Composite conductive adhesive and preparation method and application thereof

The conductive agent modified by the silane coupling agent co-coagulates with the fluorine-containing polymer to form a composite conductive binder, which solves the problem of uneven distribution of binders and conductive agents in dry electrodes, and achieves reduction in electrode internal resistance and The performance improvement meets the comprehensive performance requirements of the battery.

CN118448634BActive Publication Date: 2024-10-11SHENZHEN QINGYAN ELECTRONIC TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410756426.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-13
Publication Date
2024-10-11
Estimated Expiration
2044-06-13

AI Technical Summary

Technical Problem

The uneven distribution of binders and conductive agents in existing dry electrodes results in high electrode impedance and limits electrode performance.

Method used

The conductive agent is surface modified with a silane coupling agent and co-condensed with the fluoropolymer to prepare a composite conductive adhesive. The surface of the fluoropolymer is coated with the silane coupling agent to form a uniform conductive network. structure to reduce the internal resistance of the electrode.

Benefits of technology

The microscopic uniform compounding of the conductive agent and the binder is achieved, which reduces the impact of the flocculant on the electrochemical performance, simplifies the process, reduces the production cost, and improves the rate performance and cycle performance of the electrode.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118448634B_ABST
    Figure CN118448634B_ABST
Patent Text Reader

Abstract

The present application proposes a composite conductive adhesive and its preparation method and application. The preparation method of the present application realizes the uniform compounding of the conductive agent and the adhesive (fluoropolymer) on a microscopic scale, the surface of the fluoropolymer is uniformly coated with the conductive agent, the conductive agent and the fluoropolymer are tightly combined, the interaction between the two is strong, and the uniformity of the prepared composite conductive adhesive is greatly improved. In the process of making electrode plates of the composite conductive adhesive of the present application, the conductive agent will be evenly dispersed in the membrane along with the fiberization of the fluoropolymer, forming a uniform conductive network structure, thereby reducing the internal resistance of the plate. The electrode plate of the present application, when applied to electrochemical energy storage devices (e.g., batteries), has better rate performance and cycle performance of the battery, and can meet various comprehensive performance requirements of the battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of electrochemical energy storage devices, and in particular to a composite conductive adhesive and a preparation method and application thereof. Background Art

[0002] Traditional wet-process electrodes use powdered active materials, conductive agents, binders, etc. mixed with solvents to prepare slurry, and then go through multiple processes such as coating, drying, solvent recovery, and rolling to prepare electrodes. Dry-process electrodes are prepared by directly compacting dry powdered electrode materials containing active materials, conductive agents, and binders, eliminating multiple manufacturing steps such as slurry preparation, drying, and solvent recovery. Dry-process electrodes are perfectly adapted to the development trend of next-generation electrochemical energy storage devices (e.g., batteries) because they do not require the use of liquid solvents, have simple processes, are environmentally friendly, have low costs, and have good electrode performance.

[0003] However, in existing dry electrodes, the distribution of binders and conductive agents is often not uniform, and the impedance of the electrode is also high, which limits the performance of the electrode. Summary of the invention

[0004] In view of this, the present application proposes a method for preparing a composite conductive adhesive to solve at least one of the above problems.

[0005] In addition, it is also necessary to provide a composite conductive adhesive prepared by the preparation method, and an electrode plate and an electrochemical energy storage device comprising the composite conductive adhesive.

[0006] An embodiment of the present application provides a method for preparing a composite conductive binder, wherein the composite conductive binder is suitable for use in dry-process electrodes. The preparation method comprises the following steps:

[0007] Utilizing a silane coupling agent to modify the surface of the conductive agent;

[0008] The modified conductive agent is co-coagulated with the fluorine-containing polymer to obtain a composite material;

[0009] The composite material is dried to obtain the composite conductive adhesive.

[0010] In one embodiment, the step of "surface-modifying the conductive agent using a silane coupling agent" further includes: adding the conductive agent and the silane coupling agent into a solvent to obtain a mixed solution, heating and refluxing the mixed solution, filtering and drying the mixed solution to obtain a modified conductive agent.

[0011] In one embodiment, the solvent includes one or more of anhydrous ethanol, butanone, n-hexane, and toluene, and the mass ratio of the solvent to the conductive agent is 0.5-10.

[0012] In one embodiment, the heating reflux temperature is 50° C. to 80° C., and the time is 0.5 h to 8 h.

[0013] In one embodiment, the step of "co-coagulating the modified conductive agent with the fluorine-containing polymer" further includes: diluting the fluorine-containing polymer with water, stirring evenly, adding the modified conductive agent, and co-coagulating.

[0014] One embodiment of the present application provides a composite conductive adhesive, which is suitable for use in dry electrodes. The composite conductive adhesive includes the following components by weight percentage: 24.8% to 88.7% of a fluorine-containing polymer; 11.2% to 75.1% of a conductive agent; and 0.01% to 2% of a silane coupling agent. The conductive agent is coated on the surface of the fluorine-containing polymer through the silane coupling agent.

[0015] In one embodiment, the composite conductive adhesive includes the following components by weight: 33.2% to 75.5% of fluorine-containing polymer; 24.4% to 66.7% of conductive agent; and 0.05% to 1% of silane coupling agent.

[0016] In one embodiment, the silane coupling agent includes one or more of vinyltrimethoxysilane, vinyltriethoxysilane, phenyltrimethoxysilane, diethylenetriaminopropyltrimethoxysilane, 3-(acryloxy)propyltrimethoxysilane, N-phenyl-3-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, γ-glycidyloxypropyltrimethoxysilane, γ-methacryloxypropyltrimethoxysilane, γ-mercaptopropyltrimethoxysilane, triethoxymethylsilane, and N-β-(aminoethyl)aminopropylmethyldimethoxysilane.

[0017] In one embodiment, the conductive agent includes one or more of carbon black, conductive graphite, graphene, carbon nanotubes, and carbon fibers.

[0018] In one embodiment, the fluorine-containing polymer includes one or more of polytetrafluoroethylene, tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer, hexafluoropropylene-tetrafluoroethylene copolymer, poly(ethylene-co-chlorotrifluoroethylene), poly(chlorotrifluoroethylene), and poly(ethylene-co-tetrafluoroethylene).

[0019] An embodiment of the present application provides an electrode sheet, which includes a current collector and a dry film sheet disposed on the surface of the current collector. The dry film sheet includes the composite conductive adhesive as described above.

[0020] An embodiment of the present application provides an electrochemical energy storage device, which includes the electrode plate as described above.

[0021] The preparation method of the present application realizes the uniform compounding of the conductive agent and the binder (fluoropolymer) on a microscopic scale, the surface of the fluoropolymer is uniformly coated with the conductive agent, the conductive agent and the fluoropolymer are tightly combined, the interaction between the two is strong, and the uniformity of the prepared composite conductive binder is greatly improved. Since co-coagulation can be achieved without the need to add additional flocculants in the preparation process, it can reduce the influence of the flocculant itself on the electrochemical performance of subsequent devices, simplify the process, and reduce production costs. In the process of making the electrode plate of the composite conductive binder of the present application, the conductive agent will be uniformly dispersed in the membrane along with the fiberization of the fluoropolymer, forming a uniform conductive network structure, thereby reducing the internal resistance of the plate. The electrode plate of the present application has a lower internal resistance. When it is applied to an electrochemical energy storage device (for example, a battery), the rate performance and cycle performance of the battery are better, and can meet the various comprehensive performance requirements of the battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 The present invention is a flow chart of a method for preparing a composite conductive adhesive according to an embodiment of the present application.

[0023] Figure 2 This is a scanning electron microscope image (10,000 times) of the composite conductive adhesive according to one embodiment of the present application.

[0024] Figure 3 This is a schematic diagram of the structure of an electrode plate according to one embodiment of the present application.

[0025] Figure 4 It is a schematic structural diagram of a battery according to one embodiment of the present application.

[0026] Figure 5 This is a scanning electron microscope image (10,000 times) of the composite conductive adhesive of Comparative Example 2 of the present application.

[0027] Main component symbols

[0028] 10: electrode plate; 11: current collector; 12: dry process membrane; 101: positive electrode plate; 102: negative electrode plate; 20: separator; 30: electrolyte; 100: battery.

[0029] The following specific implementation manner will further illustrate the embodiments of the present application in conjunction with the above-mentioned drawings. DETAILED DESCRIPTION

[0030] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the technical field belonging to the embodiments of the present application. The terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the embodiments of the present application. If specific conditions are not specified in the embodiments, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified in the reagents or instruments used, they are all conventional products that can be purchased commercially. The term "and / or" used herein includes all and any combination of one or more related listed items.

[0031] Some embodiments of the present application are described in detail below in conjunction with the accompanying drawings. In the absence of conflict, the following embodiments and features in the embodiments can be combined with each other.

[0032] See also Figure 1 In a first aspect, the present application provides a method for preparing a composite conductive adhesive, which is suitable for use in dry-process electrodes. The method for preparing the composite conductive adhesive includes steps S10 to S30.

[0033] Step S10, using a silane coupling agent to modify the surface of the conductive agent.

[0034] The structural formula of the silane coupling agent can be expressed as R-Si-X, where the R group is a functional group with affinity to the fluorine-containing polymer molecule (to be added in the subsequent steps), and the X group is a hydrolyzable group. After hydrolysis, the X group is easy to combine with the hydroxyl group on the surface of carbon (the conductive agent contains carbon). In this way, the conductive agent after surface modification by the silane coupling agent will be coated on the surface of the fluorine-containing polymer through the R group in the silane coupling agent during the subsequent co-coagulation process, forming a microscopic cross-linked network structure covering the entire surface. The dry electrode made of the conductive agent-silane coupling agent-fluorine-containing polymer composite material provides a continuous path for electron transmission under the action of the conductive agent, making electron transmission easier and significantly reducing the resistance of the electrode.

[0035] In some embodiments, the silane coupling agent may be, but is not limited to, vinyl trimethoxy silane (C5H 12 O3Si, CAS No.: 2768-02-7), vinyl triethoxysilane (C8H 18 O3Si, CAS No.: 78-08-0), phenyltrimethoxysilane (C9H 14 O3Si, CAS No.: 2996-92-1), diethylenetriaminepropyltrimethoxysilane (C 10 H 27 N3O3Si, CAS No.: 35141-30-1), 3-(acryloyloxy)propyltrimethoxysilane (C9H 18O5Si, CAS No.: 4369-14-6), N-phenyl-3-aminopropyltrimethoxysilane (C 12 H 21 NO3Si, CAS No.: 3068-76-6), N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane (C8H 22 N2O3Si, CAS No.: 1760-24-3, also known as silane coupling agent KH-792), γ-aminopropyltriethoxysilane (C9H 23 NO3Si, CAS No.: 919-30-2, also known as silane coupling agent KH-550), γ-glycidyloxypropyltrimethoxysilane (C9H 20 O5Si, CAS No.: 2530-83-8, also known as silane coupling agent KH-560), γ-methacryloxypropyltrimethoxysilane (C 10 H 22 O4Si, CAS No.: 2530-85-0, also known as silane coupling agent KH-570), γ-mercaptopropyltrimethoxysilane (C6H 16 O3SSi, CAS No.: 4420-74-0, also known as silane coupling agent KH-590), N-β-(aminoethyl)aminopropylmethyldimethoxysilane (C8H 22 N2O2Si, CAS No.: 3069-29-2, also known as silane coupling agent KH-602) Methyltriethoxysilane (C7H 18 O3Si, CAS No. 2031-67-6) or more.

[0036] Further, the silane coupling agent may be one or more of phenyltrimethoxysilane, diethylenetriaminopropyltrimethoxysilane, N-phenyl-3-aminopropyltrimethoxysilane, KH-602, KH-792 and KH-550.

[0037] In some embodiments, the conductive agent may be, but is not limited to, one or more of carbon black, conductive graphite, graphene, carbon nanotubes, and carbon fibers.

[0038] In some embodiments, the conductive agent can be modified by a wet method. Specifically, the conductive agent and the silane coupling agent can be added to a solvent to obtain a mixed solution, the mixed solution is heated and refluxed, filtered and dried to obtain a modified conductive agent. The solvent may be, but is not limited to, one or more of anhydrous ethanol, butanone, n-hexane, and toluene, preferably anhydrous ethanol. The mass ratio of the solvent to the conductive agent may be 0.5 to 10. The temperature of heating and reflux may be 50°C to 80°C, and the time may be 0.5h to 8h. The temperature of heating and reflux may be 50°C, 60°C, 70°C, 80°C, or any value between any two adjacent values ​​above, and the time may be 0.5h, 1h, 2h, 3h, 4h, 5h, 6h, 7h, 8h, or any value between any two adjacent values ​​above. Heating and reflux can provide a higher temperature and a longer reaction time. The reaction rate can be increased by heating, and the reaction process can be accelerated. At the same time, the reflux process can effectively reduce the loss and volatilization of the reactants. That is, heating and reflowing can make the silane coupling agent and the conductive agent react more fully.

[0039] In some embodiments, the conductive agent can be modified by a dry method. Specifically, the conductive agent and the silane coupling agent can be fully mixed by, but not limited to, strong mixing, ultrasonic stirring, etc. until the surface of the conductive agent is evenly coated with a silane coupling agent layer, thereby obtaining surface-modified conductive agent particles, which are dried and used for later use.

[0040] Step S20, co-coagulating the modified conductive agent and the fluorine-containing polymer to obtain a composite material.

[0041] In some embodiments, the fluorine-containing polymer may be, but is not limited to, one or more of polytetrafluoroethylene (PTFE), tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer (also known as fusible polytetrafluoroethylene, PFA), hexafluoropropylene-tetrafluoroethylene copolymer (FEP), poly(ethylene-co-chlorotrifluoroethylene) (ECTFE), poly(chlorotrifluoroethylene) (PCTFE), and poly(ethylene-co-tetrafluoroethylene) (ETFE). The above-mentioned fluorine-containing polymer can react with the aforementioned silane coupling agent to make the modified conductive agent co-coagulate with the fluorine-containing polymer.

[0042] Furthermore, the fluorine-containing polymer may be polytetrafluoroethylene and / or tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer.

[0043] In some embodiments, the fluorinated polymer (which can be synthesized by emulsion polymerization, and the obtained fluorinated polymer particles are generally suspended in a solution) can be diluted by adding a certain proportion of water, stirred evenly, and then the modified conductive agent is added for co-coagulation. In the present application, co-coagulation means that the fluorinated polymer latex particles and the inorganic particles are coagulated at the same time to form functionalized polymer particles (conductive agent-silane coupling agent-fluorinated polymer). The charge on the surface of the silane coupling agent neutralizes the charge on the surface of the fluorinated polymer latex particles, compressing the double electric layer on the surface of the latex particles, reducing the repulsive potential energy, and increasing the interaction force between the particles, so that the particles are coagulated to obtain solid granular polymer particles (conductive agent-silane coupling agent-fluorinated polymer). If the solvent (that is, water) becomes clear, it indicates that the co-coagulation is complete.

[0044] Furthermore, the mass ratio of the fluorinated polymer to water may be 1:(5-15). For example, the mass ratio of the fluorinated polymer to water may be 1:5, 1:6, 1:7, 1:8, 1:9, 1:10, 1:11, 1:12, 1:13, 1:14, 1:15, etc., which are not listed here one by one.

[0045] Step S30, drying the composite material to obtain the composite conductive adhesive.

[0046] In some embodiments, the drying method can be vacuum drying, blast drying and freeze drying. The drying temperature of vacuum drying and blast drying can be 80°C~150°C, and the time can be 8h~24h. For example, the drying temperature can be 80°C, 90°C, 100°C, 120°C, 150°C or any value between any two adjacent values ​​above, and the time can be 8h, 10h, 12h, 13h, 14h, 15h, 18h, 20h, 24h or any value between any two adjacent values ​​above. Further, it can be dried for 12h at a temperature of 120°C. The temperature of freeze drying is -40°C~-50°C, and the drying time is 24h-36h.

[0047] See also Figure 2In the second aspect of the present application, a composite conductive adhesive is provided by the above-mentioned preparation method. The composite conductive adhesive comprises the following components by weight percentage: 24.8% to 88.7% of fluorine-containing polymer, 11.2% to 75.1% of conductive agent, and 0.01% to 2% of silane coupling agent. Among them, the conductive agent is coated on the surface of the fluorine-containing polymer by the silane coupling agent. If the content of the conductive agent is too high, the bonding performance of the composite conductive adhesive prepared will be reduced; if the content of the conductive agent is too low, the conductivity of the dry-process membrane prepared is not good. If the content of the fluorine-containing polymer is too high, the conductivity of the dry-process membrane prepared is not good; if the content of the fluorine-containing polymer is too low, the co-coagulation effect is not good and the bonding effect is affected. If the content of the silane coupling agent is too high or too low, the coating effect will be affected, so that the conductive agent cannot be evenly coated on the surface of the fluorine-containing polymer. That is, each component is within the above-mentioned content range, which can not only ensure that the composite conductive adhesive has good conductivity and bonding properties at the same time, but also make the conductive agent evenly coated on the surface of the fluorine-containing polymer. In this way, when the dry diaphragm is formed later, the conductive agent can be evenly dispersed in the diaphragm along with the fiberization of the fluoropolymer (under the action of shear force, the fluoropolymer will be physically stretched from its original spherical shape into filaments, which is called "fiberization". The formed network structure can connect the active particles together, thereby achieving better bonding effect), forming a uniform conductive network structure, thereby reducing the internal resistance of the electrode.

[0048] In some embodiments, the composite conductive adhesive includes the following components by weight: 33.2% to 75.5% of fluorine-containing polymer, 24.4% to 66.7% of conductive agent, and 0.05% to 1% of silane coupling agent.

[0049] In some embodiments, the silane coupling agent may be, but is not limited to, one or more of vinyltrimethoxysilane, vinyltriethoxysilane, phenyltrimethoxysilane, diethylenetriaminopropyltrimethoxysilane, 3-(acryloxy)propyltrimethoxysilane, N-phenyl-3-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, γ-glycidyloxypropyltrimethoxysilane, γ-methacryloxypropyltrimethoxysilane, γ-mercaptopropyltrimethoxysilane, triethoxymethylsilane, and N-β-(aminoethyl)aminopropylmethyldimethoxysilane.

[0050] In some embodiments, the conductive agent may be, but is not limited to, one or more of carbon black, conductive graphite, graphene, carbon nanotubes, and carbon fibers.

[0051] In some embodiments, the fluorine-containing polymer may be, but is not limited to, one or more of polytetrafluoroethylene, tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer, hexafluoropropylene-tetrafluoroethylene copolymer, poly(ethylene-co-chlorotrifluoroethylene), poly(chlorotrifluoroethylene), and poly(ethylene-co-tetrafluoroethylene).

[0052] See also Figure 3 In a third aspect, the present application provides an electrode plate 10, which includes a current collector 11 and a dry film 12 disposed on the surface of the current collector 11. The electrode plate 10 can be a positive electrode plate or a negative electrode plate, and the present application does not limit it. It can be understood that when the electrode plate 10 is a positive electrode plate, the current collector is a positive electrode current collector, the dry film is a positive electrode film, and the positive electrode film includes the above-mentioned composite conductive adhesive and positive electrode active material; when the electrode plate 10 is a negative electrode plate, the current collector is a negative electrode current collector, the dry film is a negative electrode plate, and the negative electrode film includes the above-mentioned composite conductive adhesive and negative electrode active material. The positive electrode current collector can be made of aluminum foil. When the electrode plate 10 is used in a capacitor, carbon and resin can be provided on the aluminum foil. The positive electrode active material may be, but is not limited to, lithium cobalt oxide (LiCoO2), lithium nickel manganese cobalt ternary material (NCM), lithium nickel cobalt aluminum ternary material (NCA), lithium manganese oxide (LiMn2O4), lithium nickel manganese oxide (LiNi 0.5 Mn 1.5 O4), lithium iron phosphate (LiFePO4), lithium titanate (LTO), activated carbon, transition metal oxides (Na x MO2), polyanionic compounds (Na x M y (X a O b )Z w ), Prussian blue compounds (Na x M1[M2(CN)6] 1-y □ y ·nH2O(0≤x≤2,0≤y≤1)). The negative electrode current collector may be copper foil. When the electrode plate 10 is used in a capacitor, carbon and resin may be provided on the copper foil. The negative electrode active material may be, but is not limited to, activated carbon, graphite, soft carbon, hard carbon, carbon fiber, mesophase carbon microspheres, silicon-based materials, tin-based materials, and lithium titanate. Among them, graphite may be selected from a combination of one or more of artificial graphite, natural graphite, and modified graphite; silicon-based materials may be selected from a combination of one or more of elemental silicon, silicon oxide compounds, silicon-carbon composites, and silicon alloys; tin-based materials may be selected from a combination of one or more of elemental tin, tin oxide compounds, and tin alloys.

[0053] The dry process membrane can be made by the following steps: the positive electrode active material (negative electrode active material) and the composite conductive agent described in the present application are mixed evenly, and hot pressed by a roller press to obtain a positive electrode membrane (negative electrode membrane). The positive electrode membrane (negative electrode membrane) is placed on the positive electrode collector (negative electrode collector), and hot pressed to obtain an electrode sheet.

[0054] See also Figure 4 In a fourth aspect, the present application provides an electrochemical energy storage device 100, which may be, but not limited to, a battery and a capacitor. The battery may be, but not limited to, a lithium-ion battery, a sodium-ion battery, etc., and the capacitor may be, but not limited to, a supercapacitor, a lithium-ion capacitor, a hybrid capacitor, etc. Figure 4 The electrochemical energy storage device is a lithium-ion battery. Figure 4 As shown, the lithium-ion battery may include electrode sheets 10 (positive electrode sheet 101 , negative electrode sheet 102 ), a separator 20 and an electrolyte 30 .

[0055] The present application will be further described below in conjunction with specific embodiments and comparative examples.

[0056] Example 1

[0057] S10, add 0.01 g KH-550 (silane coupling agent), 6.67 g carbon black (conductive agent) and 84.5 mL anhydrous ethanol into a heating reflux device, the heating reflux temperature is 80 ° C, the time is 0.5 h, and the modified conductive agent is obtained after filtering and drying.

[0058] S20, diluting 3.32 g of PTFE (fluoropolymer) with 33.2 g of deionized water, stirring evenly, adding the modified conductive agent prepared in step S10, and co-coagulating to obtain a composite material.

[0059] S30, vacuum drying the composite material obtained in step S20 at a temperature of 120° C. for 18 h to obtain Figure 2 The composite conductive adhesive shown in the figure has a fluorine-containing polymer content of 33.2% by weight, a conductive agent content of 66.7% by weight, and a silane coupling agent content of 0.1% by weight.

[0060] like Figure 2 As shown, in the composite conductive adhesive, the conductive agent and the fluorine-containing polymer (binder) are uniformly compounded on a microscopic scale through a silane coupling agent, and the conductive agent particles are uniformly coated on the surface of the fluorine-containing polymer, so that the conductive agent and the fluorine-containing polymer are tightly combined, the interaction between the two is strong, and the uniformity of the composite material is greatly improved.

[0061] The positive electrode active material lithium nickel manganese cobalt ternary material (NCM) and the composite conductive binder prepared in Example 1 were homogeneously mixed in a weight ratio of 9:1, and hot-pressed by a roller press to prepare a dry film. The dry film was placed on an aluminum foil (current collector) and hot-pressed to obtain a positive electrode sheet. The volume resistivity of the dressing layer, i.e., the volume resistivity of the film, was tested using a Hoki electrode resistance test system.

[0062] The positive electrode sheet in Example 1 was assembled into a 2032 button cell, and its related electrochemical properties were tested.

[0063] The rate performance test method is as follows: charge to 4.3V at 0.1C constant current at room temperature, charge at 4.3V constant voltage to a current ≤0.02C, discharge to 3.0V at 0.1C, 1C and 3C constant currents respectively, cycle for 3 weeks at each discharge rate, record the discharge capacity of the battery in the third week at different discharge rates, and calculate the discharge capacity retention rate of the battery at 1C and 3C relative to 0.1C respectively.

[0064] The cycle performance test method is as follows: charge to 4.3V at 0.5C constant current at room temperature, charge at 4.3V constant voltage to a current ≤0.02C, discharge to 3.0V at 1C constant current, cycle 50 times, record the discharge capacity at different cycle numbers, and calculate the capacity retention rate of the battery after 50 cycles.

[0065] Example 2

[0066] S10, 0.005 g KH-792 (silane coupling agent), 4.995 g conductive graphite (conductive agent) and 60 mL anhydrous ethanol were added into a heating reflux device, the heating reflux temperature was 60°C, the time was 8 h, and the modified conductive agent was obtained after filtering and drying.

[0067] S20, diluting 5 g of PFA (fluoropolymer) with 50 g of deionized water, stirring evenly, adding the modified conductive agent prepared in step S10, and co-coagulating to obtain a composite material.

[0068] S30, drying the composite material obtained in step S20 by air blast at a temperature of 80°C for 20 hours to obtain a composite conductive adhesive. In the composite conductive adhesive, the weight percentage of the fluorine-containing polymer is 50%, the weight percentage of the conductive agent is 49.95%, and the weight percentage of the silane coupling agent is 0.05%.

[0069] The positive electrode active material lithium nickel manganese cobalt ternary material (NCM) and the composite conductive binder prepared in Example 2 were homogeneously mixed in a weight ratio of 9:1, and hot-pressed by a roller press to prepare a dry film. The dry film was placed on an aluminum foil (current collector) and hot-pressed to obtain a positive electrode sheet. The volume resistivity of the dressing layer, i.e., the volume resistivity of the film, was tested using a Hoki electrode resistance test system.

[0070] The positive electrode sheet in Example 2 was assembled into a 2032 button-type battery, and the rate performance and cycle performance of the battery were tested according to the test method described in Example 1.

[0071] Example 3

[0072] S10, 0.01 g KH-602 (silane coupling agent), 2.44 g carbon nanotubes (conductive agent) and 30 mL anhydrous ethanol were added into a heating reflux device, the heating reflux temperature was 60 ° C, the time was 5 h, and the modified conductive agent was obtained after filtering and drying.

[0073] S20, diluting 7.55 g of PTFE (fluoropolymer) with 75.5 g of deionized water, stirring evenly, adding the modified conductive agent obtained in step S10, and co-coagulating to obtain a composite material.

[0074] S30, freeze-drying the composite material obtained in step S20 at a drying temperature of -40°C for 24 hours to obtain a composite conductive adhesive. In the composite conductive adhesive, the weight percentage of the fluorine-containing polymer is 75.5%, the weight percentage of the conductive agent is 24.4%, and the weight percentage of the silane coupling agent is 0.1%.

[0075] The positive electrode active material lithium nickel manganese cobalt ternary material (NCM) and the composite conductive binder in Example 3 were homogeneously mixed in a weight ratio of 9:1, and hot-pressed by a roller press to prepare a dry film. The dry film was placed on an aluminum foil (current collector) and hot-pressed to obtain a positive electrode sheet. The volume resistivity of the dressing layer, i.e., the volume resistivity of the film, was tested using a Hoki electrode resistance test system.

[0076] The positive electrode sheet in Example 3 was assembled into a 2032 button-type battery, and the rate performance and cycle performance of the battery were tested according to the test method described in Example 1.

[0077] Example 4

[0078] S10, 0.1 g of phenyltrimethoxysilane (silane coupling agent), 1.12 g of graphene (conductive agent) and 84.5 mL of anhydrous ethanol were added into a heating reflux device, the heating reflux temperature was 80°C, the time was 0.5 h, and the modified conductive agent was obtained after filtering and drying.

[0079] S20, diluting 8.78 g of PTFE (fluoropolymer) with 33.2 g of deionized water, stirring evenly, adding the modified conductive agent obtained in step S10, and co-coagulating to obtain a composite material.

[0080] S30, vacuum drying the composite material obtained in step S20 at a temperature of 120° C. for 18 h to obtain Figure 2 The composite conductive adhesive shown in the figure has a fluorine-containing polymer of 87.8% by weight, a conductive agent of 11.2% by weight, and a silane coupling agent of 1% by weight.

[0081] The positive electrode active material lithium nickel manganese cobalt ternary material (NCM) and the composite conductive binder in Example 4 were homogeneously mixed in a weight ratio of 9:1, and hot-pressed by a roller press to prepare a dry film. The dry film was placed on an aluminum foil (current collector) and hot-pressed to obtain a positive electrode sheet. The volume resistivity of the dressing layer, i.e., the volume resistivity of the film, was tested using a Hoki electrode resistance test system.

[0082] The positive electrode sheet in Example 4 was assembled into a 2032 button-type battery, and the rate performance and cycle performance of the battery were tested according to the test method described in Example 1.

[0083] Comparative Example 1

[0084] S10, add 0.3 g KH-550 (silane coupling agent), 0.2 g carbon black (conductive agent) and 84.5 mL anhydrous ethanol into a heating reflux device, the heating reflux temperature is 80 ° C, the time is 0.5 h, and the modified conductive agent is obtained after filtering and drying.

[0085] S20, diluting 9.5 g of PTFE (fluoropolymer) with 95 g of deionized water, stirring evenly, adding the modified conductive agent obtained in step S10, and co-coagulating to obtain a composite material.

[0086] S30, vacuum drying the composite material obtained in step S20 at a drying temperature of 120°C for 18 hours to obtain a composite conductive adhesive. In the composite conductive adhesive, the weight percentage of the fluorine-containing polymer is 80%, the weight percentage of the conductive agent is 18%, and the weight percentage of the silane coupling agent is 2%.

[0087] The positive electrode active material lithium nickel manganese cobalt ternary material (NCM) and the composite conductive binder prepared in comparative example 1 were ball-milled and mixed in a weight ratio of 9:1, heated and sheared, and hot-pressed by a roller press to prepare a dry film. The dry film was placed on an aluminum foil (current collector) and hot-pressed to obtain a positive electrode sheet. The volume resistivity of the dressing layer, i.e., the volume resistivity of the film, was tested using a Hoki electrode resistance test system.

[0088] The positive electrode sheet in Comparative Example 1 was assembled into a 2032 button-type battery, and the rate performance and cycle performance of the battery were tested according to the test method described in Example 1.

[0089] Comparative Example 2

[0090] The difference from Example 1 is that step S10 is omitted, and steps S20 and S30 are directly performed. That is, the conductive agent is directly co-coagulated with the fluorine-containing polymer, and after drying, the following is obtained: Figure 5 The composite conductive adhesive shown.

[0091] Figure 5 In the composite conductive adhesive shown, the conductive agent is randomly dispersed on the surface of the fluorine-containing polymer, and the distribution of the conductive agent is very uneven.

[0092] The positive electrode active material lithium nickel manganese cobalt ternary material (NCM) and the composite conductive binder prepared in comparative example 1 were homogeneously mixed in a weight ratio of 9:1, and hot-pressed by a roller press to prepare a dry film. The dry film was placed on an aluminum foil (current collector) and hot-pressed to obtain a positive electrode sheet. The volume resistivity of the dressing layer, i.e., the volume resistivity of the film, was tested using a Hoki electrode resistance test system.

[0093] The positive electrode sheet in Example 1 was assembled into a 2032 button-type battery, and the rate performance and cycle performance of the battery were tested according to the test method described in Example 1.

[0094] Comparative Example 3

[0095] 6.67 g of carbon black (conductive agent) was directly mixed with 3.32 g of PTFE (fluoropolymer) to obtain a mixed conductive adhesive.

[0096] The positive electrode active material lithium nickel manganese cobalt ternary material (NCM) and the mixed conductive binder prepared in comparative example 2 were homogeneously mixed in a weight ratio of 9:1, and hot-pressed by a roller press to prepare a dry film. The dry film was placed on an aluminum foil (current collector) and hot-pressed to obtain a positive electrode sheet. The volume resistivity of the dressing layer, i.e., the volume resistivity of the film, was tested using a Hoki electrode resistance test system.

[0097] The positive electrode sheet in Example 2 was assembled into a 2032 button-type battery, and the rate performance and cycle performance of the battery were tested according to the test method described in Example 1.

[0098] The component parameters of the above embodiments and comparative examples are shown in Table 1, and the performance test results of the above embodiments and comparative examples are shown in Table 2.

[0099] Table 1

[0100]

[0101] Table 2

[0102]

[0103] As can be seen from Table 2, the volume resistivity of the diaphragms of Examples 1 to 4 of the present application is much lower than that of the diaphragms of Comparative Examples 1 to 3, indicating that the composite conductive adhesive prepared in the present application makes the electrode have a lower internal resistance. The battery discharge gram capacity of the button batteries of Examples 1 to 4 of the present application at 0.1C / 1C / 3C rates is much higher than that of the battery discharge gram capacity of Comparative Examples 1 to 3, and the discharge capacity retention rate of 1C and 3C relative to 0.1C and the capacity retention rate after 50 cycles are also much higher than those of Comparative Examples 1 to 3. It can be seen that the rate performance and cycle performance of the button batteries of Examples 1 to 4 of the present application are better than those of Comparative Examples 1 to 3, indicating that the composite conductive adhesive prepared in the present application can improve the rate performance and cycle performance of the battery, and make the battery have long-term reliability.

[0104] The preparation method of the present application realizes the uniform compounding of the conductive agent and the binder (fluoropolymer) on a microscopic scale, the surface of the fluoropolymer is uniformly coated with the conductive agent, the conductive agent and the fluoropolymer are tightly combined, the interaction between the two is strong, and the uniformity of the prepared composite conductive binder is greatly improved. Since co-coagulation can be achieved without the need to add additional flocculants in the preparation process, it can reduce the influence of the flocculant itself on the electrochemical performance of subsequent devices, simplify the process, and reduce production costs. In the process of making the electrode plate of the composite conductive binder of the present application, the conductive agent will be uniformly dispersed in the membrane along with the fiberization of the fluoropolymer, forming a uniform conductive network structure, thereby reducing the internal resistance of the plate. The electrode plate of the present application has a lower internal resistance. When it is applied to an electrochemical energy storage device (for example, a battery), the rate performance and cycle performance of the battery are better, and can meet the various comprehensive performance requirements of the battery.

[0105] The above descriptions are some specific implementations of the present application, but they are not limited to these implementations in actual application. For ordinary technicians in this field, other variations and changes made according to the technical concept of the present application should all fall within the protection scope of the present application.

Claims

1. A method for preparing a composite conductive adhesive, wherein the composite conductive adhesive is suitable for use in dry-process electrodes, characterized in that: The preparation method comprises the following steps: Adding a conductive agent and a silane coupling agent into a solvent to obtain a mixed solution, heating the mixed solution to reflux, filtering and drying to obtain a modified conductive agent; The modified conductive agent is co-coagulated with the fluorine-containing polymer to obtain a composite material; Drying the composite material to obtain the composite conductive adhesive; The conductive agent is coated on the surface of the fluorinated polymer through the silane coupling agent, and the silane coupling agent includes vinyl trimethoxy silane, vinyl triethoxy silane, phenyl trimethoxy silane, diethylene triamino propyl trimethoxy silane, 3-(acryloxy) propyl trimethoxy silane, N-phenyl-3-aminopropyl trimethoxy silane, N-β-(aminoethyl)-γ-aminopropyl trimethoxy silane, γ-aminopropyl triethoxy silane, γ-glycidyloxy propyl trimethoxy silane, γ-methacryloxy propyl The conductive agent includes one or more of carbon black, conductive graphite, graphene, carbon nanotubes, and carbon fibers; the fluorine-containing polymer includes one or more of polytetrafluoroethylene, tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer, hexafluoropropylene-tetrafluoroethylene copolymer, poly(ethylene-co-chlorotrifluoroethylene), poly(chlorotrifluoroethylene), and poly(ethylene-co-tetrafluoroethylene); The composite conductive adhesive comprises the following components by weight percentage: Fluorinated polymers 24.8%~88.7%; Conductive agent 11.2%~75.1%; Silane coupling agent 0.01%~2%.

2. The preparation method according to claim 1, characterized in that The solvent includes one or more of anhydrous ethanol, butanone, n-hexane, and toluene, and the mass ratio of the solvent to the conductive agent is 0.5-10.

3. The preparation method according to claim 1, characterized in that: The heating reflux temperature is 50° C. to 80° C., and the time is 0.5 h to 8 h.

4. The preparation method according to claim 1, characterized in that: The step of "co-coagulating the modified conductive agent with the fluorine-containing polymer" further includes: diluting the fluorine-containing polymer with water, stirring evenly, adding the modified conductive agent, and co-coagulating.

5. A composite conductive binder, which is suitable for use in dry-process electrodes, characterized in that: The composite conductive adhesive is prepared by the preparation method according to any one of claims 1 to 4, and the composite conductive adhesive comprises the following components by weight percentage: Fluorinated polymers 24.8%~88.7%; Conductive agent 11.2%~75.1%; Silane coupling agent 0.01%~2%; The conductive agent is coated on the surface of the fluorinated polymer through the silane coupling agent, and the silane coupling agent includes vinyl trimethoxy silane, vinyl triethoxy silane, phenyl trimethoxy silane, diethylene triamino propyl trimethoxy silane, 3-(acryloxy) propyl trimethoxy silane, N-phenyl-3-aminopropyl trimethoxy silane, N-β-(aminoethyl)-γ-aminopropyl trimethoxy silane, γ-aminopropyl triethoxy silane, γ-glycidyloxy propyl trimethoxy silane, γ-methacryloxy propyl The conductive agent comprises one or more of carbon black, conductive graphite, graphene, carbon nanotubes, and carbon fibers; the fluorine-containing polymer comprises one or more of polytetrafluoroethylene, tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer, hexafluoropropylene-tetrafluoroethylene copolymer, poly(ethylene-co-chlorotrifluoroethylene), poly(chlorotrifluoroethylene), and poly(ethylene-co-tetrafluoroethylene).

6. The composite conductive adhesive according to claim 5, characterized in that: The composite conductive adhesive comprises the following components by weight percentage: Fluorinated polymers 33.2%~75.5%; Conductive agent 24.4%~66.7%; Silane coupling agent 0.05%~1%.

7. An electrode plate, characterized in that: The invention comprises a current collector and a dry film arranged on the surface of the current collector, wherein the dry film comprises the composite conductive adhesive as claimed in claim 5 or 6.