A method for detecting 12 elements in lithium tetrafluoroborate battery electrolyte
By entering the lithium tetrafluoroborate electrolyte sample solution into the inductively coupled plasma emission spectrometer in the form of an aerosol, combined with superior pure reagents and high-sensitivity ICP-OES instruments, the existing problem of poor detection accuracy of lithium-ion battery electrolyte is solved. Comprehensive and accurate detection of elements in the lithium-ion battery electrolyte is achieved.
Patent Information
- Application Number
- CN202410573813.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-10
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-05-10
AI Technical Summary
Existing lithium-ion battery electrolyte detection methods cannot accurately and quantitatively detect impurities in the electrolyte, and there are few parameters in the quality inspection process, resulting in poor detection accuracy.
The lithium tetrafluoroborate electrolyte sample solution is introduced into the atomization system from the carrier gas and enters the inductively coupled plasma emission spectrometer. The signal intensity of the characteristic spectral line of the element to be measured in the sample is proportional to the element concentration for quantitative analysis. Combined with the superior grade Pure reagents and highly sensitive ICP-OES instruments enable rapid and accurate detection of multiple elements.
It improves the accuracy and precision of detection results, can comprehensively and effectively detect elements in lithium tetrafluoroborate battery electrolyte, reduces errors in detection results, and provides accurate element mass and concentration data.
Smart Images

Figure CN118408923B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of battery raw material detection, and more specifically, to a method for detecting 12 elements in a lithium tetrafluoroborate battery electrolyte. Background Art
[0002] Lithium batteries are a type of battery that uses lithium metal or lithium alloy as positive / negative electrode materials and non-aqueous electrolyte solutions. Strictly speaking, lithium batteries are divided into two types: lithium metal batteries and lithium ion batteries. Lithium metal batteries use metallic lithium as electrodes, while lithium ion batteries exist in the form of ions at the electrodes. Lithium metal batteries generate electricity through the corrosion or oxidation of metallic lithium. They are useless after use and cannot be recharged, so they are also called primary batteries. Lithium ion batteries use the concentration difference of lithium ions to store and discharge energy. There is no metallic lithium in the battery, so they are also called lithium secondary batteries (rechargeable batteries). Currently, the rechargeable lithium batteries used in mobile phones, cameras, power tools, electric vehicles, energy storage, communication base stations, etc. on the market are all lithium ion batteries. Generally, most commonly used lithium batteries on the market are lithium ion batteries. They are the representative of modern high-performance batteries, and people are also accustomed to simply calling them lithium batteries.
[0003] Lithium-ion batteries mainly rely on the movement of lithium ions between the positive and negative electrodes to work. During the charge and discharge process, Li+ is embedded and deintercalated back and forth between the two electrodes: when charging, Li+ is deintercalated from the positive electrode and embedded into the negative electrode through the electrolyte, and the negative electrode is in a lithium-rich state. The opposite is true during discharge. Lithium tetrafluoroborate (LiBF4) has the advantages of low toxicity and high safety, and has relatively high thermal stability. It is not easy to decompose at high temperatures. At the same time, under low temperature conditions, LiBF4 also exhibits good battery performance. Therefore, it is often used as an electrolyte in lithium batteries.
[0004] However, the existing rapid detection method for impurities in lithium-ion battery electrolyte cannot accurately and quantitatively obtain the amount of electrolyte; at the same time, the detection operation of the existing lithium-ion battery electrolyte quality inspection method is too simple, and the detection parameters in the quality inspection process are relatively few, which cannot comprehensively and effectively detect and analyze the quality of lithium-ion battery electrolyte, thereby resulting in poor accuracy in the quality inspection and analysis of lithium-ion battery electrolyte.
[0005] Therefore, the present invention aims to provide a method for detecting 12 elements in lithium tetrafluoroborate battery electrolyte to solve the above problems. Summary of the invention
[0006] The purpose of the present invention is to provide a detection method for 12 elements in a lithium tetrafluoroborate battery electrolyte. The detection method introduces a sample solution into an atomization system through a carrier gas, and then enters an inductively coupled plasma emission spectrometer in the form of an aerosol. The signal intensity of characteristic spectral lines of the elements to be measured in the sample solution is proportional to the element concentration for quantitative analysis. The elements in the lithium tetrafluoroborate battery electrolyte can be comprehensively and effectively detected, and the accuracy of the detection result can be improved.
[0007] The above technical objectives of the present invention are achieved through the following technical solutions: A method for detecting 12 elements in lithium tetrafluoroborate battery electrolyte, comprising the following steps:
[0008] S1. Obtaining a lithium tetrafluoroborate electrolyte sample solution;
[0009] S2, the sample solution is introduced into the atomization system by the carrier gas, and then enters the inductively coupled plasma emission spectrometer in the form of aerosol, and is fully evaporated, dissociated, atomized and ionized in high temperature and inert gas to generate composite light;
[0010] S3, decomposing the generated composite light into spectral lines arranged in order of wavelengths through a monochromator to form a spectrum;
[0011] S4. Use a detector to detect the wavelength and intensity of the spectral lines in the spectrum, and calculate the determination results of the elements in the lithium tetrafluoroborate electrolyte sample.
[0012] The present invention is further configured as follows: the method for preparing the lithium tetrafluoroborate electrolyte sample solution comprises the following steps:
[0013] S11. Weigh a certain amount of lithium tetrafluoroborate electrolyte sample and add it to a polytetrafluoroethylene beaker. Heat it on a hot plate in a fume hood at low temperature until it evaporates to near dryness. Remove it and let it cool slightly. Then add nitric acid, cover it, and heat it on a hot plate until it is completely digested.
[0014] S12. Continue heating to drive out the acid until a small amount of nitric acid solution remains. After cooling to room temperature, rinse the beaker repeatedly with an appropriate amount of pure water. Transfer all the washing liquid to a volumetric flask, dilute to the mark with pure water, and mix well to obtain the sample solution.
[0015] The present invention is further configured such that: the number of times the beaker is rinsed repeatedly in step S12 is 3 to 5 times.
[0016] The present invention is further configured as follows: the reagents used in the preparation process of the lithium tetrafluoroborate electrolyte sample solution are all high-grade pure reagents, and the preparation water is first-grade water that complies with the provisions of GB / T 6682.
[0017] The present invention is further configured as follows: the detector in step S4 uses an Agilent inductively coupled plasma optical emission spectrometer (ICP-OES, Aglient 5100) for analysis, which has high sensitivity and can achieve rapid analysis of multiple elements in one injection.
[0018] The present invention is further configured as follows: the measurement result in step S4 is calculated by the following formula:
[0019]
[0020] Wherein, X is the content of the element to be measured in the sample, in milligrams per kilogram (mg / kg); C is the mass concentration of the element to be measured in the sample solution, in milligrams per liter (mg / L); C0 is the mass concentration of the element to be measured in the blank solution of the sample, in milligrams per liter (mg / L); V is the volume of the sample digestion solution, in milliliters (mL); f is the sample dilution multiple; m is the weighed mass of the sample, in grams (g).
[0021] In summary, the present invention has the following beneficial effects:
[0022] 1. In the present invention, after the sample solution is introduced into the atomization system by the carrier gas, it enters the inductively coupled plasma emission spectrometer in the form of aerosol, and quantitative analysis is performed by using the characteristic spectral line signal intensity of the element to be measured in the sample solution to be proportional to the element concentration, so that the elements in the lithium tetrafluoroborate battery electrolyte can be comprehensively and effectively detected, and the accuracy of the detection results can be improved at the same time;
[0023] 2. The reagents used in this test method are all high-grade pure reagents, and the experimental water is first-grade water that complies with GB / T 6682. This can reduce interference with the test results and avoid the situation in which the test results are too large due to excessive impurities in the raw materials during the preparation and testing of the sample solution, thereby improving the accuracy of the test results;
[0024] 3. The measuring instrument used in this detection method is ICP, which has very high sensitivity and can realize rapid analysis of multiple elements in one injection. At the same time, the content levels of many heavy metal elements in lithium tetrafluoroborate electrolyte are very low. The use of this instrument can more accurately detect the mass and concentration of elements in the sample solution, providing accurate data for the calculation of the test results, further improving the accuracy of the test results. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is a flow chart of a method for detecting 12 elements in a lithium tetrafluoroborate battery electrolyte according to an embodiment of the present invention;
[0026] Figure 2It is a flow chart of the method for preparing a lithium tetrafluoroborate electrolyte sample solution in an embodiment of the present invention. DETAILED DESCRIPTION
[0027] The following is combined with Figure 1-2 The present invention is described in further detail.
[0028] Embodiment: A method for detecting 12 elements in lithium tetrafluoroborate battery electrolyte, comprising the following steps:
[0029] S1. Weigh a quantitative amount of lithium tetrafluoroborate electrolyte sample and add it to a polytetrafluoroethylene beaker. Heat it on a hot plate in a fume hood at low temperature until it evaporates to near dryness, remove it and cool it slightly, then add nitric acid, cover it, and heat it on a hot plate until it is completely digested; then continue to heat to drive out the acid until a small amount of nitric acid solution remains. After cooling to room temperature, rinse the beaker repeatedly with an appropriate amount of pure water, transfer all the washings to a volumetric flask, dilute it to the mark with pure water, and then mix it to obtain a lithium tetrafluoroborate electrolyte sample solution;
[0030] S2, the sample solution is introduced into the atomization system by the carrier gas, and then enters the inductively coupled plasma emission spectrometer in the form of aerosol, and is fully evaporated, dissociated, atomized and ionized in high temperature and inert gas to generate composite light;
[0031] S3, decomposing the generated composite light into spectral lines arranged in order of wavelengths through a monochromator to form a spectrum;
[0032] S4. Use a detector to detect the wavelength and intensity of the spectral lines in the spectrum, and calculate the determination results of the elements in the lithium tetrafluoroborate electrolyte sample.
[0033] The preferred reagents used in this embodiment are all high-grade pure reagents, and the experimental water is first-grade water in accordance with GB / T6682. Nitric acid is: ρ(HNO3)=1.42g / ml, high-grade pure or higher, purified if necessary; nitric acid solution: 5+95, prepared with nitric acid; single element standard stock solution: C=1.00mg / ml; wherein spectrally pure metals (purity greater than 99.99%) or other standard substances can be used to prepare a standard stock solution with a concentration of 1000mg / L, and a suitable medium can be selected according to the properties of each element, or a certified standard solution can be directly purchased; multi-element standard stock solution: C=100mg / L, a certified mixed standard solution can be purchased, or the elements can be grouped and prepared into a mixed standard stock solution with a concentration of 100mg / L according to the mutual interference between elements, the properties of the standard solution and the content of the element to be measured; argon: purity ≥99.999%; lithium borate: purity greater than 99%.
[0034] The preferred ICP measuring instrument in this embodiment has very high sensitivity and can realize rapid analysis of multiple elements in one injection; at the same time, the content level of many heavy metal elements in lithium tetrafluoroborate electrolyte is very low, which is suitable for determination by this instrument. All glass instruments must be soaked in (1+1) nitric acid solution for more than 24 hours, and then rinsed with tap water and deionized water in turn; the inductively coupled plasma emission spectrometer: equipped with polytetrafluoroethylene matrix tube and atomization chamber; temperature-controlled electric heating plate: control temperature ±2.5°C; polytetrafluoroethylene beaker: 100mL; analytical balance: accuracy ±0.1mg; volumetric flask: 10mL; and instruments and equipment commonly used in general laboratories are used.
[0035] Experimental data
[0036] 1. Preparation of standard solution and standard curve
[0037] Standard solution series 1: Accurately pipette 5 mL of potassium, calcium, and sodium single standard solutions (1000 mg / L) into a 50 mL volumetric flask, dilute to scale with pure water, shake well, and then dilute the above mixed standard solution step by step into standard solutions of different concentrations for testing;
[0038] Standard solution series 2: a mixed certified standard solution (100 mg / L) containing 9 elements: arsenic, cadmium, chromium, copper, iron, magnesium, nickel, lead, and zinc. The mixed standard solution is then diluted step by step to form a series of element standard solutions of different concentrations to be tested, as shown in Table 1:
[0039] Table 1 Concentration of element standard solution series
[0040]
[0041]
[0042] 2. Selection of instrument analysis conditions
[0043] In this embodiment, an Agilent inductively coupled plasma optical emission spectrometer (ICP-OES, Aglient5100) is specifically used for analysis; after starting up, it needs to be preheated for more than 20 minutes. Different types of inductively coupled plasma mass spectrometers have different optimal working conditions. Tuning is required before analysis, and appropriate analysis conditions are selected according to the properties of the elements to be measured. The recommended reference conditions for determination are shown in Table 2, and the analysis spectra of element selection are shown in Table 3.
[0044] Table 2 Recommended instrument conditions and parameters
[0045] Parameter name parameter Observation method Axial power 1.20kW Plasma gas flow 12.0L / min Carrier gas flow 1.00L / min Atomizing gas flow 0.70L / min Analyze pump speed 12rpm
[0046] Table 3 Wavelengths of spectral lines of elements to be tested
[0047]
[0048] 3. Preparation of sample solution
[0049] Weigh about 2.5 g of sample (accurate to 0.0001 g) and add it into a 100 ml polytetrafluoroethylene beaker. Heat it on a hot plate in a fume hood at low temperature (about 100°C). Wait until it evaporates to near dryness, remove it and cool it slightly. Then add 5 ml of nitric acid (1.2.2), cover it, and heat it on a hot plate at 160°C until it is completely digested.
[0050] Continue heating to drive out the acid until 2ml~3ml of nitric acid solution remains. After cooling to room temperature, rinse the beaker 3~5 times with an appropriate amount of pure water. Transfer all the washing liquid to a 25mL volumetric flask, make up to the mark with pure water, mix well, and perform the measurement.
[0051] According to the preparation method of the sample solution, a blank solution was prepared without adding a sample. The blank solution was measured 7 times, and 3 times the standard deviation was taken as the corresponding detection limit, and 3 times the detection limit was the determination lower limit. The detection limit and determination lower limit of the method of the present invention are shown in Table 4:
[0052] Table 4 Summary of detection limits and lower limits of determination for lithium tetrafluoroborate electrolyte method
[0053]
[0054]
[0055] Prepare the sample solution according to the sample solution preparation method. The repeatability of arsenic, calcium, iron, potassium, magnesium, and sodium elements is determined by preparing 6 samples in parallel for determination. The repeatability of cadmium, chromium, copper, nickel, lead, and zinc elements is determined by adding 2 mg / kg of the target substance (adding standard solutions containing cadmium, chromium, copper, nickel, lead, and zinc elements) after weighing the sample, and preparing 6 samples in parallel for determination. The consistency between the determination results is tested by the RSD% of the 6 measured values. The results of the method repeatability test are shown in Table 5:
[0056] Table 5 Repeatability test results of lithium tetrafluoroborate electrolyte method
[0057]
[0058] The results showed that the relative standard deviation was between 1.07% and 4.08%, meeting the requirements of relevant control standards.
[0059] Prepare the sample solution according to the preparation method of the sample solution. Weigh 9 parallel lithium tetrafluoroborate samples, of which the sample solutions for calcium, chromium, iron, potassium, magnesium, sodium, and zinc element recovery are target substances (calcium, chromium, iron, potassium, magnesium, sodium, and zinc element standard solutions) at three levels of 0.5 times, 1 times, and 5 times the background value of the added sample, and the sample solutions for arsenic, cadmium, copper, nickel, and lead element recovery are target substances (arsenic, cadmium, copper, nickel, and lead element standard solutions) with 1 mg / kg, 2 mg / kg, and 10 mg / kg, respectively. Three parallel samples were prepared for each added level for determination. The experimental results of the method accuracy are shown in Table 6:
[0060] Table 6 Lithium tetrafluoroborate electrolyte method accuracy experimental results
[0061]
[0062]
[0063]
[0064] The results showed that the recovery rate was between 83.2% and 110.4%, meeting the requirements of relevant control standards.
[0065] In this embodiment, the calculation is performed according to the following formula:
[0066]
[0067] Where: X is the content of the element to be measured in the sample, in milligrams per kilogram (mg / kg); C is the mass concentration of the element to be measured in the sample solution, in milligrams per liter (mg / L); C0 is the mass concentration of the element to be measured in the blank solution of the sample, in milligrams per liter (mg / L); V is the volume of the sample digestion solution, in milliliters (mL); f is the sample dilution multiple; M is the weighed mass of the sample, in grams (g).
[0068] This embodiment includes blank test, calibration validity check, precision control and accuracy control; in the blank test, at least 2 digestion blanks shall be measured for each batch of samples, and the blank value shall be lower than the method determination lower limit, otherwise the experimental water quality, reagent purity, vessel cleanliness and instrument performance shall be checked; in the calibration validity check, a calibration curve shall be drawn for each batch of sample analysis, and the correlation coefficient γ of the calibration curve shall be ≥ 0.999. For every 10 samples analyzed, a calibration solution of the intermediate concentration of the calibration curve shall be used for calibration verification, and the relative deviation of the measurement result from the concentration of the most recent calibration curve at that point shall be ≤ ± 10%, otherwise the calibration curve shall be redrawn; in the precision control, at least 10% of the parallel samples shall be measured for each batch of samples, and when the number of samples is less than 10, at least one parallel sample shall be measured, and the relative deviation of the two parallel measurement results shall be ≤ ± 10%; in the accuracy control, at least one recovery test shall be carried out for each batch of samples, and the recovery rate shall be between 80% and 120%.
[0069] The method detection limit and determination lower limit, method repeatability and recovery rate experiment in this example all meet the methodological investigation requirements, indicating that the standard detection method is reliable and stable.
[0070] This specific embodiment is merely an explanation of the present invention and is not a limitation of the present invention. After reading this specification, those skilled in the art may make non-creative modifications to the present embodiment as needed. However, as long as they are within the scope of the claims of the present invention, they are protected by the patent law.
Claims
1. A method for detecting 12 elements in lithium tetrafluoroborate battery electrolyte. Its characteristics are: The following steps are involved: S1. Obtaining a lithium tetrafluoroborate electrolyte sample solution; S2, the sample solution is introduced into the atomization system by the carrier gas, and then enters the inductively coupled plasma emission spectrometer in the form of aerosol, and is fully evaporated, dissociated, atomized and ionized in high temperature and inert gas to generate composite light; S3, decomposing the generated composite light into spectral lines arranged in order of wavelengths through a monochromator to form a spectrum; S4. Using a detector to detect the wavelength and intensity of the spectrum line in the spectrum, and calculating the determination results of the elements in the lithium tetrafluoroborate electrolyte sample; The measurement result in step S4 is calculated by the following formula: ; In the formula, X is the content of the element to be tested in the sample, in milligrams per kilogram (mg / kg); C is the mass concentration of the element being measured in the sample solution, in milligrams per liter (mg / L); is the mass concentration of the element being measured in the blank solution of the sample, in milligrams per liter (mg / L); V is the fixed volume of the sample digestion solution, in milliliters (mL); is the dilution multiple of the sample; m Weigh the mass of the sample in grams (g); The elements contained in the sample solution include As, Ca, Cd, Cr, Cu, Fe, K, Mg, Na, Ni, Pb and Zn; The detection instrument conditions and parameters were as follows: observation mode was axial, power was 1.20 kW, plasma gas flow rate was 12.0 L / min, carrier gas flow rate was 1.00 L / min, nebulizer gas flow rate was 0.70 L / min, and analytical pump speed was 12 rpm.
2. A method for detecting 12 elements in a lithium tetrafluoroborate battery electrolyte according to claim 1, Its characteristics are: The method for preparing the lithium tetrafluoroborate electrolyte sample solution comprises the following steps: S11. Weigh a certain amount of lithium tetrafluoroborate electrolyte sample and add it to a polytetrafluoroethylene beaker. Heat it on a hot plate in a fume hood at low temperature until it evaporates to near dryness. Remove it and let it cool slightly. Then add nitric acid, cover it, and heat it on a hot plate until it is completely digested. S12. Continue heating to drive out the acid until a small amount of nitric acid solution remains. After cooling to room temperature, rinse the beaker repeatedly with an appropriate amount of pure water. Transfer all the washing liquid to a volumetric flask, dilute to the mark with pure water, and mix well to obtain the sample solution.
3. A method for detecting 12 elements in a lithium tetrafluoroborate battery electrolyte according to claim 2, Its characteristics are: The beaker is rinsed 3 to 5 times in step S12.
4. A method for detecting 12 elements in a lithium tetrafluoroborate battery electrolyte according to claim 2, Its characteristics are: The reagents used in the preparation process of the lithium tetrafluoroborate electrolyte sample solution are all high-grade pure reagents, and the preparation water is first-grade water that complies with the provisions of GB / T 6682.
5. A method for detecting 12 elements in a lithium tetrafluoroborate battery electrolyte according to claim 2, Its characteristics are: The reagents used in the preparation process of the lithium tetrafluoroborate electrolyte sample solution are all high-grade pure reagents, and the preparation water is first-grade water that complies with the provisions of GB / T 6682.
Citation Information
Patent Citations
Method for determining content of Fe in carbon-coated SiO lithium battery negative electrode material
CN111638206A
Method for rapidly determining 12 impurity elements in battery grade cobaltous sulfate
CN114965444A
Method for rapidly detecting impurities in lithium ion battery electrolyte
CN116990293A
Simultaneous determination of lithium difluoro (oxalato) borate and lithium bis (oxalato) borate in lithium battery electrolyte
CN117092089A