Amorphous carbon-based composite negative electrode material and preparation method and application thereof

By using amorphous carbon-based composite negative electrode materials in sodium-ion batteries, the low gram capacity and cycle performance of sodium-ion battery negative electrode materials are solved by interweaving bismuth antimony selenide in the carbon skeleton and doping antimony-based particles and metal telluride powder. problem, achieving high energy density and long-life battery performance.

CN118398799BActive Publication Date: 2024-10-11JIANGXI JIANGTONG SIYING NEW ENERGY TECHNOLOGY CO LTD
View PDF 17 Cites 0 Cited by

Patent Information

Application Number
CN202410851615.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-11
Estimated Expiration
2044-06-28

AI Technical Summary

Technical Problem

Existing sodium-ion battery anode materials have low gram capacity, low first efficiency, poor volume expansion and cycle performance, and cannot meet the high energy density and long life requirements of sodium-ion batteries.

Method used

An amorphous carbon-based composite negative electrode material is used. By interweaving bismuth antimony selenide in the carbon skeleton and doping antimony-based particles and metal telluride powder, a composite skeleton is formed to improve structural stability and electrochemical performance.

Benefits of technology

It significantly improves the capacity performance and cycle stability of the anode material, prevents structural damage caused by volume expansion, enhances conductivity and the ability to insert and deintercalate sodium ions, and extends the cycle life of sodium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118398799B_ABST
    Figure CN118398799B_ABST
Patent Text Reader

Abstract

The present invention provides an amorphous carbon-based composite negative electrode material and a preparation method and application thereof, and relates to the technical field of battery negative electrode materials. The amorphous carbon-based composite negative electrode material provided by the present invention comprises a composite skeleton and antimony-based particles formed on the composite skeleton, and metal telluride powder doped in the composite skeleton; the composite skeleton comprises a carbon skeleton and bismuth antimony selenide interwoven in the carbon skeleton. The present invention can improve structural stability and electrical conductivity, thereby improving the electrochemical performance of the negative electrode material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of battery negative electrode materials, and in particular to an amorphous carbon-based composite negative electrode material and a preparation method and application thereof. Background Art

[0002] As the demand for new energy storage is growing explosively, sodium-ion batteries will become one of the best solutions to large-scale energy storage problems. The energy density of sodium-ion batteries is much higher than that of lead-acid batteries. Compared with the currently large-scale lithium-ion batteries, sodium-ion batteries have the advantages of abundant sodium reserves and the ability to use low-concentration electrolytes. They have extremely broad application and development prospects.

[0003] However, the requirements for positive and negative electrodes of sodium-ion batteries and lithium-ion batteries are completely different. The graphite negative electrode material currently widely used in the field of lithium-ion batteries has no sodium storage capacity in sodium-ion batteries. The negative electrode materials for sodium-ion batteries currently under research mainly include carbon-based negative electrode materials, titanium-based negative electrode materials, organic negative electrode materials, and alloy negative electrode materials. However, the above-mentioned types of negative electrode materials all have different defects, such as low gram capacity, low initial efficiency, volume expansion, poor cycle performance, etc. Therefore, it is urgent to provide a solution to improve the above problems. Summary of the invention

[0004] The purpose of the present invention is to provide an amorphous carbon-based composite negative electrode material and a preparation method and application thereof.

[0005] In a first aspect, the amorphous carbon-based composite negative electrode material provided by the present invention comprises a composite skeleton and antimony-based particles formed on the composite skeleton, and metal telluride powder doped in the composite skeleton; the composite skeleton comprises a carbon skeleton and bismuth antimony selenide interwoven in the carbon skeleton.

[0006] The amorphous carbon-based composite negative electrode material provided by the present invention has a carbon skeleton in the composite skeleton as a matrix material that can provide mechanical support and a conductive path, and can improve the overall structural stability of the negative electrode material. At the same time, bismuth antimony selenide is interwoven in the carbon skeleton to form a composite skeleton, which can provide additional conductive paths and improve structural stability. The introduction of selenium and bismuth elements can also promote the embedding and de-embedding of sodium ions in the negative electrode material, and can also stabilize the antimony-based particles and telluride powder, and can further improve the electrochemical performance of the negative electrode material.

[0007] In addition, antimony-based particles as active materials can significantly improve the capacity performance of negative electrode materials. At the same time, metal telluride powder can not only improve the conductivity, but also stabilize the structure of the composite skeleton, prevent structural damage caused by volume expansion and contraction, prevent pulverization of negative electrode materials, and enhance the cycle stability and conductivity of negative electrode materials.

[0008] Optionally, the metal telluride powder includes at least one of zinc telluride, bismuth telluride, lead telluride, antimony telluride, cadmium telluride, and copper telluride, and the average particle size of the metal telluride powder is 1-5 μm.

[0009] In a second aspect, the present invention provides a method for preparing an amorphous carbon-based composite negative electrode material, comprising the steps of stirring and mixing an organic complex with an antimony salt solution to separate a complex precipitate; dispersing the complex precipitate with sodium bismuthate and sodium selenate in anhydrous ethanol and stirring and dispersing the complex precipitate, and then heating and boiling the mixture in an argon atmosphere until the solvent is evaporated to obtain a mixed precipitate; thermally decomposing the mixed precipitate in an inert atmosphere at 500-600°C to obtain a composite skeleton; ultrasonically mixing the composite skeleton in an antimony trichloride solution, evaporating the solvent, and reducing the composite skeleton in a hydrogen atmosphere to generate antimony-based nanoparticles to obtain a composite antimony-based skeleton; and ball-milling and blending the composite antimony-based skeleton with metal telluride powder to obtain an amorphous carbon-based composite negative electrode material.

[0010] The preparation method provided by the present invention helps to evenly disperse antimony ions in the complex and form a uniform complex precipitate by mixing an organic complex with an antimony salt solution and then separating them, thereby improving the uniformity of dispersion of antimony-based particles in the negative electrode material; and heating the complex precipitate, sodium bismuthate and sodium selenate in anhydrous ethanol to boil, which helps to improve the uniformity of dispersion of bismuth salt, selenium salt and the complex precipitate, so that the bismuth salt and selenium salt can be combined with the surface of the complex precipitate, and a carbon skeleton is formed after thermal decomposition, and bismuth antimony selenide is formed in the carbon skeleton to form a composite skeleton; antimony-based nanoparticles generated by reduction in an antimony trichloride solution can be evenly dispersed in the composite skeleton, thereby improving the overall electrochemical activity and capacity of the negative electrode material; when the composite antimony-based skeleton is ball-milled with metal telluride powder, it helps to fully mix and can form good interface contact during the ball-milling process.

[0011] Optionally, in the process of stirring and mixing the organic complex with the antimony salt solution: the organic complex includes at least one of trimesic acid and isophthalic acid.

[0012] Optionally, in the process of stirring and mixing the organic complex with the antimony salt solution: the solute in the antimony salt solution includes at least one of antimony trioxide, antimony nitrate and antimony trichloride.

[0013] Optionally, during the process of stirring and mixing the organic complex and the antimony salt solution, the mass ratio of the organic complex to the antimony ions in the antimony salt solution is 1:(5-10).

[0014] Optionally, during the process of ball-milling and blending the composite antimony-based framework and the metal telluride powder, the mass mixing ratio of the composite antimony-based framework and the metal telluride powder is (70-90): (10-30).

[0015] Optionally, in the process of ball-milling and blending the composite antimony-based framework with metal telluride powder: the metal telluride powder includes at least one of zinc telluride, bismuth telluride, lead telluride, antimony telluride, cadmium telluride, and copper telluride.

[0016] Optionally, during the process of ball-milling and blending the composite antimony-based framework and the metal telluride powder: the average particle size of the metal telluride powder is 1-5 μm.

[0017] Optionally, in the process of dispersing the complex precipitate, sodium bismuthate and sodium selenate in anhydrous ethanol, the mass ratio of the complex precipitate, the sodium bismuthate and the sodium selenate is 1:(0.3-0.5):(0.3-0.5).

[0018] Optionally, during the process of ultrasonically mixing the composite framework in the antimony trichloride solution, the mass ratio of the composite framework to the antimony trichloride in the antimony trichloride solution is 1:(3-5).

[0019] In a third aspect, the present invention also provides the application of amorphous carbon-based composite negative electrode materials in sodium ion batteries. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 A flowchart of a method for preparing an amorphous carbon-based composite negative electrode material provided by the present invention. DETAILED DESCRIPTION

[0021] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Unless otherwise defined, the technical terms or scientific terms used herein should be understood by people with general skills in the field to which the present invention belongs. "Including" and similar words used in this article mean that the elements or objects appearing before the word include the elements or objects listed after the word and their equivalents, without excluding other elements or objects.

[0022] The present invention provides an amorphous carbon-based composite negative electrode material, comprising a composite skeleton and antimony-based particles formed on the composite skeleton, and also comprising metal telluride powder doped in the composite skeleton. In fact, by using antimony-based particles as active materials, since antimony materials can form a reversible alloying reaction with sodium ions during the sodium ion charging and discharging process, the energy density and reversible capacity of the battery can be improved, and the introduction of metal telluride powder can stabilize the structure of the negative electrode material, prevent structural damage caused by volume changes during the charging and discharging process, and improve the cycle stability and conductivity of the negative electrode material.

[0023] Specifically, the composite skeleton includes a carbon skeleton and bismuth antimony selenide interwoven in the carbon skeleton. The carbon skeleton, as the matrix skeleton of the entire negative electrode material, has certain mechanical strength and supporting performance, can prevent the antimony-based particles from falling off, and provide more active sites and doping sites for the growth of antimony-based particles. At the same time, it can also improve the conductivity and structural stability of the negative electrode material, thereby improving the cycle life of the sodium ion battery. The bismuth antimony selenide interwoven in the carbon skeleton can form a composite skeleton with the carbon skeleton, which helps to improve the structural stability and conductivity of the carbon skeleton. At the same time, the introduction of bismuth and selenium elements promotes the embedding and de-embedding of sodium ions.

[0024] In some embodiments, the metal telluride powder includes at least one of zinc telluride, bismuth telluride, lead telluride, antimony telluride, cadmium telluride, and copper telluride, and the average particle size of the metal telluride powder is 1-5 μm. In fact, by using different metal telluride powders to dope in the composite skeleton, different electrochemical properties can be given to the negative electrode material.

[0025] See also Figure 1 The present invention also provides a method for preparing an amorphous carbon-based composite negative electrode material, comprising the following steps:

[0026] S1, stirring and mixing the organic complex and the antimony salt solution to obtain a complex precipitate;

[0027] S2, dispersing the complex precipitate, sodium bismuthate and sodium selenate in anhydrous ethanol, stirring and dispersing, heating and boiling in an argon atmosphere until the solvent is evaporated to obtain a mixed precipitate, and thermally decomposing the mixed precipitate in an inert atmosphere at 500-600° C. to obtain a composite framework;

[0028] S3, ultrasonically mixing the composite framework in an antimony trichloride solution, evaporating the solvent, and reducing the composite framework under a hydrogen atmosphere to generate antimony-based nanoparticles to obtain a composite antimony-based framework;

[0029] S4. The composite antimony-based skeleton and metal telluride powder are ball-milled and mixed to obtain an amorphous carbon-based composite negative electrode material.

[0030] In some embodiments, the organic complex used in step S1 includes at least one of trimesic acid and isophthalic acid. In fact, by using different organic complexes, the antimony salt in the antimony salt solution is complexed to form complex precipitates with different densities, so that the density and surface active sites of the carbon skeleton can be regulated after the carbon skeleton is formed.

[0031] In some embodiments, the solute in the antimony salt solution used in step S1 includes at least one of antimony trioxide, antimony nitrate, and antimony trichloride. In fact, by selecting different solutes in the antimony salt solution, different dissolution amounts can be adjusted, thereby controlling the relative concentration of the organic complex and the solute antimony salt after the organic complex is mixed with the antimony salt solution, thereby facilitating the organic complex to precipitate the antimony salt.

[0032] In some embodiments, when the organic complex and the antimony salt solution are stirred and mixed in step S1, the mixing is controlled to be carried out in a water bath environment at 35-50° C. This is conducive to the complexation precipitation of the organic complex on the antimony salt and can improve the complexation efficiency.

[0033] In some embodiments, after the organic complex and the antimony salt solution are stirred and mixed in step S1, the mass ratio of the organic complex to the antimony ions in the antimony salt solution is 1:(5-10), which is beneficial for regulating the antimony element content in the complex precipitate, thereby controlling the content ratio of antimony element, selenium element and bismuth element in the composite framework, thereby controlling the formation of bismuth antimony selenide.

[0034] In some embodiments, in the process of dispersing the complex precipitate, sodium bismuthate and sodium selenate in anhydrous ethanol in step S2, the mass ratio of the complex precipitate, sodium bismuthate and sodium selenate is 1:(0.3-0.5):(0.3-0.5). In fact, in step S2, the complex precipitate, sodium bismuthate and sodium selenate are mixed and heated to boil until evaporated to dryness, so that the sodium bismuthate and sodium selenate can enter the pores of the complex precipitate and be evenly distributed with the boiling anhydrous ethanol.

[0035] Specifically, in the process of thermally decomposing the mixed precipitate at 500-600° C. in an inert atmosphere in step S2, the inert atmosphere used may be an argon atmosphere or a helium atmosphere. In fact, during the thermal decomposition process, the complex layer in the mixed precipitate is carbonized to form a carbon skeleton, and sodium bismuthate, sodium selenate and antimony salt react and interweave to form bismuth antimony selenide, which is interwoven with the carbon skeleton to form a composite skeleton.

[0036] In some embodiments, during the process of performing step S2, the complex precipitate, sodium bismuthate and sodium selenate are stirred and dispersed in anhydrous ethanol, refluxed for 5-10 hours under an argon atmosphere, and then the anhydrous ethanol is evaporated to obtain a mixed precipitate. In fact, the reflux reaction is conducive to the uniform entry of sodium bismuthate and sodium selenate into the organic complex layer in the complex precipitate.

[0037] In some embodiments, when the composite framework is ultrasonically mixed in the antimony trichloride solution in step S3, the composite framework is put into the antimony trichloride solution, ultrasonically mixed at an ultrasonic power of 150-250 W, and the ultrasonic state is maintained to heat and evaporate the solvent. When the volume of the solvent drops to 1 / 2 of the original volume, the ultrasound is stopped and the heating is continued until the solvent is completely evaporated.

[0038] In some embodiments, in step S3, when reducing antimony-based nanoparticles to produce a composite antimony-based skeleton under a hydrogen atmosphere, the method includes: placing the solid obtained after evaporating the solvent in a ceramic boat, replacing it three times with hydrogen in an atmosphere furnace, heating the solid to 400-450°C at 5°C / min, keeping the temperature for 2-4h and cooling it to room temperature with the furnace to obtain a composite antimony-based skeleton with antimony-based nanoparticles grown on the surface.

[0039] In some embodiments, in the process of ball-milling and blending the composite antimony-based skeleton and the metal telluride powder in step S4, the mass mixing ratio of the composite antimony-based skeleton and the metal telluride powder is (70-90): (10-30). In fact, by regulating the doping amount of the metal telluride powder in the composite antimony-based skeleton, the electrochemical performance of the negative electrode material can be effectively improved. Specifically, the metal telluride powder used includes at least one of zinc telluride, bismuth telluride, lead telluride, antimony telluride, cadmium telluride, and copper telluride, and the average particle size of the metal telluride powder is 1-5 μm.

[0040] The present invention also provides the use of a negative electrode material prepared by any of the above optional preparation methods in a sodium ion battery, wherein the negative electrode material is mixed with a conductive agent and an adhesive, coated on a current collector and dried as a battery negative electrode, and assembled with a battery separator, a battery positive electrode, and an electrolyte to form a sodium ion battery. Example 1

[0041] Embodiment 1 of the present invention provides a method for preparing an amorphous carbon-based composite negative electrode material, comprising the following steps:

[0042] S1. After mixing isophthalic acid and antimony trichloride solution, stirring and reacting at 40° C. for 3 hours, centrifuging and separating the precipitate, and washing the precipitate alternately with deionized water and anhydrous ethanol to obtain a complex precipitate; wherein the mass ratio of isophthalic acid to antimony ions in the antimony trichloride solution is 1:5;

[0043] S2, the complex precipitate, sodium bismuthate and sodium selenate were mixed in a mass ratio of 1:0.4:0.4, put into anhydrous ethanol, stirred and dispersed, heated under reflux for 8 hours in an argon atmosphere, evaporated the solvent to obtain a mixed precipitate, and pyrolyzed the mixed precipitate at 550° C. in an argon atmosphere for 3 hours to obtain a composite skeleton;

[0044] S3, after the composite framework is ultrasonically mixed in the antimony trichloride solution, the solvent is evaporated, and the obtained solid is kept at 430° C. for 3 hours in a hydrogen atmosphere to reduce and generate antimony-based nanoparticles, thereby obtaining a composite antimony-based framework; wherein the mass ratio of the composite framework to the antimony trichloride in the antimony trichloride solution is 1:4;

[0045] S4. After mixing the composite antimony-based skeleton and cadmium telluride powder with an average particle size of 3 μm in a mass ratio of 80:20, zirconium oxide balls were used as ball milling media, and the amorphous carbon-based composite negative electrode material was obtained after ball milling for 8 hours at a ball-to-material ratio of 10:1. Example 2

[0046] Embodiment 2 of the present invention provides a method for preparing an amorphous carbon-based composite negative electrode material, which is different from Embodiment 1 in that the cadmium telluride powder in step S4 is replaced by tin telluride powder.

[0047] Comparative Example 1

[0048] Comparative Example 1 of the present invention provides a method for preparing an amorphous carbon-based composite negative electrode material, which is different from Example 1 in that in step S2, the complex precipitate is directly pyrolyzed in an argon atmosphere at 550° C. for 3 hours to obtain a composite skeleton.

[0049] Comparative Example 2

[0050] Comparative Example 2 of the present invention provides a method for preparing an amorphous carbon-based composite negative electrode material, which is different from Example 1 in that sodium bismuthate is not added in step S2.

[0051] Comparative Example 3

[0052] Comparative Example 3 of the present invention provides a method for preparing an amorphous carbon-based composite negative electrode material, which is different from Example 1 in that sodium selenate is not added in step S2.

[0053] Comparative Example 4

[0054] Comparative Example 4 of the present invention provides a method for preparing an amorphous carbon-based composite negative electrode material, which is different from Example 1 in that, in step S2, the complex precipitate is pyrolyzed at 550°C in an argon atmosphere for 3 hours, mixed with sodium bismuthate and sodium selenate, put into anhydrous ethanol, stirred and dispersed, and heated under reflux for 8 hours in an argon atmosphere, and then the solvent is evaporated to obtain a composite skeleton; wherein the mass ratio of the complex precipitate, sodium bismuthate and sodium selenate is 1:0.4:0.4.

[0055] Comparative Example 5

[0056] Comparative Example 5 of the present invention provides a method for preparing an amorphous carbon-based composite negative electrode material, which is different from Example 1 in that step S3 is not performed.

[0057] Comparative Example 6

[0058] Comparative Example 6 of the present invention provides a method for preparing an amorphous carbon-based composite negative electrode material, which is different from Example 1 in that step S4 is not performed.

[0059] Comparative Example 7

[0060] Comparative Example 7 of the present invention provides a method for preparing an amorphous carbon-based composite negative electrode material, which is different from Example 1 in that steps S3 and S4 are not performed.

[0061] Performance Testing

[0062] The amorphous carbon-based composite negative electrode material prepared in Examples 1 to 2 and Comparative Examples 1 to 7 was used as an active material, mixed with sodium carboxymethyl cellulose and acetylene black in a ratio of 90:5:5, and then coated on a current collector copper foil, vacuum dried and rolled into a composite sheet, which was cut into a circular electrode sheet with a diameter of 10 mm, metallic sodium was used as a counter electrode and a reference electrode, sodium hexafluorophosphate was used as an electrolyte, and assembled into a CR2032 button battery in an argon atmosphere glove box, and the following tests were performed:

[0063] First coulombic efficiency test: at room temperature, discharge at a constant current of 0.1C to 0.01V, then discharge at a constant current of 0.02C to 0.005V, and finally charge at a constant current of 0.1C to 2.0V. The capacity when charged to 2.0V is measured as the first reversible specific capacity, and the first coulombic efficiency is calculated. The results are shown in Table 1.

[0064] Cycle performance test: constant current charge and discharge were performed at room temperature with a current density of 0.1C, the charge and discharge voltage was limited to 0.005-2.0V, and the charge specific capacity after 100 cycles was measured, and the capacity retention rate after 100 cycles was calculated. The results are shown in Table 1.

[0065] Table 1

[0066] ,

[0067] Combining Example 1 and Example 2, and from Table 1, it can be seen that the amorphous carbon-based composite negative electrode material provided by the present invention has high capacity performance and cycle stability, and the capacity can still be maintained at 93-94% after 100 cycles. At the same time, it can also be seen that due to the differences in the properties of different telluride powders, the electrochemical performance of the sodium ion battery will also be different.

[0068] Combining Example 1 and Comparative Example 1, it can be seen that compared with the composite skeleton used in Example 1, the conductivity and structural stability of the carbon skeleton used in Comparative Example 1 are relatively poor. Although the carbon skeleton can also provide some conductivity, its conductivity and stability are insufficient, resulting in the negative electrode material of Comparative Example 1 being more prone to structural collapse and performance degradation during the cycle.

[0069] Combining Example 1 and Comparative Example 2, it can be seen that since a carbon skeleton and antimony selenide are used to form a composite skeleton in Comparative Example 2, the lack of bismuth in the composite skeleton causes a slight decrease in the structural stability and conductivity of the negative electrode material. Although the carbon-antimony selenide skeleton in Comparative Example 2 is slightly improved in structural stability compared to Comparative Example 1, the improvement is not obvious enough, which illustrates the necessity of bismuth in the composite skeleton structure.

[0070] Combining Example 1 and Comparative Example 3, it can be seen that due to the lack of selenium in the skeleton structure of Comparative Example 3, it is difficult to form a bismuth antimony selenide skeleton, and only nano-antimony particles and nano-bismuth particles are formed on the carbon skeleton. Although the addition of nano-bismuth can improve the conductivity of the negative electrode material, the structural stability of the negative electrode material in Comparative Example 3 is weaker than that in Comparative Example 2 due to the failure to form a composite skeleton. However, compared with Comparative Example 1, doping nano-antimony and nano-bismuth in the carbon skeleton can slightly improve the cycle performance.

[0071] Combining Example 1 and Comparative Example 4, it can be seen that in Comparative Example 4, due to the pre-pyrolysis to form a carbon skeleton, although bismuth antimony selenide is formed subsequently, it is difficult to form a composite skeleton similar to that in Example 1. Therefore, the structural stability of the composite skeleton is lacking, resulting in the cycle performance in Comparative Example 4 being weaker than that in Example 1. Compared with Comparative Example 3, although no composite skeleton is formed, bismuth antimony selenide can still slightly improve the first coulombic efficiency, but the cycle performance decreases.

[0072] Combining Example 1 and Comparative Example 5, it can be seen that the negative electrode material in Comparative Example 5 does not generate antimony-based nanoparticles, thereby affecting the capacity performance of the sodium ion battery, and the overall electrochemical performance is still worse than that of Example 1.

[0073] Combining Example 1 and Comparative Example 6, it can be seen that cadmium telluride is not added to the negative electrode material in Comparative Example 6, resulting in a decrease in the electrical conductivity of the negative electrode material. At the same time, due to the lack of cadmium telluride powder, the cycle performance of the sodium ion battery is reduced, which shows that the addition of cadmium telluride powder can also help improve the structural stability of the negative electrode material.

[0074] Combining Example 1 and Comparative Example 7, it can be seen that the negative electrode material in Comparative Example 7 not only does not add cadmium telluride, but also does not generate antimony-based nanoparticles, resulting in the capacity performance and cycle performance of the negative electrode material being worse than those of Comparative Examples 5 and 6.

[0075] Although the embodiments of the present invention are described in detail above, it is obvious to those skilled in the art that various modifications and variations can be made to these embodiments. However, it should be understood that such modifications and variations are within the scope and spirit of the present invention as described in the claims. Moreover, the present invention described herein may have other embodiments and may be implemented or realized in a variety of ways.

Claims

1. An amorphous carbon-based composite negative electrode material, characterized in that: It comprises a composite skeleton, antimony-based particles formed on the composite skeleton, and metal telluride powder doped in the composite skeleton; the composite skeleton comprises a carbon skeleton and bismuth antimony selenide interwoven in the carbon skeleton; wherein the antimony-based nanoparticles are generated by ultrasonically mixing the composite skeleton in an antimony trichloride solution, evaporating the solvent, and then reducing the composite skeleton in a hydrogen atmosphere at 400-450° C. for 2-4 hours; the metal telluride powder comprises at least one of zinc telluride, bismuth telluride, lead telluride, antimony telluride, cadmium telluride, and copper telluride.

2. The amorphous carbon-based composite negative electrode material according to claim 1, characterized in that: The average particle size of the metal telluride powder is 1-5 μm.

3. A method for preparing the amorphous carbon-based composite negative electrode material according to any one of claims 1 to 2, characterized in that: The following steps are involved: The organic complex is mixed with the antimony salt solution by stirring, and a complex precipitate is obtained by separation; The complex precipitate, sodium bismuthate and sodium selenate are dispersed in anhydrous ethanol and stirred, and then heated and boiled in an argon atmosphere until the solvent is evaporated to obtain a mixed precipitate; The mixed precipitate is thermally decomposed at 500-600° C. in an inert atmosphere to obtain a composite skeleton; The composite framework is ultrasonically mixed in an antimony trichloride solution, the solvent is evaporated, and then reduced in a hydrogen atmosphere at 400-450° C. to generate antimony-based nanoparticles to obtain a composite antimony-based framework; The amorphous carbon-based composite negative electrode material is prepared by ball-milling and blending the composite antimony-based skeleton and metal telluride powder.

4. The preparation method according to claim 3, characterized in that: During the stirring and mixing of the organic complex and the antimony salt solution: The organic complex comprises at least one of trimesic acid and isophthalic acid; And / or, the solute in the antimony salt solution includes at least one of antimony nitrate and antimony trichloride.

5. The preparation method according to claim 3, characterized in that: The mass ratio of the organic complex to the antimony ions in the antimony salt solution is 1:(5-10).

6. The preparation method according to claim 3, characterized in that: During the process of ball milling and blending the composite antimony-based framework and the metal telluride powder, the mass mixing ratio of the composite antimony-based framework and the metal telluride powder is (70-90): (10-30).

7. The preparation method according to claim 3, characterized in that: The average particle size of the metal telluride powder is 1-5 μm.

8. The preparation method according to claim 3, characterized in that: In the process of dispersing the complex precipitate, sodium bismuthate and sodium selenate in anhydrous ethanol, the mass ratio of the complex precipitate, the sodium bismuthate and the sodium selenate is 1:(0.3-0.5):(0.3-0.5).

9. The preparation method according to claim 3, characterized in that: During the process of ultrasonically mixing the composite framework in the antimony trichloride solution, the mass ratio of the composite framework to the antimony trichloride in the antimony trichloride solution is 1:(3-5).

10. Use of an amorphous carbon-based composite negative electrode material prepared by the preparation method according to any one of claims 3 to 9 in a sodium ion battery.

Citation Information

Patent Citations

  • Preparation method of composite material of carbon nanotube loaded with Bi2Te3 nanosphere

    CN101746713A

  • Novel lithium ion battery electrode material and application of lithium ion battery electrode material

    CN103872293A

  • Novel electrode material of sodium-ion battery and application of electrode material

    CN105185958A

  • Lithium secondary battery anode material based on atomic hybridization chalcogen solid solution TexSeySz, and preparation method

    CN109616634A

  • Preparation method of sodium-ion battery cathode material

    CN109921002A