A positive electrode sodium supplement and its preparation method and application
By using NaNi1/3Mn1/3Fe1/3O2@NaMnBO3 cathode sodium supplementation agent, the problems of sodium ion loss and gas release in sodium-ion batteries are solved, high electrochemical stability and cycle stability are achieved, and it is suitable for commercial applications.
Patent Information
- Application Number
- CN202410855044.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-06-28
AI Technical Summary
In existing sodium-ion batteries, the loss of sodium ions and the irreversible slippage of the transition metal layer in the cathode material during charging lead to low battery capacity, and organic and inorganic additives generate gas during the electrochemical oxidation and decomposition process, hindering commercial application.
NaNi1/3Mn1/3Fe1/3O2@NaMnBO3 is used as the cathode sodium supplement. It is prepared by mixing sodium source, manganese source and boron source in absolute ethanol, adding citric acid, evaporating to dryness and sintering to form a structure with stable structure and low gas content. Sodium supplement with releasing properties.
The sodium supplementing agent does not produce a large amount of gas during the electrochemical oxidation and decomposition process, improves sodium utilization and electrochemical stability, enhances the cycle stability and discharge specific capacity of the battery, and is suitable for industrial production.
Smart Images

Figure CN118398800B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of battery materials, and in particular to a positive electrode sodium supplement and a preparation method and application thereof. Background Art
[0002] In the sodium-ion battery system, the positive electrode material plays a key role in improving the energy density. Layered transition metal oxides have become one of the most commercially valuable positive electrode materials due to their simple synthesis methods and high theoretical capacity. The P2-type nickel-manganese-based positive electrode materials that have been studied more have the advantages of high voltage and high energy density. However, the sodium ions released from the positive electrode during the first cycle of charging will react at the negative electrode to form an SEI film or other side reactions, resulting in the loss of active sodium ions. In this way, when the sodium-ion battery is discharged, the same amount of sodium ions cannot be released from the negative electrode to return to the positive electrode, and the performance of the material cannot be fully exerted, resulting in a low battery capacity. Moreover, in the highly de-sodiumized state, the irreversible slip of the transition metal layer and the highly activated lattice oxygen will cause great damage to the electrochemical properties of Ni / Mn-based oxides.
[0003] The above problems can be solved by supplementing sodium to sodium ion batteries. For example, patent CN110165218A discloses the application of a positive electrode sodium supplement in sodium ion batteries. x O y N z , positive electrode material, conductive agent and binder are added to solvent and mixed into a slurry, then coated on the surface of the current collector and dried in vacuum; Patent CN110112475A discloses a positive electrode material for a sodium ion battery containing a sodium supplement additive, wherein the sodium supplement additive Na2(CO) m and Na2C n O n+2 , positive electrode active material, conductive agent and binder are mixed evenly in a solvent and then coated on the current collector. However, in addition to releasing sodium ions, almost all organic additives and some inorganic additives will produce gas during the electrochemical oxidation decomposition process, resulting in an increase in the internal pressure of the battery. This requires additional processing steps to remove the gas during the battery assembly process, which hinders commercial applications. Therefore, it remains a challenge to develop new positive electrode sodium supplement additives that are environmentally friendly, have high sodium utilization, suitable decomposition voltage and low gas release. Summary of the invention
[0004] In order to overcome the problem of instability of the sodium supplement, the present invention provides a positive electrode sodium supplement and a preparation method and application thereof, the sodium supplement NaNi 1 / 3 Mn 1 / 3 Fe 1 / 3 O2@NaMnBO3 has excellent structural stability and electron transfer properties, and does not produce a large amount of gas during electrochemical oxidation and decomposition.
[0005] In order to achieve the above object, the present invention adopts the following technical solutions:
[0006] A positive electrode sodium supplement, the structural formula is NaNi 1 / 3 Mn 1 / 3 Fe 1 / 3 O2@NaMnBO3.
[0007] As a preferred coating amount of NaMnBO3 is NaNi 1 / 3 Mn 1 / 3 Fe 1 / 3 10-20% of the mass of O2.
[0008] Preferably, NaNi 1 / 3 Mn 1 / 3 Fe 1 / 3 The particle size of O2@NaMnBO3 is 5-8 μm.
[0009] The present invention also provides a method for preparing the positive electrode sodium supplement, comprising the following steps:
[0010] (1) Mix a sodium source, a manganese source and a boron source, disperse them in anhydrous ethanol, add citric acid, and continue to disperse them evenly to obtain a dispersion;
[0011] (2) Add NaNi to the dispersion prepared in step (1) 1 / 3 Mn 1 / 3 Fe 1 / 3 O2, disperse evenly, evaporate the solvent to obtain a solid;
[0012] (3) Sintering the solid obtained in step (2) at 400-800 °C for 20-24 h under inert gas to obtain the positive electrode sodium supplement NaNi 1 / 3 Mn 1 / 3 Fe 1 / 3 O2@NaMnBO3.
[0013] Preferably, in step (1), the sodium source is one or more of sodium carbonate, sodium acetate, and sodium oxalate; the manganese source is one or more of manganese acetate, manganese oxalate, manganese carbonate, and manganese tetraoxide; and the boron source is boric acid or boron trioxide.
[0014] Preferably, in step (1), the sodium source, manganese source and boron source are mixed in a molar ratio of (1-1.1):1:1.
[0015] Preferably, the mass of citric acid in step (1) is 25-40% of the total mass of the sodium source, the manganese source and the boron source.
[0016] Preferably, the dispersion in step (1) is carried out by stirring at a speed of 400-600 rpm for 1-3 h, and the continued dispersion is carried out by stirring at a speed of 400-600 rpm for 30-60 min; and the dispersion in step (2) is carried out by stirring at a speed of 400-600 rpm for 1-3 h.
[0017] The present invention also provides the application of the positive electrode sodium supplement agent, wherein NaNi 1 / 3 Mn 1 / 3 Fe 1 / 3 O2@NaMnBO3 and P2 phase positive electrode material are uniformly mixed in a molar ratio of 1:(8-10) to obtain active material.
[0018] Preferably, NaNi 1 / 3 Mn 1 / 3 Fe 1 / 3 O2@NaMnBO3 was ball-milled before mixing to prevent agglomeration.
[0019] Preferably, the active material is assembled into a button cell. Specifically, the active material (80 wt%) is mixed with acetylene black (AB, 10 wt%) and polyvinylidene fluoride (PVDF, 10 wt%) in N-methylpyrrolidone (NMP) to form a slurry. Then, the slurry is coated on an aluminum foil. The pole piece is dried in a vacuum drying oven at 80 °C for 12 h, and assembled into a battery in a glove box in the order of negative electrode shell-spring-gasket-negative electrode (sodium sheet)-electrolyte-diaphragm-electrolyte-positive electrode-positive electrode shell.
[0020] Preferably, the active materials are assembled into a full battery, specifically, the sodium sheet of the negative electrode in the above-mentioned button battery assembly process is replaced with the corresponding hard carbon, which will not be described in detail here.
[0021] Therefore, the beneficial effects of the present invention are as follows: (1) NaMnBO3 has a tetrahedral open framework structure, and the hexagonal phase is composed of MnO5 tetrahedral pyramids. On the BO3 plane, the BO3 unit connects the MnO5 tetrahedral pyramids along the c axis, so the material itself has structural stability and excellent electron transfer performance. It sacrifices itself at high potential and produces Na by electro-oxidation decomposition. + , compensate for the sodium consumption caused by the formation of the positive and negative electrode interface film, and reduce Na + loss.
[0022] (2) BO3 3−The polyanion group has the advantages of high thermal stability, high crustal abundance and low environmental impact. The small volume change during the charge and discharge cycle enhances the electrochemical stability. It is well known that the surface oxygen function in the material is crucial to achieve high electrochemical stability, because the surface oxygen function will have a negative impact on the conductivity of the positive electrode material. These surface oxygen groups will have unnecessary side reactions with the electrolyte, thereby affecting its electrochemical stability in the high potential window. Due to the inductive effect of the boron-oxygen covalent bond and the presence of low surface oxygen function, the compound exhibits very excellent structural stability and does not produce a large amount of gas during the reaction.
[0023] (3) NaNi 1 / 3 Mn 1 / 3 Fe 1 / 3 O2 itself can be used as a positive electrode material, which has the characteristics of no gas production or little gas production.
[0024] (4) In addition to the sodium supplementation function, the compound can also improve the discharge specific capacity to a certain extent. The sodium supplement has a simple use process and is cheap, making it very suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 Example 1 NaNi 1 / 3 Mn 1 / 3 Fe 1 / 3 SEM image of O2@NaMnBO3;
[0026] Figure 2 is the first cycle charge and discharge curve of the button battery in Example 1;
[0027] Figure 3 It is a 50-cycle life test chart of the full battery of each embodiment and comparative example. DETAILED DESCRIPTION
[0028] The technical solution of the present invention is further described below through specific embodiments.
[0029] In the present invention, unless otherwise specified, the raw materials and equipment used can be purchased from the market or are commonly used in the art. The methods in the embodiments, unless otherwise specified, are all conventional methods in the art. Unless otherwise specified, parts are by weight, temperatures are expressed in ° C or at ambient temperature, and pressures are atmospheric pressure or near atmospheric pressure. There are many variations and combinations of reaction conditions (such as component concentrations, desired solvents, solvent mixtures, temperatures, pressures, and other reaction ranges) and conditions that can be used to optimize the purity and yield of the product obtained by the method, and only reasonable routine experiments will be required to optimize such method conditions.
[0030] A positive electrode sodium supplement, the structural formula is NaNi 1 / 3Mn 1 / 3 Fe 1 / 3 O2@NaMnBO3, particle size is 5-8 μm; the coating amount of NaMnBO3 is NaNi 1 / 3 Mn 1 / 3 Fe 1 / 3 10-20% of the mass of O2.
[0031] The preparation method of the above-mentioned positive electrode sodium supplement comprises the following steps:
[0032] (1) Mix the sodium source, manganese source and boron source in a ratio of sodium, manganese and boron (1-1.1):1:1, add to anhydrous ethanol, and stir at 400-600 rpm for 1-3 h; then add citric acid in an amount of 25-40% of the sum of the mass of the sodium source, manganese source and boron source, and continue stirring at 400-600 rpm for 30-60 min to obtain a dispersion. The sodium source is one or more of sodium carbonate, sodium acetate and sodium oxalate; the manganese source is one or more of manganese acetate, manganese oxalate, manganese carbonate and manganese tetraoxide; the boron source is boric acid or boron trioxide.
[0033] (2) Add NaNi to the dispersion prepared in step (1) 1 / 3 Mn 1 / 3 Fe 1 / 3 O2, stirring at 400-600 rpm for 1-3 h, evaporating the solvent to obtain a solid;
[0034] (3) Sintering the solid obtained in step (2) at 400-800 °C for 20-24 h under an inert gas atmosphere to obtain a positive electrode sodium supplement NaNi 1 / 3 Mn 1 / 3 Fe 1 / 3 O2@NaMnBO3.
[0035] The above-mentioned positive electrode sodium supplement is used for active materials, specifically: NaNi 1 / 3 Mn 1 / 3 Fe 1 / 3 After ball milling, O2@NaMnBO3 powder is uniformly mixed with P2 phase positive electrode material in a drying room at a molar ratio of 1:(8-10) to obtain active material.
[0036] The above active materials were assembled into button cells. Specifically, the active material (80 wt%) was mixed with acetylene black (AB, 10 wt%) and polyvinylidene fluoride (PVDF, 10 wt%) in N-methylpyrrolidone (NMP) to form a slurry. Then, the slurry was coated on aluminum foil. The electrode was dried in a vacuum drying oven at 80 °C for 12 h, and assembled into a button cell in a glove box in the order of negative electrode shell-spring-gasket-negative electrode (sodium sheet)-electrolyte-diaphragm-electrolyte-positive electrode-positive electrode shell.
[0037] The above active materials were assembled into a full battery. Specifically, the active material (80 wt%) was mixed with acetylene black (AB, 10 wt%) and polyvinylidene fluoride (PVDF, 10 wt%) in N-methylpyrrolidone (NMP) to form a slurry. Then, the slurry was coated on aluminum foil. The pole piece was dried in a vacuum drying oven at 80 °C for 12 h, and assembled into a full battery in a glove box in the order of negative electrode shell-spring-gasket-negative electrode (hard carbon)-electrolyte-diaphragm-electrolyte-positive electrode-positive electrode shell.
[0038] Example 1
[0039] A positive electrode sodium supplement, the structural formula is NaNi 1 / 3 Mn 1 / 3 Fe 1 / 3 O2@NaMnBO3, coating amount is 15%.
[0040] The preparation method of the above-mentioned positive electrode sodium supplement agent is:
[0041] Step 1. Sodium carbonate, manganese acetate and boric acid were first mixed in a molar ratio of 0.54:1:1, added to 100 mL of anhydrous ethanol, and magnetically stirred at 500 rpm for 2 h. Then, 25% citric acid was added, which was the sum of the mass of the sodium source, the manganese source and the boron source, and stirring was continued for 30 min.
[0042] Step 2. Add NaNi according to the coating amount of 15% 1 / 3 Mn 1 / 3 Fe 1 / 3 The O2 positive electrode material was stirred for 1 h and then evaporated to dryness in an oil bath at 80 °C;
[0043] Step 3. Sinter it at 700 °C in an inert atmosphere for 24 h to obtain NaNi 1 / 3 Mn 1 / 3 Fe 1 / 3 O2@NaMnBO3.
[0044] The prepared NaNi 1 / 3 Mn 1 / 3 Fe 1 / 3 O2@NaMnBO3 was characterized for performance, SEM images are shown in Figure 1 As shown in the figure, it can be seen that the coated material still maintains the secondary spherical structure of the core material, and there is an obvious coating layer on the surface, which proves the successful coating of NaMnBO3, and the particle size is 5 μm.
[0045] The above-mentioned positive electrode sodium supplement is used for active materials, specifically: NaNi 1 / 3 Mn 1 / 3 Fe 1 / 3The O2@NaMnBO3 powder was ball-milled for 8 h. After being fully ground, it was uniformly mixed with the P2 phase positive electrode material in a drying room at a molar ratio of 1:9 to obtain the active material.
[0046] The above active materials were assembled into button cells. Specifically, the active material (80 wt%) was mixed with acetylene black (AB, 10 wt%) and polyvinylidene fluoride (PVDF, 10 wt%) in N-methylpyrrolidone (NMP) to form a slurry. Then, the slurry was coated on aluminum foil. The electrode was dried in a vacuum drying oven at 80 °C for 12 h, and assembled into a button cell in a glove box in the order of negative electrode shell-spring-gasket-negative electrode (sodium sheet)-electrolyte-diaphragm-electrolyte-positive electrode-positive electrode shell.
[0047] The first cycle charge and discharge curve of the button battery test was obtained under 2-4V, 0.1C conditions. The results are as follows Figure 2 As shown in the figure, it can be seen that the first effect is 66.47%, which is suitable as a sodium supplement material.
[0048] The above active materials were assembled into a full battery. Specifically, the active material (80 wt%) was mixed with acetylene black (AB, 10 wt%) and polyvinylidene fluoride (PVDF, 10 wt%) in N-methylpyrrolidone (NMP) to form a slurry. Then, the slurry was coated on aluminum foil. The pole piece was dried in a vacuum drying oven at 80 °C for 12 h, and assembled into a full battery in a glove box in the order of negative electrode shell-spring-gasket-negative electrode (hard carbon)-electrolyte-diaphragm-electrolyte-positive electrode-positive electrode shell.
[0049] Example 2
[0050] A positive electrode sodium supplement, the structural formula is NaNi 1 / 3 Mn 1 / 3 Fe 1 / 3 O2@NaMnBO3, coating amount is 10%.
[0051] The preparation method of the above-mentioned positive electrode sodium supplement agent is:
[0052] Step 1: First, mix sodium carbonate, manganese acetate and boric acid in a molar ratio of 0.5:1:1, add to 100 mL of anhydrous ethanol, and stir magnetically at 600 rpm for 1 h. Then, add 30% citric acid with a mass equal to the sum of the mass of the sodium source, manganese source and boron source, and continue stirring for 30 min.
[0053] Step 2: Add NaNi according to the coating amount of 10% 1 / 3 Mn 1 / 3 Fe 1 / 3 The O2 positive electrode material was stirred for 1 h and then evaporated to dryness in an oil bath at 80 °C.
[0054] Step 3: Sinter it at 400℃ in an inert atmosphere for 20h to obtain NaNi 1 / 3 Mn 1 / 3 Fe 1 / 3 O2@NaMnBO3.
[0055] The above-mentioned positive electrode sodium supplement is used for active materials, specifically: NaNi 1 / 3 Mn 1 / 3 Fe 1 / 3 The O2@NaMnBO3 powder was ball-milled for 8 h. After being fully ground, it was uniformly mixed with the P2 phase positive electrode material in a drying room at a molar ratio of 1:8 to obtain the active material.
[0056] The above active materials were assembled into a full battery, specifically: the active material (80 wt%) was mixed with acetylene black (AB, 10 wt%) and polyvinylidene fluoride (PVDF, 10 wt%) in N-methylpyrrolidone (NMP) to form a slurry. Then, the slurry was coated on aluminum foil. The pole piece was dried in a vacuum drying oven at 80 °C for 12 h, and assembled into a full battery in a glove box in the order of negative electrode shell-spring-gasket-negative electrode (hard carbon)-electrolyte-diaphragm-electrolyte-positive electrode-positive electrode shell.
[0057] Example 3
[0058] A positive electrode sodium supplement, the structural formula is NaNi 1 / 3 Mn 1 / 3 Fe 1 / 3 O2@NaMnBO3, coating amount is 20%.
[0059] The preparation method of the above-mentioned positive electrode sodium supplement agent is:
[0060] Step 1: First, mix sodium carbonate, manganese acetate and boric acid in a molar ratio of 0.55:1:1, add to 200 mL of anhydrous ethanol, and stir magnetically at 400 rpm for 3 h. Then, add 40% citric acid with a mass equal to the sum of the mass of the sodium source, manganese source and boron source, and continue stirring for 60 min.
[0061] Step 2: Add NaNi according to the coating amount of 20% 1 / 3 Mn 1 / 3 Fe 1 / 3 The O2 positive electrode material was stirred for 3 h and then evaporated to dryness in an oil bath at 120 °C.
[0062] Step 3: Sinter it at 800 °C in an inert atmosphere for 24 h to obtain NaNi 1 / 3 Mn 1 / 3 Fe 1 / 3 O2@NaMnBO3.
[0063] The above-mentioned positive electrode sodium supplement is used for active materials, specifically: NaNi 1 / 3 Mn 1 / 3 Fe 1 / 3 The O2@NaMnBO3 powder was ball-milled for 8 h. After being fully ground, it was uniformly mixed with the P2 phase positive electrode material in a drying room at a molar ratio of 1:10 to obtain the active material.
[0064] The above active materials were assembled into a full battery, specifically: the active material (80 wt%) was mixed with acetylene black (AB, 10 wt%) and polyvinylidene fluoride (PVDF, 10 wt%) in N-methylpyrrolidone (NMP) to form a slurry. Then, the slurry was coated on aluminum foil. The pole piece was dried in a vacuum drying oven at 80 °C for 12 h, and assembled into a full battery in a glove box in the order of negative electrode shell-spring-gasket-negative electrode (hard carbon)-electrolyte-diaphragm-electrolyte-positive electrode-positive electrode shell.
[0065] Example 4
[0066] A positive electrode sodium supplement, the structural formula is NaNi 1 / 3 Mn 1 / 3 Fe 1 / 3 O2@NaMnBO3, the coating amount is 12%.
[0067] The preparation method of the above-mentioned positive electrode sodium supplement agent is:
[0068] Step 1: First, mix sodium carbonate, manganese acetate and boric acid in a molar ratio of 0.51:1:1, add to 100 mL of anhydrous ethanol, stir magnetically at 450 rpm for 1.5 h, then add 28% citric acid (the sum of the mass of the sodium source, manganese source and boron source), and continue stirring for 40 min.
[0069] Step 2: Add NaNi according to the coating amount of 12% 1 / 3 Mn 1 / 3 Fe 1 / 3 The O2 positive electrode material was stirred for 1.5 h and then evaporated to dryness in an oil bath at 80 °C.
[0070] Step 3: Sinter it at 500 °C in an inert atmosphere for 22 h to obtain NaNi 1 / 3 Mn 1 / 3 Fe 1 / 3 O2@NaMnBO3.
[0071] The above-mentioned positive electrode sodium supplement is used for active materials, specifically: NaNi 1 / 3 Mn 1 / 3 Fe 1 / 3The O2@NaMnBO3 powder was ball-milled for 8 h. After being fully ground, it was uniformly mixed with the P2 phase positive electrode material in a drying room at a molar ratio of 1:8.5 to obtain the active material.
[0072] The above active materials were assembled into a full battery, specifically: the active material (80 wt%) was mixed with acetylene black (AB, 10 wt%) and polyvinylidene fluoride (PVDF, 10 wt%) in N-methylpyrrolidone (NMP) to form a slurry. Then, the slurry was coated on aluminum foil. The pole piece was dried in a vacuum drying oven at 80 °C for 12 h, and assembled into a full battery in a glove box in the order of negative electrode shell-spring-gasket-negative electrode (hard carbon)-electrolyte-diaphragm-electrolyte-positive electrode-positive electrode shell.
[0073] Example 5
[0074] A positive electrode sodium supplement, the structural formula is NaNi 1 / 3 Mn 1 / 3 Fe 1 / 3 O2@NaMnBO3, the coating amount is 14%.
[0075] The preparation method of the above-mentioned positive electrode sodium supplement agent is:
[0076] Step 1: First, sodium carbonate, manganese acetate and boric acid were mixed in a molar ratio of 0.52:1:1, added to 100 mL of anhydrous ethanol, and magnetically stirred at 520 rpm for 1.3 h. Then, 33% citric acid was added, which was the sum of the mass of the sodium source, manganese source and boron source, and stirring was continued for 35 min.
[0077] Step 2: Add NaNi according to the coating amount of 14% 1 / 3 Mn 1 / 3 Fe 1 / 3 The O2 positive electrode material was stirred for 1 h and then evaporated to dryness in an oil bath at 80 °C.
[0078] Step 3: Sinter it at 700 °C in an inert atmosphere for 21 h to obtain NaNi 1 / 3 Mn 1 / 3 Fe 1 / 3 O2@NaMnBO3.
[0079] The above-mentioned positive electrode sodium supplement is used for active materials, specifically: NaNi 1 / 3 Mn 1 / 3 Fe 1 / 3 The O2@NaMnBO3 powder was ball-milled for 8 h. After being fully ground, it was uniformly mixed with the P2 phase positive electrode material in a drying room at a molar ratio of 1:8 to obtain the active material.
[0080] The above active materials were assembled into a full battery, specifically: the active material (80 wt%) was mixed with acetylene black (AB, 10 wt%) and polyvinylidene fluoride (PVDF, 10 wt%) in N-methylpyrrolidone (NMP) to form a slurry. Then, the slurry was coated on aluminum foil. The pole piece was dried in a vacuum drying oven at 80 °C for 12 h, and assembled into a full battery in a glove box in the order of negative electrode shell-spring-gasket-negative electrode (hard carbon)-electrolyte-diaphragm-electrolyte-positive electrode-positive electrode shell.
[0081] Example 6
[0082] A positive electrode sodium supplement, the structural formula is NaNi 1 / 3 Mn 1 / 3 Fe 1 / 3 O2@NaMnBO3, the coating amount is 18%.
[0083] The preparation method of the above-mentioned positive electrode sodium supplement agent is:
[0084] Step 1: First, mix sodium carbonate, manganese acetate and boric acid in a molar ratio of 0.53:1:1, add to 100 mL of anhydrous ethanol, and stir magnetically at 550 rpm for 2.5 h. Then, add 35% citric acid, which is the sum of the mass of the sodium source, manganese source and boron source, and continue stirring for 50 min.
[0085] Step 2: Add NaNi according to the coating amount of 18% 1 / 3 Mn 1 / 3 Fe 1 / 3 The O2 positive electrode material was stirred for 1 h and then evaporated to dryness in an oil bath at 80 °C.
[0086] Step 3: Sinter it at 500 °C in an inert atmosphere for 23 h to obtain NaNi 1 / 3 Mn 1 / 3 Fe 1 / 3 O2@NaMnBO3.
[0087] The above-mentioned positive electrode sodium supplement is used for active materials, specifically: NaNi 1 / 3 Mn 1 / 3 Fe 1 / 3 The O2@NaMnBO3 powder was ball-milled for 8 h. After being fully ground, it was uniformly mixed with the P2 phase positive electrode material in a drying room at a molar ratio of 1:8 to obtain the active material.
[0088] The above active materials were assembled into a full battery, specifically: the active material (80 wt%) was mixed with acetylene black (AB, 10 wt%) and polyvinylidene fluoride (PVDF, 10 wt%) in N-methylpyrrolidone (NMP) to form a slurry. Then, the slurry was coated on aluminum foil. The pole piece was dried in a vacuum drying oven at 80 °C for 12 h, and assembled into a full battery in a glove box in the order of negative electrode shell-spring-gasket-negative electrode (hard carbon)-electrolyte-diaphragm-electrolyte-positive electrode-positive electrode shell.
[0089] Comparative Example 1
[0090] The difference from Example 1 is that no positive electrode sodium supplement is added to the active material.
[0091] The P2 phase cathode material (80 wt%) was mixed with acetylene black (AB, 10 wt%) and polyvinylidene fluoride (PVDF, 10 wt%) in N-methylpyrrolidone (NMP) to form a slurry. Then, the slurry was coated on aluminum foil. The electrode was dried in a vacuum oven at 80 °C for 12 h and assembled into a full battery in a glove box in the order of anode shell-spring-gasket-anode (hard carbon)-electrolyte-diaphragm-electrolyte-cathode-cathode shell.
[0092] Comparative Example 2
[0093] The difference from Example 1 is that the structural formula of the sodium supplement is NaNi 1 / 3 Mn 1 / 3 Fe 1 / 3 O2@NaFeBO3.
[0094] NaNi 1 / 3 Mn 1 / 3 Fe 1 / 3 The O2@NaFeBO3 powder was ball-milled for 8 h. After being fully ground, it was uniformly mixed with the P2 phase positive electrode material in a drying room at a molar ratio of 1:9 to obtain the active material.
[0095] The above active materials were assembled into a full battery, specifically: the active material (80 wt%) was mixed with acetylene black (AB, 10 wt%) and polyvinylidene fluoride (PVDF, 10 wt%) in N-methylpyrrolidone (NMP) to form a slurry. Then, the slurry was coated on aluminum foil. The pole piece was dried in a vacuum drying oven at 80 °C for 12 h, and assembled into a full battery in a glove box in the order of negative electrode shell-spring-gasket-negative electrode (hard carbon)-electrolyte-diaphragm-electrolyte-positive electrode-positive electrode shell.
[0096] Comparative Example 3
[0097] The difference from Example 1 is that the coating amount is 8%.
[0098] A positive electrode sodium supplement, the structural formula is NaNi 1 / 3 Mn 1 / 3 Fe 1 / 3 O2@NaMnBO3, coating amount is 8%.
[0099] The preparation method of the above-mentioned positive electrode sodium supplement agent is:
[0100] Step 1. Sodium carbonate, manganese acetate and boric acid were first mixed in a molar ratio of 0.54:1:1, added to 100 mL of anhydrous ethanol, and magnetically stirred at 500 rpm for 2 h. Then, 25% citric acid was added, which was the sum of the mass of the sodium source, the manganese source and the boron source, and stirring was continued for 30 min.
[0101] Step 2. Add NaNi according to the coating amount of 8% 1 / 3 Mn 1 / 3 Fe 1 / 3 O2 cathode material, stirred for 1 h and evaporated to dryness in an oil bath at 80 °C;
[0102] Step 3. Sinter it at 700 °C in an inert atmosphere for 24 h to obtain NaNi 1 / 3 Mn 1 / 3 Fe 1 / 3 O2@NaMnBO3.
[0103] The above-mentioned positive electrode sodium supplement is used for active materials, specifically: NaNi 1 / 3 Mn 1 / 3 Fe 1 / 3 The O2@NaMnBO3 powder was ball-milled for 8 h. After being fully ground, it was uniformly mixed with the P2 phase positive electrode material in a drying room at a molar ratio of 1:9 to obtain the active material.
[0104] The above active materials were assembled into a full battery. Specifically, the active material (80 wt%) was mixed with acetylene black (AB, 10 wt%) and polyvinylidene fluoride (PVDF, 10 wt%) in N-methylpyrrolidone (NMP) to form a slurry. Then, the slurry was coated on aluminum foil. The pole piece was dried in a vacuum drying oven at 80 °C for 12 h, and assembled into a full battery in a glove box in the order of negative electrode shell-spring-gasket-negative electrode (hard carbon)-electrolyte-diaphragm-electrolyte-positive electrode-positive electrode shell.
[0105] Comparative Example 4
[0106] The difference from Example 1 is that the coating amount is 23%.
[0107] A positive electrode sodium supplement, the structural formula is NaNi 1 / 3 Mn 1 / 3 Fe 1 / 3O2@NaMnBO3, the coating amount is 23%.
[0108] The preparation method of the above-mentioned positive electrode sodium supplement agent is:
[0109] Step 1. Sodium carbonate, manganese acetate and boric acid were first mixed in a molar ratio of 0.54:1:1, added to 100 mL of anhydrous ethanol, and magnetically stirred at 500 rpm for 2 h. Then, 25% citric acid was added, which was the sum of the mass of the sodium source, the manganese source and the boron source, and stirring was continued for 30 min.
[0110] Step 2. Add NaNi according to the coating amount of 23% 1 / 3 Mn 1 / 3 Fe 1 / 3 The O2 positive electrode material was stirred for 1 h and then evaporated to dryness in an oil bath at 80 °C;
[0111] Step 3. Sinter it at 700 °C in an inert atmosphere for 24 h to obtain NaNi 1 / 3 Mn 1 / 3 Fe 1 / 3 O2@NaMnBO3.
[0112] The above-mentioned positive electrode sodium supplement is used for active materials, specifically: NaNi 1 / 3 Mn 1 / 3 Fe 1 / 3 The O2@NaMnBO3 powder was ball-milled for 8 h. After being fully ground, it was uniformly mixed with the P2 phase positive electrode material in a drying room at a molar ratio of 1:9 to obtain the active material.
[0113] The above active materials were assembled into a full battery. Specifically, the active material (80 wt%) was mixed with acetylene black (AB, 10 wt%) and polyvinylidene fluoride (PVDF, 10 wt%) in N-methylpyrrolidone (NMP) to form a slurry. Then, the slurry was coated on aluminum foil. The pole piece was dried in a vacuum drying oven at 80 °C for 12 h, and assembled into a full battery in a glove box in the order of negative electrode shell-spring-gasket-negative electrode (hard carbon)-electrolyte-diaphragm-electrolyte-positive electrode-positive electrode shell.
[0114] Performance Testing
[0115] The full batteries prepared in Examples 1-3 and Comparative Examples 1-4 were subjected to a 50-cycle life test under the test conditions of 2-4V, 1C. The results are as follows: Figure 3 shown.
[0116] As can be seen from the figure, the discharge specific capacities of Examples 1-3 are 108 mAh / g, 105.3 mAh / g, and 102 mAh / g, respectively; the capacity retention rates after 50 cycles are 91.29%, 89.17%, and 85.88%, respectively; the discharge specific capacities of Comparative Examples 1-4 are 98.2 mAh / g, 106.2 mAh / g, 98.3 mAh / g, and 107.6 mAh / g, respectively, and the capacity retention rates after 50 cycles are 58.35%, 61.49%, 67.45%, and 76.49%, respectively. This indicates that the addition of the sodium supplement not only significantly improves the cycle stability of the battery, but also increases the capacity.
[0117] It can be seen from Comparative Example 3 that NaNi 1 / 3 Mn 1 / 3 Fe 1 / 3 O2@NaFeBO3 can improve capacity, but its effect on cycle stability is not as good as that of NaNi 1 / 3 Mn 1 / 3 Fe 1 / 3 O2@NaMnBO3 is significant because Fe 2+ / 3+ It can undergo redox reactions and provide partial capacity, but the high iron content can also cause structural collapse during the charge and discharge process, resulting in structural instability. NaMnBO3 has a stable tetrahedral open framework structure and therefore exhibits excellent electrochemical stability.
[0118] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technician familiar with this profession can make some changes or modifications to equivalent embodiments of equivalent changes using the technical contents disclosed above without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still fall within the scope of the technical solution of the present invention.
Claims
1. An application of a positive electrode sodium supplement, characterized in that: The positive electrode sodium supplement NaNi 1 / 3 Mn 1 / 3 Fe 1 / 3 O2@NaMnBO3 and P2 phase positive electrode material are uniformly mixed in a molar ratio of 1:(8-10) to obtain active material; the coating mass of NaMnBO3 is NaNi 1 / 3 Mn 1 / 3Fe 1 / 3 10-20% of the mass of O2.
2. The use of a positive electrode sodium supplement according to claim 1, characterized in that: NeNi 1 / 3 Mn 1 / 3 Fe 1 / 3 The particle size of O2@NaMnBO3 is 5-8 μm.
3. The use of a positive electrode sodium supplement according to claim 1, characterized in that: The preparation of the positive electrode sodium supplement comprises the following steps: (1) Mix a sodium source, a manganese source and a boron source, disperse them in anhydrous ethanol, add citric acid, and continue to disperse them evenly to obtain a dispersion; (2) Add NaNi to the dispersion prepared in step (1) 1 / 3 Mn 1 / 3 Fe 1 / 3 O2, disperse evenly, evaporate the solvent to obtain a solid; (3) Sintering the solid obtained in step (2) at 400-800 °C for 20-24 h under inert gas to obtain the positive electrode sodium supplement NaNi 1 / 3 Mn 1 / 3 Fe 1 / 3 O2@NaMnBO3.
4. The use of a positive electrode sodium supplement according to claim 3, characterized in that: In step (1), the sodium source is one or more of sodium carbonate, sodium acetate and sodium oxalate; the manganese source is one or more of manganese acetate, manganese oxalate, manganese carbonate and manganese tetraoxide; and the boron source is boric acid or boron trioxide.
5. The use of a positive electrode sodium supplement according to claim 3, characterized in that: Step (1) The sodium source, manganese source and boron source are mixed in a molar ratio of (1-1.1):1:
1.
6. The use of a positive electrode sodium supplement according to claim 3, 4 or 5, characterized in that: The mass of the citric acid in step (1) is 25-40% of the total mass of the sodium source, the manganese source and the boron source.
7. The use of a positive electrode sodium supplement according to claim 3, characterized in that: The dispersion in step (1) is carried out by stirring at a speed of 400-600 rpm for 1-3 h, and the continued dispersion is carried out by stirring at a speed of 400-600 rpm for 30-60 min.
8. The use of a positive electrode sodium supplement according to claim 3 or 7, characterized in that: The dispersion in step (2) is carried out by stirring at a speed of 400-600 rpm for 1-3 h.
9. The use of a positive electrode sodium supplement according to claim 1, characterized in that: The active materials are assembled into button cells.
10. The use of a positive electrode sodium supplement according to claim 9, characterized in that: The active material is mixed with acetylene black and polyvinylidene fluoride in N-methylpyrrolidone to form a slurry, and the slurry is coated on an aluminum foil to obtain a positive electrode sheet; the positive electrode sheet is dried in a vacuum drying oven, and assembled into a button battery in a glove box in the order of negative electrode shell-spring-gasket-negative sodium sheet-electrolyte-diaphragm-electrolyte-positive electrode sheet-positive electrode shell.
Citation Information
Patent Citations
Sodium ion battery positive electrode containing sodium supplementation additive and preparation method and application thereof
CN110112475A
Application of positive electrode sodium supplement agent in sodium ion battery
CN110165218A
Sodium-rich transition metal oxide composite sodium-supplementing positive electrode active material, positive electrode material, positive electrode, preparation of positive electrode and application of positive electrode in sodium-ion battery
CN111293290A
Metal boride and borate composite coated modified nickel-cobalt-manganese ternary material precursor and preparation method thereof
CN113540466A
Modified sodium ion battery layered ternary positive electrode material and preparation method thereof
CN114695853A