A method for corrosion protection of zinc-aluminum-magnesium coated steel plates during welding
By using welding heat to clad low-melting-point anti-corrosion materials during the welding process of zinc-aluminum-magnesium coated steel plates to form an anti-corrosion layer, the problem of insufficient weld corrosion resistance is solved, achieving efficient and environmentally friendly anti-corrosion effect, and improving production efficiency and metallurgical bonding.
Patent Information
- Application Number
- CN202410489325.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-23
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2044-04-23
AI Technical Summary
The weld seam of zinc-aluminum-magnesium coated steel plates has insufficient corrosion resistance after welding, and conventional protection methods are ineffective, which also affects production efficiency and cost.
Low-melting-point anti-corrosion materials are used to clad the weld surface with welding heat during the welding process to form an anti-corrosion layer. The anti-corrosion layer is prepared simultaneously using welding heat and protective gas, avoiding the need for spraying or brushing processes.
It improves the corrosion resistance of welds and heat-affected zones, increases production efficiency, reduces costs, and has a metallurgical bond between the anti-corrosion layer and the weld, resulting in good friction resistance, low oxygen content, and environmental friendliness and energy saving.
Smart Images

Figure CN118437609B_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of welding corrosion protection technology, and in particular to a method for welding corrosion protection of zinc-aluminum-magnesium coated steel plates during welding. Background Technology
[0002] Zinc-aluminum-magnesium coated steel sheets, due to their high corrosion resistance and self-healing properties, are now widely used in the automotive, photovoltaic, and highway guardrail industries, gradually replacing the post-immersion galvanizing process. However, the processing requires welding using a Gaussian heat source (TIG welding, MIG welding, plasma welding, laser welding, etc.). Since the melting point of steel is much higher than the boiling points of zinc and magnesium in the coating, the weld surface lacks coating protection, making it difficult to guarantee the overall corrosion resistance of the structure. The conventional method is to apply a coating after welding for protection. However, because the weld surface is oxidized after welding, the adhesion between the weld surface and the coating is insufficient, making it easy to peel off under actual working conditions, thus failing to guarantee corrosion resistance. Furthermore, this method increases and reduces production efficiency; the overall cost of pre-plating is basically the same as that of post-immersion galvanizing, failing to achieve the goal of reducing costs and improving production efficiency.
[0003] Therefore, there is an urgent need to develop a method for corrosion protection of zinc-aluminum-magnesium coated products during welding, in order to solve the problem of insufficient corrosion resistance of the weld bead after welding of zinc-aluminum-magnesium coated steel plates. Summary of the Invention
[0004] This application provides a method for corrosion protection of zinc-aluminum-magnesium coated steel plates during welding, in order to solve the technical problem of insufficient corrosion resistance of weld beads after welding of zinc-aluminum-magnesium coated steel plates in the prior art.
[0005] In a first aspect, this application provides a method for welding corrosion protection of zinc-aluminum-magnesium coated steel plates during welding, the method comprising:
[0006] Weld at least two zinc-aluminum-magnesium coated steel plates to form a weld bead;
[0007] A low-melting-point anti-corrosion material is placed at the weld bead, and the welding heat source is used to melt the low-melting-point anti-corrosion material so that the melted low-melting-point anti-corrosion material is fused onto at least a portion of the surface of the weld bead to form an anti-corrosion layer.
[0008] Optionally, the temperature at which the low-melting-point anti-corrosion material is placed at the weld bead satisfies the following relationship:
[0009] T m ≤T≤T B -20
[0010] In the formula, T represents the temperature at which the low-melting-point anti-corrosion material is placed at the weld bead. m T represents the melting point of the low-melting-point anti-corrosion material. mThe melting point of the zinc-aluminum-magnesium coated steel sheet, T B This indicates the boiling point of the low-melting-point corrosion-resistant material.
[0011] Optionally, the chemical composition of the low-melting-point corrosion-resistant material, by mass fraction, includes: Zn > 50% or Al > 50%.
[0012] Optionally, the low-melting-point anti-corrosion material includes one or more of anti-corrosion wires and anti-corrosion tapes.
[0013] Optionally, the diameter of the anti-corrosion wire is 0.8 mm to 3.0 mm.
[0014] Optionally, the thickness of the anti-corrosion strip is 0.2mm to 3.0mm.
[0015] Optionally, the welding heat source is a Gaussian distributed heat source; the welding shielding gas includes carbon dioxide, argon, and a mixture of carbon dioxide and argon.
[0016] Optionally, before placing the low-melting-point anti-corrosion material at the weld bead, the method further includes:
[0017] Preheat the low-melting-point anti-corrosion material.
[0018] Optionally, in the initial stage of the welding process, the feeding speed and preheating temperature of the low-melting-point anti-corrosion material are higher than those in the stable welding stage; in the final stage of the welding process, the feeding speed and preheating temperature of the low-melting-point anti-corrosion material are lower than those in the stable welding stage.
[0019] The technical solutions provided in this application have the following advantages compared with the prior art:
[0020] This application provides a method for welding corrosion protection onto zinc-aluminum-magnesium coated steel plates during welding. By heating a low-melting-point corrosion-resistant material using a welding heat source, and achieving cladding on the weld surface under the action of a protective gas, the welding of the zinc-aluminum-magnesium coated steel plate and the preparation of the corrosion-resistant layer on the weld surface are carried out simultaneously. This method solves the problem of insufficient corrosion resistance in the weld and heat-affected zone of zinc-aluminum-magnesium coated steel plates. Furthermore, it eliminates the need for spraying and brushing processes, improving production efficiency. The corrosion-resistant layer prepared by this method has good anti-friction properties due to its metallurgical bond with the weld. The prepared corrosion-resistant layer has high purity and low oxygen content. Simultaneously, it fully utilizes welding energy and protective gas, making it energy-saving and environmentally friendly. Attached Figure Description
[0021] The accompanying drawings, which are incorporated in and form part of this specification, illustrate embodiments consistent with this application and, together with the description, serve to explain the principles of this application.
[0022] To more clearly illustrate the technical solutions in the embodiments of this application or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, for those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0023] Figure 1 A flowchart illustrating a method for corrosion protection during welding of zinc-aluminum-magnesium coated steel plates, provided in this application embodiment;
[0024] Figure 2 A schematic diagram illustrating a method for corrosion protection of zinc-aluminum-magnesium coated steel plates during welding, provided in an embodiment of this application;
[0025] Figure 3 This is a cross-sectional view of the anti-corrosion layer of the zinc-aluminum-magnesium coated steel plate weld bead provided in Embodiment 2 of this application. Detailed Implementation
[0026] To make the objectives, technical solutions, and advantages of the embodiments of this application clearer, the technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, not all embodiments. Based on the embodiments of this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application.
[0027] Various embodiments of this application may exist in the form of a range; it should be understood that the description in the form of a range is merely for convenience and brevity and should not be construed as a hard limitation on the scope of this application; therefore, it should be considered that the range description has specifically disclosed all possible sub-ranges and single numerical values within that range. For example, it should be considered that the range description from 1 to 6 has specifically disclosed sub-ranges such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., and single numbers within the range, such as 1, 2, 3, 4, 5, and 6, regardless of the range. Furthermore, whenever a numerical range is referred to herein, it means including any referenced number (fraction or integer) within the referred range.
[0028] Furthermore, in the description of this application, the terms "comprising," "including," etc., mean "including but not limited to." In this document, relational terms such as "first" and "second" are used merely to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. In this document, "and / or" describes the relationship between related objects, indicating that three relationships can exist; for example, A and / or B can represent: A alone, A and B simultaneously, or B alone. A and B can be singular or plural. In this document, "at least one" means one or more, and "more than" means two or more. "At least one," "at least one of the following," or similar expressions refer to any combination of these items, including any combination of single or plural items. For example, "at least one of a, b, or c" or "at least one of a, b, and c" can both mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, and c can be a single or multiple.
[0029] Unless otherwise specified, all raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.
[0030] Figure 1 This is a flowchart illustrating a method for corrosion protection of zinc-aluminum-magnesium coated steel plates during welding, as provided in an embodiment of this application.
[0031] Figure 2 This is a schematic diagram of a method for corrosion protection of zinc-aluminum-magnesium coated steel plates by welding, provided in an embodiment of this application.
[0032] Please see Figure 1 and Figure 2 This application provides a method for corrosion protection of zinc-aluminum-magnesium coated steel plates during welding, the method comprising:
[0033] S1. Weld at least two zinc-aluminum-magnesium coated steel plates to form a weld bead;
[0034] In some specific implementations, at least two zinc-aluminum-magnesium coated steel plates are spliced together. The high-temperature zone of the welding heat source heats and melts the steel plates and welding wire. After the temperature is lower than the melting point of the steel plates, the steel plates solidify to form a weld bead.
[0035] In some embodiments, the method further includes, prior to placing the low-melting-point corrosion-resistant material at the weld bead:
[0036] Low-melting-point corrosion-resistant materials are preheated using high-frequency induction or resistance.
[0037] In the embodiments of this application, preheating facilitates the better spread of the molten low-melting-point anti-corrosion material on the weld surface, thereby improving the bonding force between the anti-corrosion layer and the weld.
[0038] S2. Place the low-melting-point anti-corrosion material at the weld bead, and use the welding heat source of the welding to melt the low-melting-point anti-corrosion material so that the melted low-melting-point anti-corrosion material is fused onto at least a portion of the surface of the weld bead to form an anti-corrosion layer.
[0039] In some specific embodiments, the low-melting-point anti-corrosion material is transported behind the central region away from the welding heat source relative to the welding direction. The low-melting-point anti-corrosion material is placed at the weld bead and melted using the low-temperature zone of the welding heat source, so that the melted low-melting-point anti-corrosion material is fused onto at least a portion of the surface of the weld bead to form an anti-corrosion layer.
[0040] In this embodiment, transporting the low-melting-point anti-corrosion material behind the central region away from the welding heat source helps control the temperature of the low-melting-point anti-corrosion material when placed near the welding heat source. Simultaneously, the residual heat on the weld surface after welding facilitates better spreading of the molten low-melting-point anti-corrosion material on the weld surface, improving the adhesion between the anti-corrosion layer and the weld.
[0041] In some embodiments, the heating temperature satisfies the following relationship:
[0042] T m ≤T≤T B -20
[0043] In the formula, T represents the temperature at which the low-melting-point anti-corrosion material is placed at the weld bead, Tm represents the melting point of the low-melting-point anti-corrosion material, Tm < the melting point of the zinc-aluminum-magnesium coated steel plate, and TB represents the boiling point of the low-melting-point anti-corrosion material.
[0044] In this embodiment, the low-melting-point anti-corrosion material is placed in the temperature range of the welding heat source, which is from the melting point to the boiling point -20°C. Within this temperature range, it is more conducive to the low-melting-point anti-corrosion material being fused onto the weld surface to form an anti-corrosion layer.
[0045] In some embodiments, the chemical composition of the low-melting-point corrosion-resistant material, by mass fraction, includes: Zn > 50% or Al > 50%.
[0046] In the embodiments of this application, the main elements of the low-melting-point anti-corrosion material are zinc or aluminum. For example, the mass fraction of Zn in the chemical composition of the low-melting-point anti-corrosion material can be 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, etc., or the mass fraction of Al>50% can be 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, etc.
[0047] In some embodiments, the low-melting-point anti-corrosion material includes one or more of anti-corrosion wires and anti-corrosion tapes.
[0048] In some embodiments, the diameter of the anti-corrosion wire is 0.8 mm to 3.0 mm.
[0049] In this embodiment, the amount of anti-corrosion wire used can be 1 to 5 wires relative to the area of the weld bead. For example, the diameter of the anti-corrosion wire can be 0.8mm, 1.0mm, 1.4mm, 1.6mm, 1.8mm, 2.0mm, 2.4mm, 2.8mm, 3.0mm, etc.
[0050] In some embodiments, the thickness of the anti-corrosion strip is 0.2 mm to 3.0 mm.
[0051] In the embodiments of this application, the amount of anti-corrosion tape used can be 1 to 5 strips relative to the area of the weld bead. For example, the thickness of the anti-corrosion tape can be 0.2mm, 0.6mm, 1.0mm, 1.6mm, 1.8mm, 2.0mm, 2.4mm, 2.8mm, 3.0mm, etc.
[0052] In some embodiments, the welding heat source is a Gaussian distributed heat source; the welding shielding gas includes carbon dioxide, argon, and a mixture of carbon dioxide and argon.
[0053] In some embodiments, the welding method includes: MIG welding, MAG welding, TIG welding, plasma arc welding, and laser welding.
[0054] By applying the anti-corrosion coating under the protection of welding gases before the weld bead is oxidized, the bonding strength between the anti-corrosion coating and the weld bead is significantly improved. Simultaneously, it avoids the oxidation of low-melting-point anti-corrosion materials in high-temperature environments, which is beneficial for the formation of the anti-corrosion coating on the weld bead.
[0055] In some embodiments, during the initial stage of the welding process, the feeding rate and preheating temperature of the low-melting-point anti-corrosion material are higher than those during the stable welding stage; during the final stage of the welding process, the feeding rate and preheating temperature of the low-melting-point anti-corrosion material are lower than those during the stable welding stage.
[0056] In the initial stage of welding (arc ignition stage), the welding heat source provides less heat, so the feeding speed of the low melting point anti-corrosion material should be reduced and the preheating temperature of the low melting point anti-corrosion material should be increased.
[0057] In the embodiments of this application, after the low-melting-point anti-corrosion material melts, it can be coated onto at least a portion of the surface of the weld by gravity or by direct application, thereby forming an anti-corrosion layer.
[0058] The present application is further illustrated below with reference to specific embodiments. It should be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of the application. Experimental methods in the following embodiments that do not specify specific conditions are generally determined according to industry standards. If there is no corresponding industry standard, then common international standards, conventional conditions, or conditions recommended by the manufacturer are followed.
[0059] Embodiments 1-4 of this application provide a method for corrosion protection of zinc-aluminum-magnesium coated steel plates during welding, including the following steps:
[0060] S11. Two zinc-aluminum-magnesium coated steel plates are spliced together. The high-temperature zone of the welding heat source heats and melts the steel plates and welding wire. After the temperature is lower than the melting point of the steel plates, the steel plates solidify to form a weld.
[0061] S21. Use high-frequency induction or resistance to preheat the low-melting-point corrosion-resistant material.
[0062] S31. Relative to the welding direction, a low-melting-point anti-corrosion material is transported behind the central area away from the welding heat source. The low-melting-point anti-corrosion material is placed at the weld bead, and the low-temperature zone of the welding heat source is used to melt the low-melting-point anti-corrosion material so that the melted low-melting-point anti-corrosion material is fused onto the surface of the weld bead to form an anti-corrosion layer.
[0063] The process parameters for the corrosion protection method of zinc-aluminum-magnesium coated steel plates by welding are shown in Tables 1 to 3. Figure 3 This is a cross-sectional view of the anti-corrosion coating on the weld bead of the zinc-aluminum-magnesium coated steel plate provided in Embodiment 2 of this application. For the cross-sectional view of the anti-corrosion coating on the weld bead of the zinc-aluminum-magnesium coated steel plate in Embodiment 2, please refer to... Figure 3 .
[0064] Table 1. Thickness and chemical composition (wt%) of zinc-aluminum-magnesium coated steel sheets
[0065]
[0066] Table 2 Welding process parameters
[0067]
[0068] Table 3 Process parameters for low melting point anti-corrosion materials
[0069]
[0070] Table 4. Process parameters for the preparation of the anti-corrosion coating
[0071] Group Heating temperature Feeding speed of low melting point anti-corrosion materials cladding thickness Example 1 720℃ 7.1 m / min 28μm Example 2 950℃ 6.0 m / min 22μm Example 3 650℃ 3.2 m / min 12μm Example 4 0℃ 2m / min 15μm
[0072] The anti-corrosion layers prepared in Examples 1-4 were subjected to neutral salt spray tests, and the results are shown in Table 5.
[0073] Table 5. Neutral salt spray results of the anti-corrosion coating.
[0074] Group Neutral salt spray time Example 1 4200h Example 2 5500h Example 3 600h Example 4 1200h
[0075] Furthermore, one or more technical solutions in the embodiments of the present invention have at least the following technical effects or advantages:
[0076] (1) In the embodiments of the present invention, the corrosion resistance of the weld and the heat-affected zone can be effectively improved.
[0077] (2) In this embodiment of the invention, the anti-corrosion layer is treated before the weld bead is oxidized, which greatly improves the bonding force between the anti-corrosion layer and the weld bead.
[0078] (3) In the embodiments of the present invention, the utilization rate of welding energy can be improved, the number of processes and costs can be reduced, and the production efficiency can be improved.
[0079] The above description is merely a specific embodiment of this application, enabling those skilled in the art to understand or implement this application. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of this application. Therefore, this application is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features claimed herein.
Claims
1. A method for corrosion protection of zinc-aluminum-magnesium coated steel plates during welding, characterized in that, The method includes: Weld at least two zinc-aluminum-magnesium coated steel plates to form a weld bead; Relative to the welding direction, a low-melting-point anti-corrosion material is transported behind a central region away from the welding heat source. The low-melting-point anti-corrosion material is placed at the weld bead, and the welding heat source is used to melt it, causing the molten material to clad at least a portion of the weld bead surface, forming a metallurgically bonded anti-corrosion layer. The chemical composition of the low-melting-point anti-corrosion material includes, by mass fraction, Al > 50%. The temperature at which the low-melting-point anti-corrosion material is placed at the weld bead satisfies the following relationship: T m ≤T≤T B -20; In the formula, T represents the temperature at which the low-melting-point anti-corrosion material is placed at the weld bead. m T represents the melting point of the low-melting-point anti-corrosion material. m The melting point of the zinc-aluminum-magnesium coated steel sheet, T B This indicates the boiling point of the low-melting-point anti-corrosion material; In the initial stage of the welding process, the preheating temperature of the low-melting-point anti-corrosion material is higher than that in the stable welding stage; in the final stage of the welding process, the preheating temperature of the low-melting-point anti-corrosion material is lower than that in the stable welding stage.
2. The method according to claim 1, characterized in that, The low-melting-point anti-corrosion material includes one or more of anti-corrosion wires and anti-corrosion strips.
3. The method according to claim 2, characterized in that, The diameter of the anti-corrosion wire is 0.8mm to 3.0mm.
4. The method according to claim 2, characterized in that, The thickness of the anti-corrosion strip is 0.2mm to 3.0mm.
5. The method according to claim 1, characterized in that, The welding heat source is a Gaussian distributed heat source; the welding shielding gas includes carbon dioxide, argon, and a mixture of carbon dioxide and argon.
6. The method according to claim 1, characterized in that, Before placing the low-melting-point anti-corrosion material at the weld bead, the method further includes: Preheat the low-melting-point anti-corrosion material.
Citation Information
Patent Citations
Application of low-melting-point flux to large-power TIG welding joint protection
CN104708229A
Cladding powder, zinc-aluminum-magnesium coated steel plate weld bead anticorrosive coating and preparation method thereof
CN117802356A