydroxide solution and deionized water, filtered, and a washed product is obtained;
[0169] ④ Place the washed product in a common drying oven and dry it at 105℃ for 5h to obtain a dry product; after sieving, a spherical or quasi-spherical nickel-manganese hydroxide precursor is obtained. Among them, the primary particles in the secondary particles of the precursor product are plate-shaped, with a D50 of 3.773μm, a Span of 0.68, and a specific surface area of 19.42m 2 / g, tap density is 1.14g / cm 3 .
[0170] 2. Preparation of cathode materials
[0171] The precursor product prepared above was weighed and moved into a box furnace for the first sintering treatment. The atmosphere was air. The heating rate was 4° C. / min. The temperature was raised to 550° C. and kept at this temperature for 9 hours to obtain nickel manganese oxide.
[0172] Nickel manganese oxide and lithium hydroxide were weighed and ground and mixed according to the molar ratio of Li:TM=1.2:1. After the mixture was evenly mixed, the second sintering was performed at a heating rate of 21°C / min to 950°C for 8h in the air atmosphere. After sintering, the lithium-rich manganese-based oxide positive electrode material Li 1.2 Ni 0.2 Mn 0.8 O 2.4 .
[0173] The obtained secondary particles of the positive electrode material product include plate-like primary particles and granular primary particles, and D50 is 3.672 μm.
[0174] Example 4
[0175] 1. Precursor Ni 0.3 Mn 0.7 Preparation of (OH)2
[0176] ①Preparing the solution: dissolving nickel sulfate crystals and manganese sulfate crystals to prepare a manganese-containing metal salt solution with a total metal content of 4 mol / L and a molar ratio of Ni:Mn of 3:7; preparing ammonia water with a concentration of 16wt% and a sodium hydroxide solution with a concentration of 19.2wt%;
[0177] ② Reaction: Add water, sodium hydroxide solution and ammonia water to the reactor to prepare a bottom liquid, control the pH of the bottom liquid to 11.2-11.6, and the ammonia concentration in the bottom liquid to 5.5-6.0 g / L, raise the temperature to 75°C, and control the feed flow rate of the manganese-containing metal salt solution to 1.0-1.2% / h of the reactor container volume under the stirring action of 620 rpm, and introduce nitrogen at the same time, and control the pH of the coprecipitation reaction process to 10.2-10.4 by sodium hydroxide solution; control the ammonia concentration of the coprecipitation reaction process to 5.9-6.3 g / L by ammonia solution; discharge the mother liquor through the concentration equipment during the coprecipitation reaction, and the discharge rate of the mother liquor is consistent with the total liquid feed rate; until the target particle size D50 is 4.0±0.5 μm, stop the reaction;
[0178] ③ After the synthesis stage, the material is washed with 0.2 mol / L sodium hydroxide solution and deionized water, filtered, and a washed product is obtained;
[0179] ④ Place the washed product in a common drying oven and dry it at 105℃ for 5h to obtain a dry product; after sieving, a spherical or quasi-spherical nickel-manganese hydroxide precursor is obtained. Among them, the primary particles in the secondary particles of the precursor product are plate-shaped, with a D50 of 4.118μm, a Span of 0.56, and a specific surface area of 13.26m 2 / g, tap density is 1.17g / cm 3 .
[0180] 2. Preparation of cathode materials
[0181] The precursor product prepared above was weighed and moved into a box furnace for the first sintering treatment. The atmosphere was air. The heating rate was 2° C. / min. The temperature was raised to 600° C. and kept at this temperature for 6 hours to obtain nickel manganese oxide.
[0182] Nickel manganese oxide and lithium hydroxide were weighed and ground and mixed according to the molar ratio of Li:TM=1.4:1. After the mixture was uniformly mixed, a second sintering was performed at a heating rate of 28°C / min to 1000°C for 8h in an air atmosphere. After sintering, a lithium-rich manganese-based oxide positive electrode material Li 1.4 Ni 0.3 Mn 0.7 O 2.4 .
[0183] The obtained secondary particles of the positive electrode material product include plate-like primary particles and granular primary particles, and D50 is 3.976 μm.
[0184] Comparative Example 1
[0185] The difference from Example 1 is:
[0186] The precursor product prepared in Example 1 and lithium hydroxide were ground and mixed according to the molar ratio of Li:TM=1.35:1. After the mixture was evenly mixed, it was moved into a box furnace for sintering. The sintering heating rate was 25°C / min, the sintering temperature was 975°C, the sintering time was 8h, and the sintering atmosphere was air. After sintering, a lithium-rich manganese-based oxide positive electrode material was obtained.
[0187] The secondary particles of the obtained positive electrode material product include plate-like primary particles and granular primary particles, with a D50 of 3.483 μm. The SEM photo of the positive electrode material product is shown in FIG. Figure 4 shown.
[0188] Comparative Example 2
[0189] The difference from Comparative Example 1 is that the sintering atmosphere is oxygen.
[0190] Comparative Example 3
[0191] The difference from Comparative Example 1 is that lithium hydroxide is replaced by lithium carbonate and the sintering atmosphere is oxygen.
[0192] Comparative Example 4
[0193] The difference from Example 1 is that lithium hydroxide is replaced by lithium carbonate; the first sintering temperature is raised to 600° C., and the second sintering temperature is raised to 950° C.
[0194] Comparative Example 5
[0195] The difference from Example 1 is that lithium hydroxide is replaced by lithium carbonate; and the sintering atmosphere is oxygen.
[0196] Comparative Example 6
[0197] The difference from Comparative Example 1 is that the sintering temperature is 850° C. and the sintering atmosphere is oxygen.
[0198] The XRD pattern of the obtained positive electrode material product is as follows: Figure 5 shown.
[0199] Comparative Example 7
[0200] The difference from Comparative Example 1 is that the sintering temperature is 900°C.
[0201] The XRD pattern of the obtained positive electrode material product is as follows: Figure 6 shown.
[0202] The XRD comparison diagrams of the positive electrode materials of each embodiment and comparative example are as follows: Figure 7 (2θ=20°-30°), Figure 8 (2θ = 55°-70° range) and Fig. 9 (2θ is in the range of 35°-40°).
[0203] The XRD test data of the positive electrode materials of the embodiment and the comparative example are shown in Table 1 and Table 2 below:
[0204] Table 1 XRD test data of positive electrode materials of embodiment and comparative example 1
[0205]
[0206] Note: d (A) It is the interplanar spacing of the crystal plane corresponding to the diffraction peak A of the lithium-rich manganese-based oxide positive electrode material in the range of 20.0°-21.0° with a diffraction angle 2θ.
[0207] Table 2 XRD test data of positive electrode materials of embodiment and comparative example 2
[0208]
[0209] The positive electrode materials obtained in Examples 1-2 and Comparative Examples 1-7 were assembled into button cells for electrochemical testing. The assembly method was:
[0210] The slurry was prepared by mixing the cathode material, acetylene black and polyvinylidene fluoride in a ratio of 8:1:1, with N-methylpyrrolidone (NMP) as the solvent. The high voltage electrolyte (LB-111) was purchased from Suzhou Duoduo Chemical Co., Ltd. The battery was assembled using a CR-2032 button cell and electrochemically tested at room temperature using a Neware battery test system at different rates in the range of 3.0-4.5V, 1C=250 mAh / g.
[0211] The electrochemical test results of the embodiments and comparative examples are shown in Table 3:
[0212] Table 3 Electrochemical test data
[0213]
[0214] It can be clearly seen from Table 1, Table 2 and Table 3 that compared with the positive electrode material comparative examples 1-7, the position of the strongest diffraction peak of the lithium-rich manganese-based oxide positive electrode material product prepared in Example 1-2 in the diffraction angle 2θ range of 20.0°-24.5° is slightly shifted to a low angle, and the width of the strongest diffraction peak is significantly larger, and its crystal structure is changed to form a better lithium-rich manganese phase Li2MnO3, which can improve the Li + The migration channel can be better participated in the electrochemical reaction, showing the improvement of capacity performance and cycle performance.
[0215] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present application.
Claims
1. A lithium-rich manganese-based oxide positive electrode material, characterized in that: In the X-ray diffraction pattern of the lithium-rich manganese-based oxide positive electrode material, the diffraction peak in the range of a diffraction angle 2θ of 20.0°-24.5° is a single peak, and the single peak is recorded as diffraction peak A, and the half-peak width FWHM (A) of the diffraction peak A is 0.4°-0.6°; the diffraction angle 2θ corresponding to the peak position of the diffraction peak A of the lithium-rich manganese-based oxide positive electrode material is 20.0°-21.0°; The chemical formula of the lithium-rich manganese-based oxide positive electrode material is Li x Ni y Mn z O 2+δ , among which, 1.1≤x≤1.5, 0.1≤y≤0.4, 0.6≤z≤0.9, 0.15≤δ≤0.
65.
2. The lithium-rich manganese-based oxide positive electrode material according to claim 1, characterized in that: One or more of the following conditions are met: B. The half-peak width FWHM (A) of the diffraction peak A of the lithium-rich manganese-based oxide positive electrode material is 0.4°-0.5°; C. The number of crystal plane sheets N corresponding to the diffraction peak A of the lithium-rich manganese-based oxide positive electrode material (A) 20-70; D. Peak intensity I of diffraction peak A of the lithium-rich manganese-based oxide positive electrode material (A) The peak intensity I of the diffraction peak in the diffraction angle 2θ range of 44.0°-45.0° (104) The ratio I (A) / I (104) 0.07-0.12; E. Peak intensity I of diffraction peak A of the lithium-rich manganese-based oxide positive electrode material (A) The peak intensity I of the diffraction peak in the diffraction angle 2θ range of 18.1°-19.1° (003) The ratio I (A) / I (003) It is 0.07-0.
12.
3. The lithium-rich manganese-based oxide positive electrode material according to claim 1, characterized in that: One or more of the following conditions are met: (1) The lithium-rich manganese-based oxide positive electrode material has at least four diffraction peaks within a diffraction angle 2θ range of 55°-70°, (2) The peak intensity I of the diffraction peak of the lithium-rich manganese-based oxide positive electrode material in the diffraction angle 2θ range of 59.1°-64.5° (018) The peak intensity I of the diffraction peak in the diffraction angle 2θ range of 64.6°-65.2° (110) The ratio I (018) / I (110) 0.9-1.2; (3) The peak position of the diffraction peak of the lithium-rich manganese-based oxide positive electrode material in the diffraction angle 2θ range of 64.6°-65.2° (110) The peak position of the diffraction peak in the range of diffraction angle 2θ of 59.1°-64.5° (018) The difference 2θ (110) -2θ (018) It is 0.7°-0.8°.
4. The lithium-rich manganese-based oxide positive electrode material according to claim 1, characterized in that: One or more of the following conditions are met: (1) The lithium-rich manganese-based oxide positive electrode material has at least three diffraction peaks within a diffraction angle 2θ range of 35°-40°; (2) The grain size D(006) of the crystal plane of the lithium-rich manganese-based oxide positive electrode material corresponding to the diffraction peak in the diffraction angle 2θ range of 37.5°-38.1° is 480-850Å.
5. The lithium-rich manganese-based oxide positive electrode material according to any one of claims 1 to 4, characterized in that: One or more of the following conditions are met: a. The secondary particles of the lithium-rich manganese-based oxide positive electrode material include a plurality of plate-like primary particles; b. The average particle size D50 of the lithium-rich manganese-based oxide positive electrode material is 2-6 μm.
6. The lithium-rich manganese-based oxide positive electrode material according to claim 1, characterized in that: The precursor of the lithium-rich manganese-based oxide positive electrode material meets one or more of the following conditions: (1) The chemical formula of the precursor of the lithium-rich manganese-based oxide positive electrode material is Ni a Mn b (OH)2, 0.5≤b<1, a+b≤1; (2) The average particle size D50 of the precursor of the lithium-rich manganese-based oxide positive electrode material is 2-6 μm; (3) The secondary particles of the precursor of the lithium-rich manganese-based oxide positive electrode material have a Span = (D90-D10) / D50 of 0.5-0.7; (4) The tap density of the lithium-rich manganese-based oxide positive electrode material precursor is 1.1-1.3 g / cm³; (5) The specific surface area of the precursor of the lithium-rich manganese-based oxide positive electrode material is 10-20m 2 / g.
7. A method for preparing the lithium-rich manganese-based oxide positive electrode material according to any one of claims 1 to 5, characterized in that: include: A metal salt solution including a manganese salt and a nickel salt, a precipitant and a complexing agent are introduced into the bottom solution to perform a coprecipitation reaction to obtain a precursor; During the coprecipitation reaction, the mother liquid is discharged, and the discharge rate of the mother liquid is consistent with the total liquid inlet rate; the total metal content in the metal salt solution is 1-8 mol / L; the flow rate of the metal salt solution is 0.5-2.0% / h of the volume of the reaction container; the specific surface area of the precursor is 10-20m 2 / g; The precursor is subjected to a first sintering to obtain nickel manganese oxide; The nickel-manganese oxide is cooled and mixed with a lithium source, and subjected to a second sintering to obtain the lithium-rich manganese-based oxide positive electrode material.
8. The method for preparing a lithium-rich manganese-based oxide positive electrode material according to claim 7, characterized in that: One or more of the following conditions are met: (1) The precipitant includes sodium hydroxide, and the mass fraction of the precipitant is 10-30wt%; (2) The complexing agent includes one or more of ammonia water, ammonium sulfate or ammonium chloride, and the mass fraction of the complexing agent is 10-30wt%; (3) The base liquid includes one or more of water, the precipitant and the complexing agent; (4) The pH value of the base liquid is 10.4-12.8, and the ammonia concentration in the base liquid is 3-8 g / L; (5) The temperature of the coprecipitation reaction is 60-80°C; (6) The pH value during the coprecipitation reaction is 9.4-11.6, and the ammonia concentration during the coprecipitation reaction is 4.2-8.6 g / L; (7) The coprecipitation reaction is carried out under stirring conditions at a stirring speed of 450-800 rpm; (8) After the coprecipitation reaction is completed, the method further comprises: solid-liquid separation, and then washing and drying the solid; (9) The atmospheres of the first sintering and the second sintering are independently air or oxygen atmospheres; (10) The first sintering includes a first sintering heating stage and a first sintering heat preservation stage. The temperature in the first sintering heating stage is raised to 425-675°C. The heating rate in the first sintering heating stage is 2-4°C / min. The heat preservation time in the first sintering heat preservation stage is 6-10h. (11) The second sintering includes a second sintering heating stage and a second sintering keeping stage. The temperature in the second sintering heating stage is raised to 875-1025°C. The heating rate in the second sintering heating stage is 20-30°C / min. The keeping time in the second sintering keeping stage is 6-10h.
9. A lithium ion battery, characterized in that: The invention comprises the lithium-rich manganese-based oxide positive electrode material as described in any one of claims 1 to 5.
10. An electrical equipment, characterized in that: Includes the lithium ion battery as claimed in claim 9.