Carbon nitride / bismuth oxybromide / carbon quantum dot photocatalysts, their preparation methods, and applications
By preparing red and blue light-emitting carbon quantum dots derived from tea leaves and combining them with carbon nitride/bismuth oxybromine, the problem of low photocatalytic efficiency was solved, achieving highly efficient photocatalytic degradation of organic pollutants and broadening the application of biomass materials in the environmental field.
Patent Information
- Application Number
- CN202310881573.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-07-18
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-07-18
AI Technical Summary
Existing photocatalysts suffer from low catalytic efficiency, high electron-hole recombination rate, and poor band structure when degrading organic pollutants. In particular, graphitic carbon nitride materials have small specific surface areas for photogenerated electrons and holes and high recombination rates, which limits their application.
Using biomass tea leaves as raw material, a composite of tea-derived red and blue light emitting carbon quantum dots and carbon nitride/bismuth oxybromine was prepared. Through hydrothermal treatment and ultrasonic exfoliation, a carbon nitride/bismuth oxybromine/carbon quantum dot photocatalyst was formed, which improved the separation of photogenerated carriers and the band structure.
It achieves highly efficient photocatalytic degradation of organic pollutants, significantly improves the specific surface area and electron transfer performance of the catalyst, reduces the recombination rate of electrons and holes, and enhances photocatalytic performance.
Smart Images

Figure CN118454712B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of preparation technology of biomass carbon quantum dot composite bismuth bromide / graphite phase carbon nitride type photocatalysts, and more specifically to carbon nitride / bismuth oxybromide / carbon quantum dot photocatalysts, their preparation methods and applications. Background Technology
[0002] Organic pollutants (volatile organic compounds, dyes, antibiotics, etc.) are characterized by their diversity, high yield, and wide distribution, making them difficult to remove effectively. Traditional adsorption, thermocatalysis, and ozone oxidation methods suffer from incomplete removal and cumbersome operation. Therefore, semiconductor heterojunction photocatalysis has attracted widespread attention due to its simple and efficient degradation method. However, the accumulation of organic pollutants on the catalyst surface, the high electron-hole recombination rate during catalysis, and the influence of band structure typically result in poor catalytic efficiency. Therefore, modification of heterojunction photocatalytic materials is crucial. Graphitic carbon nitride (C3N4) is a two-dimensional non-metallic semiconductor material. Compared with other semiconductor photocatalysts, C3N4 possesses a moderate band structure (2.7 eV-2.8 eV), a good visible light absorption range, and excellent physicochemical properties, showing potential applications in photocatalysis. However, the small specific surface area and high recombination rate of photogenerated electrons and holes in C3N4 limit its further applications. To address these issues, ultrasonic exfoliation can be used to obtain ultrathin g-C3N4 nanosheets to improve the separation of photogenerated carriers. Alternatively, it can form heterojunction structures with other semiconductors to improve the band structure of the material. Currently, C3N4 / CeO2, C3N4 / NiCo2O4, and C3N4 / CoSe2 have been reported and widely used in organic degradation, carbon dioxide reduction, and water splitting for hydrogen production.
[0003] In recent years, bismuth oxyhalides (BiOX, X = Cl, Br, and I) have attracted much attention due to their unique tetragonal layered structure and indirect band gap. This facilitates the separation of photogenerated electrons and holes between electrostatic layers, which has garnered significant interest in the photocatalytic degradation of organic pollutants in water. For example, Fangfang Duo obtained N-CQDs using D-glucose and ethylenediamine as carbon sources. They then successfully synthesized CQDs / BiOBr by mixing CQDs / BiOBr in a solution of BiOBr precursors. The upconversion effect of CQDs refreshes oxygen vacancies on BiOBr, thus maintaining the photocatalytic stability of BiOBr. The catalyst achieved a photocatalytic degradation efficiency of over 90% for Rhodamine B (RhB) and bisphenol A (BPA) within 20 minutes.
[0004] Biomass-derived carbon is a material prepared from biomass and can be classified into activated carbon, hydrothermal carbon, carbon quantum dots, activated carbon fibers, etc. Carbon quantum dots, as a special type of material, possess excellent upconversion luminescence and control over the band structure of catalysts. For example, Yang Hao used cellulose as a carbon source to prepare carbon dots. The synthesized g-C3N4 / C-140 p-phenol (10 mg / L) -1 The removal rate of carbamazepine reached 83%, three times that of the original g-C3N4. However, a drawback is the lack of utilization of hydrothermal residues. Xiaoyun Xi prepared carbon quantum dots from corn cob biomass, synthesized Fe3O4 / BiOBr / CQDs photocatalysts via photodeposition, and rationally utilized hydrothermal residues to synthesize Fe3O4 / BiOBr / HC photocatalysts. Experimental results showed that both materials achieved a carbamazepine removal rate of over 95% under visible light. Typically, carbon quantum dots produced by direct hydrothermal synthesis from biomass mainly emit blue light, but there is a lack of reports on the application of red-emitting carbon dots in the field of photocatalysis. Therefore, providing a method for preparing red and blue bicolor carbon dots from biomass and their photocatalytic application has become an urgent technical problem to be solved in this field. Summary of the Invention
[0005] To address the above problems, this invention provides carbon nitride / bismuth oxybromide / carbon quantum dot photocatalysts, their preparation methods, and applications. Tea-derived red-emitting carbon dots / carbon nitride / bismuth oxybromide and tea-derived blue-emitting carbon dots / carbon nitride / bismuth oxybromide were prepared.
[0006] The first objective of this invention is to provide a method for preparing a carbon nitride / bismuth oxybromide / carbon quantum dot photocatalyst, comprising the following steps:
[0007] Step 1: Using ethanol as a solvent, perform Soxhlet extraction on tea powder. After extraction, solution A and residue A are obtained.
[0008] Step 2: The supernatant after centrifugation of solution A is subjected to hydrothermal treatment at 150-180℃ to obtain solution B. Solution B is then post-processed to obtain tea-derived red light emitting carbon quantum dots.
[0009] Step 3: Using water as a solvent and ethylenediamine as a passivating agent, add residue A and perform hydrothermal treatment at 180-200℃ to obtain solution C. Then, perform post-treatment on solution C to obtain tea-derived blue light emitting carbon quantum dots.
[0010] Step 4: Add carbon nitride, bismuth nitrate pentahydrate, and tea-derived red-emitting carbon quantum dots or tea-derived blue-emitting carbon quantum dots to ethylene glycol, and sonicate to obtain solution D. Dissolve potassium bromide and sodium hydroxide in water, and sonicate to obtain solution E. Add solution E dropwise to solution D, stir and mix evenly, and let stand for 2-6 hours to obtain carbon nitride / bismuth oxybromide or tea-derived blue-emitting carbon dots / carbon nitride / bismuth oxybromide.
[0011] A second objective of this invention is to provide a carbon nitride / bismuth oxybromide / carbon quantum dot photocatalyst prepared by the above method.
[0012] A third objective of this invention is to provide the application of the aforementioned carbon nitride / bismuth oxybromide / carbon quantum dot photocatalyst in the photocatalytic degradation of organic pollutants.
[0013] Compared with the prior art, the present invention has the following beneficial effects:
[0014] This invention uses tea leaves as raw material, providing tea-derived red-emitting carbon quantum dots and tea-derived blue-emitting carbon quantum dots, and further obtaining tea-derived active hydrothermal carbon, realizing comprehensive utilization from raw materials to residues, and broadening the application of biomass materials in the environmental field. This is an original innovation in the field of developing pure biomass carbon materials. Furthermore, the tea-derived carbon quantum dot-supported carbon nitride / bismuth oxybromine provided by this invention is a low-cost, biocompatible, and highly efficient novel photocatalyst. It has many advantages such as simple preparation method and environmental friendliness, and has significant affinity and photocatalytic performance for organic pollutants. It represents a new starting point for the high-value utilization of waste biomass resources and is widely applicable to the treatment of industrial organic pollution. The tea-derived carbon quantum dot-supported carbon nitride / bismuth oxybromine provided in this invention has extremely significant catalytic performance against organic pollutants, especially the innovative application of red-emitting carbon quantum dots in photocatalysis. Compared with traditional catalysts, the addition of red-emitting carbon quantum dots has excellent advantages in band structure modulation and electron transfer. Attached Figure Description
[0015] Figure 1 The flowchart shows the preparation process of RCD and BCD (Figure a), CN (Figure b), and carbon nitride / bismuth oxybromide / carbon quantum dot photocatalyst (Figure c) in this invention.
[0016] Figure 2 The images shown are: a photograph of the CDs solution of Example 1 of the present invention under 365 nm irradiation (Figure a), a UV-Vis absorption curve of CDs (Figure b), a Fourier transform infrared spectrum of CDs (Figure c), a fluorescence emission spectrum (Figure d), a TEM image of RCD (Figure e), and a TEM image of BCD (Figure f).
[0017] Figure 3The X-ray diffraction pattern (a), fluorescence excitation spectrum (b), three-dimensional fluorescence spectrum of RCD (c), and three-dimensional spectrum of BCD (d) are shown in Embodiment 1 of the present invention.
[0018] Figure 4 The images show the lattice fringes of red-emitting carbon quantum dots (Figure a) and blue-emitting carbon quantum dots (Figure b) of Embodiment 1 of the present invention.
[0019] Figure 5 Figure 1 shows the scanning electron microscope (SEM) images of tea hydrothermal activated carbon with a scale bar of 30 μm (Figure 1a), the scanning electron microscope (SEM) images of tea hydrothermal activated carbon with a scale bar of 5 μm (Figure 1b), the Fourier transform infrared spectrum (Figure 1c), and the adsorption curve of 20 mg tea hydrothermal activated carbon on 100 mL of 30 mg / L HRB (25 °C, pH = 7) (Figure 1d).
[0020] Figure 6 These are photographs of catalyst samples R4, B1, and comparative examples 1-3 of the present invention;
[0021] Figure 7 The SEM images of (a) SCN, (b) BiOBr, and (c) CN / BiOBr of Embodiment 2 of the present invention are shown below.
[0022] Figure 8 The images show the scanning electron microscope (a), transmission electron microscope (b), and lattice fringe pattern (c) of R4; the scanning electron microscope (d), transmission electron microscope (e), and lattice fringe pattern (f) of B1; elemental mapping images of O (g), Bi (h), Br (i), and S (j) of R4; elemental mapping images of O (k), Bi (l), Br (m), and S (n) of B1; and the N2 adsorption-desorption isotherm (o).
[0023] Figure 9 The scan images of R4 (image a) and the mapped scan images of C (image b), N (image c), and Mg (image d) are shown, along with the scan images of B1 (image e) and the mapped scan images of C (image f), N (image g), and Mg (image h).
[0024] Figure 10 The EDS spectral data for R4 (Figure a) and B1 (Figure b) of this invention are shown below.
[0025] Figure 11 Pore size distribution diagrams for R4, B1, and CN / BiOBr;
[0026] Figure 12 The full XPS spectrum for R4 and B1;
[0027] Figure 13XPS peaks for R4 and B1 catalysts: C1s (Figure a), Bi4f (Figure b); S2P (Figure c); O1s (Figure d); N1s (Figure e) and XPS valence band spectrum (Figure f);
[0028] Figure 14 The X-ray diffraction pattern (a), Fourier transform infrared spectrum (b), UV-Vis DRS reflectance spectrum (c), band structure diagrams of CN, BiOBr, CN / BiOBr (d), R4 (e), and B1 (f), PL spectrum (g), transient photocurrent spectrum (h), and electrochemical impedance spectrum of the catalyst are shown in Figure 1.
[0029] Figure 15 Mott-Schottky plots for CN (Figure a), BiOBr (Figure b), CN / BiOBr (Figure c), R4 (Figure d), and B1 (Figure e), and the relationship between the converted Kubelka-Munk function and the CN light energy (Figure f);
[0030] Figure 16 Figure 1 shows the electron spin trapping (ESR) spectrum of R4, where DMPO is dispersed in water for hydroxyl radicals (Figure a) and distributed in methanol for superoxide radicals (Figure b); radical trapping experiment (Figure c); reaction mechanism of R4 (Figure d);
[0031] Figure 17 Figure 1 shows the photocatalytic degradation curves (a) and pseudo-first-order kinetic curves (b) of R1-R5, the photocatalytic degradation curves (c) and pseudo-first-order kinetic curves (d) of R1-R5, and the degradation curves of RhB (e) and tetracycline (f) at R4.
[0032] Figure 18 Figure 1 shows the degradation curves (a) and pseudo-first-order kinetic curves (b) for CN, BiOBr, CN / BiOBr, R4, and B1; degradation curves for different dosages (c), concentrations of organic pollutants (d), and pH (e); and the degradation curve of Rhb by the catalyst under a 300W Xe lamp (f).
[0033] Figure 19 Figure 1 shows the changes on the sample surface before and after the catalytic reaction (Figure 2), the photocatalytic degradation cycle curve of RhB by R4 (Figure 2), the Fourier transform infrared spectrum of the sample before and after the reaction (Figure 2), and the X-ray diffraction pattern (Figure 2).
[0034] Figure 20The high-performance liquid chromatography (HPLC) chromatogram (A-1) and mass spectrum (MS) of the R4 catalyst for RhB photocatalytic degradation at 0 min (retention time 9.52 ppm, A-2 ppm); the HPLC chromatogram (B-1) and MS spectrum (B-2 ppm) at 10 min (retention time 7.70 ppm, B-2 ppm); and the HPLC chromatogram (C-1) and MS spectrum (C-2 ppm) at 20 min (retention time 7.72 ppm, B-2 ppm).
[0035] Figure 21 This study focuses on intermediates of RhB and their potential photocatalytic degradation pathways. Detailed Implementation
[0036] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0037] The tea leaves can be black tea, white tea, or green tea; the tea leaves used in this invention are green tea (Tieguanyin). This invention provides a method for preparing a carbon nitride / bismuth oxybromide / carbon quantum dot photocatalyst, the preparation flow chart of which is shown below. Figure 1 As shown. This invention uses Tieguanyin tea as raw material, which is pulverized and then subjected to Soxhlet extraction with ethanol. Soxhlet extraction is used to extract abundant tea polyphenols and a small amount of chlorophyll from the tea leaves. The solution A after Soxhlet extraction is subjected to hydrothermal treatment to synthesize tea-derived red-emitting carbon quantum dots from the bottom up. Then, the residue A after Soxhlet extraction is subjected to hydrothermal treatment to synthesize tea-derived blue-emitting carbon quantum dots from the top down. Using residue A as raw material, ethylenediamine and a certain amount of aqueous solution are added, and tea-derived blue-emitting carbon quantum dots are synthesized by high-temperature hydrothermal treatment. Ethylenediamine acts as a passivating agent on the surface of the carbon quantum dots, effectively improving the fluorescence performance of the tea-derived blue-emitting carbon quantum dots. Figure 1 (Figure a). Meanwhile, residue B generated during the preparation of tea-derived blue-emitting carbon quantum dots is further activated at high temperature to prepare tea-active hydrothermal carbon. After high-temperature treatment with potassium hydroxide, residue B generates numerous mesopores, which facilitate the adsorption of organic pollutants. Using tea-derived red-emitting or blue-emitting carbon quantum dots as raw materials, a highly efficient photocatalytically responsive composite catalyst is obtained by loading it into a carbon nitride / bismuth oxybromine heterojunction system. Figure 1 The b-image and Figure 1(See Figure c). The composite catalyst prepared in this invention significantly increases the specific surface area of the catalyst with carbon quantum dots, exposing more active sites. Furthermore, the introduction of carbon quantum dots greatly improves the band structure of the catalyst, making it more conducive to light absorption and thus promoting photocatalytic reactions. Simultaneously, the trace amounts of Mg contained in the carbon quantum dots give them superior electron transfer performance, reducing electron-hole recombination and further promoting photocatalytic reactions.
[0038] Example 1 This example provides a method for preparing tea-derived carbon quantum dots with different fluorescence emission and tea-derived hydrothermal activated carbon, which includes the following steps:
[0039] 10.00 g of green tea powder was weighed and extracted with 300 mL of ethanol solution at 90 °C using a Soxhlet extractor for 18 h. The resulting solution A was centrifuged at 10,000 rpm to obtain the supernatant. 60 mL of the supernatant was placed in a 100 mL Teflon reactor and reacted at 160 °C for 4 h. After cooling, the mixture was centrifuged at 10,000 rpm and filtered through a 0.22 μm filter membrane to obtain solution B (i.e., carbon dot solution). The carbon dot solution was separated and freeze-dried to obtain tea-derived red-emitting carbon quantum dots (RCDs). 3.00 g of the upper tea residue (residue A), 0.5 mL of ethylenediamine, and 60 mL of distilled water were placed in a 100 mL beaker and stirred for 30 min. The mixture was then transferred to a polytetrafluoroethylene reactor and reacted at 180 °C for 12 h. After cooling to room temperature, the hydrothermal product was extracted and washed with water and ethanol solution until the filtrate was colorless. The upper residue B will be used for further reactions. The lower layer solution C was concentrated by rotary evaporation, centrifuged at 10,000 rpm for 10 minutes, and the supernatant was filtered through a 0.22 μm aqueous filter and dialyzed in a 500-day dialysis bag for 2 days. The solution was then concentrated and freeze-dried to obtain tea-derived blue light-emitting carbon quantum dots (BCD).
[0040] In addition, hydrothermal carbon was prepared by activating the residual B (denoted as HTC) from the preparation of blue light emitting carbon quantum dots with high-temperature KOH. A certain amount of the residue and potassium hydroxide were weighed in a beaker, 30 mL of distilled water was added, and the mixture was stirred for 30 min, then dried under vacuum at 105 °C. The product was calcined in a tube furnace at 800 °C for 2 h under N2 atmosphere at a heating rate of 5 °C / min. After cooling, the product was removed and washed sequentially with 0.5 M HCl and distilled water until neutral, and then dried at 105 °C to obtain tea-activated hydrothermal carbon. The tea-activated hydrothermal carbon prepared with 1 g of residue and 1 g of potassium hydroxide was named HTC-1; the tea-activated hydrothermal carbon prepared with 1 g of residue and 2 g of potassium hydroxide was named HTC-2; and the tea-activated hydrothermal carbon prepared with 1 g of residue and 3 g of potassium hydroxide was named HTC-3.
[0041] Example 2 This example provides a method for preparing a tea-derived carbon quantum dot photocatalyst supported on carbon nitride / bismuth oxybromide, which includes the following steps:
[0042] Weigh 5g of melamine and 5g of thiourea into 40mL of methanol solution. Stir for 20min and dry at 60℃. Place the mixture in an alumina crucible covered with aluminum foil and react at 550℃ for 4h, with a heating rate of 2.5℃ / min. Then allow to cool naturally, remove the product, and grind it until no particles remain. The sample is named SCN.
[0043] First, 0.136 g SCN, 1.58 g Bi(NO3)3, and the RCD prepared in Example 1 (RCD added at 5% of the total mass of SCN, Bi(NO3)3, and ethylene glycol) were placed in 40 mL of ethylene glycol solution and sonicated for 3 h. The resulting mixture was named solution A. Simultaneously, 0.476 g KBr and 0.16 g NaOH were dissolved in 20 mL of distilled water and sonicated for 3 h. This solution was then added dropwise to solution A. The solution was stirred for 30 min, allowed to stand for 4 h, and then centrifuged repeatedly at 10000 rpm with water and ethanol, and dried at 105 °C. The resulting tea-derived red-emitting carbon dot / carbon nitride / bismuth oxybromide was named R1.
[0044] The preparation methods of R2, R3, and R4 differ from those of R1 prepared in Example 2 only in that the amount of RCD added is 10%, 15%, and 20% of the total mass of SCN, Bi(NO3)3, and ethylene glycol, respectively.
[0045] The preparation methods of B1 and B2 differ from those of R1 prepared in Example 2 only in that RCD is replaced with BCD, and the amount of BCD added is 5% and 10% of the total mass of SCN, Bi(NO3)3 and ethylene glycol, respectively.
[0046] Example 3 This example provides a method for preparing tea-derived carbon quantum dots with different fluorescence emission and tea-derived hydrothermal activated carbon, which includes the following steps:
[0047] 20.00 g of green tea powder was weighed and extracted with 300 mL of ethanol solution at 80 °C using a Soxhlet extractor for 20 h. The upper tea residue (residue A) was used for further reaction. After extraction, solution A was centrifuged at 10000 rpm to obtain the supernatant. 60 mL of the supernatant was placed in a 100 mL Lflon reactor and reacted at 150 °C for 8 h. After cooling, the mixture was centrifuged at 10000 rpm and filtered through a 0.22 μm filter membrane to obtain solution B (i.e., carbon dot solution). The carbon dot solution was separated and freeze-dried to obtain tea-derived red-emitting carbon quantum dots (RCDs).
[0048] Take 4.00 g of residue A, 1 mL of ethylenediamine, and 60 mL of distilled water, place them in a 100 mL beaker, stir for 30 min, then transfer to a polytetrafluoroethylene reactor and react at 190 °C for 14 h. After cooling to room temperature, extract the hydrothermal product, wash with water and ethanol solutions until the filtrate is colorless, and use the upper residue B for further reactions. The lower solution C is concentrated by rotary evaporation, centrifuged at 10,000 rpm for 10 min, and the supernatant is filtered through a 0.22 μm aqueous filter and dialyzed in a 500 D dialysis bag for 2 days. After concentration, the solution is freeze-dried to obtain tea-derived blue light-emitting carbon quantum dots (BCD).
[0049] Add 5g of melamine and 10g of thiourea to 40mL of methanol solution. Stir for 20min and dry at 60℃. Place the mixture in an alumina crucible covered with aluminum foil and react at 650℃ for 6h, with a heating rate of 2.5℃ / min. Then allow to cool naturally, remove the product, and grind it until no particles remain. The sample is named SCN.
[0050] 0.146 g SCN, 1.70 g Bi(NO3)3, and RCD (RCD added at 5% of the total mass of SCN, Bi(NO3)3, and ethylene glycol) were added to 40 mL of ethylene glycol solution and sonicated for 3 h. The resulting mixture was named solution A. Simultaneously, 0.556 g KBr and 0.2 g NaOH were dissolved in 20 mL of distilled water and sonicated for 3 h. This solution was then added dropwise to solution A. The solution was stirred for 30 min, allowed to stand for 6 h, and then centrifuged repeatedly at 10000 rpm with water and ethanol, and dried at 105 °C to obtain tea-derived red-emitting carbon dots / carbon nitride / bismuth oxybromide.
[0051] Example 4 This example provides a method for preparing tea-derived carbon quantum dots with different fluorescence emission and tea-derived hydrothermal activated carbon, which includes the following steps:
[0052] 30.00 g of green tea powder was weighed and extracted with 300 mL of ethanol solution at 85 °C for 19 h using a Soxhlet extractor. The upper tea residue (residue A) was used for further reaction. After extraction, solution A was centrifuged at 10000 rpm to obtain the supernatant. 60 mL of the supernatant was placed in a 100 mL Lflon reactor and reacted at 180 °C for 6 h. After cooling, the mixture was centrifuged at 10000 rpm and filtered through a 0.22 μm filter membrane to obtain solution B (i.e., carbon dot solution). The carbon dot solution was separated and freeze-dried to obtain tea-derived red-emitting carbon quantum dots (RCDs).
[0053] Take 3.500 g of residue A, 0.8 mL of ethylenediamine, and 60 mL of distilled water, place them in a 100 mL beaker, stir for 30 min, then transfer to a polytetrafluoroethylene reactor and react at 200 °C for 13 h. After cooling to room temperature, extract the hydrothermal product, wash with water and ethanol solutions until the filtrate is colorless, and use the upper residue B for further reactions. The lower solution C is concentrated by rotary evaporation, centrifuged at 10,000 rpm for 10 min, and the supernatant is filtered through a 0.22 μm aqueous filter and dialyzed in a 500 D dialysis bag for 2 days. After concentration, the solution is freeze-dried to obtain tea-derived blue light-emitting carbon quantum dots (BCD).
[0054] Weigh 5 g of melamine and 7.5 g of thiourea into 40 mL of methanol solution. Stir for 20 min and dry at 60 °C. Place the mixture in an alumina crucible covered with aluminum foil and react at 600 °C for 5 h, with a heating rate of 2.5 °C / min. Then allow to cool naturally, remove the product, and grind it until no particles remain. The sample is named SCN.
[0055] 0.14 g SCN, 1.58 g Bi(NO3)3, and BCD (BCD added at 7% of the total mass of SCN, Bi(NO3)3, and ethylene glycol) were added to 40 mL of ethylene glycol solution and sonicated for 3 h. The resulting mixture was named solution A. Simultaneously, 0.5 g KBr and 0.18 g NaOH were dissolved in 20 mL of distilled water and sonicated for 3 h. This solution was then added dropwise to solution A. The solution was stirred for 30 min, allowed to stand for 5 h, and then centrifuged repeatedly at 10000 rpm with water and ethanol, and dried at 105 °C to obtain tea-derived blue-emitting carbon dots / carbon nitride / bismuth oxybromide.
[0056] In Comparative Example 1, 0.1-0.5 g of SCN was placed in a methanol solution and sonicated at 40 kW for 4 hours. The sonicated sample was named CN. The preparation method of SCN was the same as that in Example 2.
[0057] The preparation method of BiOBr in Comparative Example 2 is the same as that of R1 in Example 2, except that SCN and RCD are not added.
[0058] The preparation method of comparative example 3CN / BiOBr is the same as that of R1 in Example 2, except that RCD is not added.
[0059] Example 5 This example provides the application of tea-derived carbon quantum dot / carbon nitride / bismuth oxybromide photocatalyst in the photocatalytic degradation of Rhodamine B or tetracycline, comprising the following steps: 0.01 g of catalyst and Rhb solution or tetracycline solution (30 mg / L, 100 mL) are placed in a photocatalytic quartz tube, and photodegradation is carried out after the dark reaction reaches adsorption / desorption equilibrium for 30 min. Then, the light source is turned on (mercury lamp: 500 W, xenon lamp: 300 W), and samples are collected at regular intervals. In addition, the supernatant is collected by centrifugation at 12000 rpm, and the absorbance is measured using a UV-Vis spectrophotometer (UV-8000S, Shanghai, China). The above experiment is repeated, and the average value is calculated as the final data. Active free radicals play an irreplaceable and important role in the photocatalytic reaction process. Therefore, 2 mmol of silver nitrate (AgNO3), isopropanol (IPA), ammonium oxalate (AO), and 1,4-benzoquinone (BQ) are selected as electron free radicals (e - ), hydroxyl radicals (·OH), photogenerated vacancies (h + ) and superoxide radicals (·O 2- ) cleaning agent.
[0060] The RCD, BCD, R1-R4, and B1-B2 prepared in the above embodiments are characterized and tested below.
[0061] The RCD and BCD prepared in Example 1 were analyzed, and the characterization results are as follows: Figures 2-4 As shown. RCD and BCD are synthesized using different preparation processes. Both RCD and BCD solutions are brown at room temperature, but emit only red light under ultraviolet light. Figure 2 (Figure a, left) and blue fluorescence ( Figure 2 (Figure a on the right). Figure 2 The absorption spectra in Figure b reveal the reason: BCD exhibits a weak absorption peak in the 200-500 nm range, while RCD shows a broad absorption band covering the UV and visible light regions in the 200-700 nm range. Typically, the photoluminescence mechanism of carbon dots is explained by the carbon nucleus state, molecular state, and surface state. Compared to BCD, the π-π* transitions in RCD in the 225-300 nm range usually originate from the sp transitions of the carbon nucleus state. 2 Conjugated domains. Due to the greater number of conjugated domains, RCD exhibits red fluorescence. Meanwhile, the molecular state of RCD in the 500-650 nm range primarily originates from some macromolecular structures on its surface. FTIR spectroscopy explains the solubility difference between RCD and BCD. Figure 2 (Figure c). Although the samples have some similar functional groups, such as 3050-3600 cm⁻¹. -1 The peak values at 1669-1738 cm⁻¹ represent the tensile vibrations of OH and NH. -1This can be attributed to C=O tensile vibration and CN tensile vibration. The C=C tensile vibration of the RCD aromatic ring skeleton (1620 cm⁻¹) -1 The peak value of the C-C tensile vibration (1452 cm⁻¹) -1 This indicates the presence of a large number of SPs. 2 Structural and CH bending vibrations. At 1300-1400 cm. -1 CN bonds at the peak, BCD at 1050 cm⁻¹ -1 The OCD exhibits a stronger absorption peak (COC stretching vibration) at 720 cm⁻¹ than the RCD, indicating better water solubility. Conversely, compared to the BCD, the RCD shows a weaker absorption peak at 720 cm⁻¹. -1 The presence of -CH2 oscillation vibrations indicates that the RCD has a certain degree of hydrophobicity. Figure 3 Figure a shows the XRD spectrum of CQDs (CQDs are a collective term for RCD and BCD). There is a diffraction peak near 2θ = 20° in the CQDs, which may be related to the 002 crystal plane of graphite. Fluorescence spectroscopy is a direct means of obtaining the spectral properties of carbon quantum dots. Based on the fluorescence excitation spectrum (… Figure 3 (Figure b) shows that the excitation of BCD occurs at 350-450 nm, while the excitation of RCD occurs at 300-700 nm, with maximum excitation wavelengths of 407 nm and 665 nm, respectively, indicating typical two-photon emission. This can also be seen from... Figure 3 This can be seen in the 2D fluorescence spectrum of cd.
[0062] In the fluorescence emission spectrum of carbon dots ( Figure 2 As shown in Figure d), the fluorescence emission range of BCD is 420-700 nm, with a maximum emission peak at 480 nm. Unlike BCD, RCD exhibits similar fluorescence emission curves under excitation at 407 nm and 665 nm, with a maximum absorption peak near 675 nm and a shoulder peak at 720 nm. Due to the vibrational fine structure in the PL spectrum, it exhibits characteristics similar to localized emission. Furthermore, comparing the quantum yields of quinine sulfate, the fluorescence quantum yields of RCD and BCD are 8.2% and 4.4%, respectively. Therefore, the excellent photoluminescence properties of carbon dots promote photocatalysis.
[0063] To obtain the overall morphology of CQDs, they were observed using TEM, such as Figure 2 As shown in the EF diagram. Compared to the BCD spherical structure ( Figure 2 Compared to the f-image, sheet-like RCD ( Figure 2 The e-graph can more easily combine with C3N4, thereby improving the overall photocatalytic performance of the material. Figure 4 The lattice fringes of RCD and BCD are shown, with 0.33 nm and 0.21 nm referring to the 002 and 100 crystal planes of the graphite crystal form, respectively.
[0064] In the preparation of CQD, the residual product—hydrothermal carbon—was not utilized. Therefore, we used hydrothermal carbon and KOH to prepare activated hydrothermal carbon. The tea-derived activated hydrothermal carbon prepared in Example 1 was analyzed. Figure 5 Figures (a and b) are scanning electron microscope images of activated hydrothermal carbon. It can be seen that, compared to conventional activated carbon (HTC), its surface has a uniform pore structure, exhibiting smaller structure, more pores, and higher density. The yields of HTC-1, HTC-2, and HTC-3 are 7.1%, 6.5%, and 4.6%, respectively. The surface functional group structure of this material was characterized by infrared spectroscopy, such as... Figure 5 As shown in Figure c, compared with non-activated carbon materials, activated carbon materials have typical carbon material spectra, with peak values starting from 1100 cm⁻¹. -1 Reduced to 1780cm -1 This indicates that aromatization occurred during the activation process. Figure 5 d shows that HCT-2 has the ability to rapidly adsorb Rhodamine B.
[0065] The surface morphology of the tea-derived carbon quantum dots supported on carbon nitride / bismuth oxybromide prepared in Example 2 was analyzed, and the characterization results are as follows: Figures 6-11 As shown.
[0066] Surface morphology, elemental distribution, and structural characteristics are the most intuitive ways to understand materials. Figure 6 As catalysts, SCN and BiOBr are yellow and white, respectively, while R4 and B1 are brownish-green and gray, respectively. SEM images of SCN, BiOBr, and CN / BiOBr are shown below. Figure 7 As shown, SCN ( Figure 7 Figure a) shows obvious layered stacking, while BiOBr ( Figure 7 Figure b) shows a macroscopic clustering state. Figure 7 As shown in Figure c, BiOBr is dispersed on the CN surface, and the ultrasonic waves cause SCN exfoliation to a certain extent, resulting in more complete loading. After carbon quantum dot loading, compared with CN / BiOBr, R4 ( Figure 8 (Figure a) and B1 ( Figure 8 The scanning electron microscope image (d) showed no significant changes. However, in the transmission electron microscope (TEM), the carbon dots were clearly dispersed on the CN surface. HRTEM image ( Figure 8The BC and EF diagrams of the figure show clear lattice fringes with interplanar spacings of 0.25 nm, 0.82 nm, and 0.21 nm, which can be indexed to the (100) plane of SCN, the (001) plane of BiOBr, and the (100) plane of carbon, respectively. BiOBr is a rod-shaped accumulation, which is beneficial for forming certain porosity and improving light utilization. Carbon dots are the connection sites between CN and BiOBr, possessing a planar RCD structure that is more conducive to their contact. The surface elemental distribution of the sample was analyzed using mapping. Figure 8 gn diagram and Figure 9 The study found that R4 exposed significantly less C and N elements compared to B1, and its surface contained abundant Bi. This confirms that BiOBr in R4 is tightly wrapped around the CN surface, indicating that RCD plays a better role in connecting BiOBr and CN.
[0067] To more accurately understand the elemental composition of the material, EDX spectroscopy and ICP-MS were used to characterize the elemental composition of the catalyst. For example... Figure 10 As shown in Table 1, the surface C (1.64 wt%) and S (0.01 wt%) of R4 were significantly lower than those of B1 (7.49 wt%) and B1 (0.41 wt%). In ICP-MS (Table 2), the S and Bi contents of the catalysts were similar, indicating that the lipophilic RCD was more effective in catalyst binding and carbon dot deposition on the catalyst. Due to the presence of chlorophyll in tea leaves, trace amounts of magnesium may be present in the carbon quantum dots, a fact confirmed by mapping, EDX, and ICP-MS analyses. The surface magnesium contents of R4 and B1 were 0.12 wt% and 0.11 wt%, respectively, accounting for 0.0046 wt% of the total catalyst mass. These trace amounts of Mg can enhance the catalyst's light absorption and electron transfer.
[0068] Table 1. Classification of catalyst elements determined by EDX spectroscopy
[0069]
[0070] Table 2. Classification of catalyst elements determined by ICP-MS spectroscopy
[0071]
[0072] The specific surface area of a catalyst is a key factor affecting photocatalytic performance. Generally, a rich porous structure in a photocatalyst is beneficial for the exposure of active sites. The pore structure of the catalyst was studied using N2 adsorption-desorption curves. Figure 8 (See figure o). All samples exhibited Type III isotherms with H3 hysteresis loops, indicating that the pores were primarily flat-slit shaped. The specific surface areas of CN / BiOBr, R4, and B1 were 33.41 m² / g.2 g -1 89.26m 2 g -1 and 40.58m 2 g -1 The abundant specific surface area of R4 originates from the interweaving of the RCD layered structure between BiOBr and CN. R4 has a large number of active sites, exhibiting ultra-high adsorption and catalytic activity. Figure 11 Table 3 shows the pore size distribution of the catalysts. All materials exhibit good mesoporous structures. However, their pore size distributions differ. The pore size distributions of CN / BiOBr, R4, and B1 are 3-50 nm, 3-28 nm, and 3-48 nm, respectively. In particular, the pores of R4 are mainly concentrated around 6.68 nm. Compared with the average pore size of CN / BiOBr (13.3705 nm) and B1 (12.5027 nm), R4 has a more concentrated average pore size of 7.9498 nm. The favorable pore size of R4 provides a good opportunity for its application in photocatalysis.
[0073] Table 3 Pore size distribution of catalysts
[0074]
[0075] XPS spectral performance analysis was performed on R4 and B1, and the characterization results are as follows: Figures 12-13 As shown.
[0076] To further investigate the superior photocatalytic performance of CQDs / BiOBr / CN, the elemental valence states and composition of these heterojunction photocatalysts were evaluated using XPS. XPS full-spectrum and high-resolution XPS spectra are shown below. Figure 12 and Figure 13 As shown. Because RCD binds more readily to the catalyst, its surface is more hydrophobic than that of BCD. R4 typically has a lower binding energy, implying more robust coupling between the heterostructures. This coupling effect is further evidenced by the fact that the peak area of R4 is higher than that of B1. Based on C1s XPS analysis of R4 and B1 (… Figure 13 (Figure a) The peaks at 288.6 eV, 285.3 eV, and 284.7 eV represent the OC=O / NC=N, CO / CN, and CH / CC bonds formed by CQDs and carbon nitride, respectively. The C-OH and C=O bonds provided by carbon quantum dots are located near 286.3 eV and 286.0 eV, respectively. BiOBr-derived Bi4F ( Figure 13 Figure b) shows the values at 164.8 eV (Bi 2f5 / 2) and 159.5 eV (Bi 2f), respectively. 7 / 2 The area at () is a typical bimodal region, belonging to Bi. 3+ The chemical state of S2P. In the XPS spectrum ( Figure 13(Figure c) shows that the SO and SC bonds peak near 164.8 eV and 595.5 eV, respectively. The O1S spectrum of the composite material (…). Figure 13 The peaks (d) are composed of hydroxyl and carbonyl groups on the surface of carbon quantum dots and Bi-O bonds in BiOBr. The peaks at 402.2 eV, 401.4 eV, and 399.3 eV represent the CN=C skeleton structure of the aromatic ring, and SP... 3 Hybridization in (N-C3) and C-NHx within the aromatic ring plane ( Figure 13 (e-figure). Meanwhile, XPS valence band spectroscopy is an effective means of characterizing the valence band of semiconductor materials. Figure 13 f shows the XPS valence band spectrum of the catalyst. Calculations show that the valence band positions of R4 and B1 are 1.64 eV and 1.82 eV, respectively. This indicates that the addition of carbon dots can alter the chemical properties of the material to some extent.
[0077] Spectral performance analysis was performed on R4 and B1, and the characterization results are as follows: Figure 14 As shown.
[0078] The phase structures and crystallinity of CN, BiOBr, CN / BiOBr, R4, and B1 were studied by XRD. Figure 14 As shown in Figure a, the planar structure of CN aromatic segments, including the filling motif and interlayer stacking, reaches peaks at 13.0° and 27.3°, respectively. For BiOBr, its crystal structure conforms to a tetragonal phase (JCPDS No. 09-0393), with typical diffraction peaks at 10.8°, 25.2°, 32.3°, 39.4°, 46.4°, and 51.7° corresponding to the (001), (101), (110), (112), (200), and (212) planes, respectively. However, no diffraction peaks of CQDs and CN were found in the XRD patterns of R4 and B1, which may be due to the low introduction of CQDs and CN. Since the binding of RCD to the catalyst is more stable, the diffraction peak intensity of R4 is significantly lower than that of B1, indicating that R4 synthesized by the photoinduced method has higher catalytic activity potential.
[0079] Figure 14 Figure b is the FTIR spectrum of the catalyst. It can be seen that at 510 cm⁻¹... -1 The peak at 808 cm⁻¹ represents the Bi-O stretching vibration bond. Meanwhile, CN at 808 cm⁻¹... -1 1140cm -1 -1640cm -1 and 3000cm -1 -3600cm -1Three absorption peaks were observed, corresponding to the bending vibration of the triazine ring structure, the stretching vibration of the aromatic carbon-nitrogen heterocyclic compound, and the NH stretching vibration, respectively. After CQDs were loaded, the composite material showed absorption peaks for CN and BiOBr, indicating the successful synthesis of the catalyst.
[0080] The light absorption performance of a catalyst is an important indicator of its photocatalytic performance. The ultraviolet-visible diffuse reflectance (DRS) absorption spectrum of a photocatalyst is shown below. Figure 14 As shown in Figure c, SCN exhibits a strong adsorption band below 463 nm, while BiOBr shows low visible light absorption at 416 nm. When CN and BiOBr combine, the catalyst exhibits a wide visible light absorption range. Compared to other catalysts, R4 demonstrates stronger visible light absorption and a wider adsorption range. The Motschottky curve is a method for obtaining the flat band potential of a material. In n-type semiconductors, the flat band potential (Efb) is approximately equal to the conduction band position of the material. Figure 15 Figures a-e show the Motschottky curves for CN, BiOBr, CN / BiOBr, R4, and B1, respectively. To convert these to the standard hydrogen electrode potential (NHE), the formula E(NHE) = E(Ag / AgCl) + 0.197 is used. Therefore, the conduction bands (CB) of CN, BiOBr and CN / BiOBr, R4, and B1 are -0.123 eV, -0.523 eV and -0.193 eV, -0.333 eV and -0.533 eV, respectively. Their horizontal intercept is estimated to be 1 / C. 2 It equals zero. Simultaneously, combined with the Tauc diagram ( Figure 15 (from the f-plot), the theoretical band positions of CN, BiOBr, and CN / BiOBr were obtained ( Figure 14 The changes in band structure (as shown in the d-plot) confirm the formation of the heterojunction. Combined with the XPS valence band spectrum, the conduction bands (CB) of R4 and B1 can be calculated to be -0.53 eV and -0.77 eV, respectively. Figure 14 The changes in band gap and band position (as shown in the EF diagram) indicate that the introduction of CQDS greatly improves the utilization rate of light.
[0081] Fluorescence emission spectroscopy (PL) is an effective method for analyzing charge recombination efficiency. A decrease in fluorescence intensity indicates lower efficiency of photogenerated electron-hole recombination, which is more favorable for catalytic reactions. Furthermore, from... Figure 14 As can be observed in the g-plot, the fluorescence intensity of R4 and B1 is lower than that of other catalysts, indicating that the recombination of photogenerated carriers is restricted, thus promoting catalytic progress. Furthermore, transient photocurrent analysis, such as... Figure 14The h-plot is shown. The magnitude of the photocurrent reflects the separation efficiency of hole pairs, with R4 and B1 exhibiting the largest photocurrent values. Furthermore, electrochemical impedance spectroscopy (EIS) is an important characterization technique for studying the mobility of photogenerated carriers. For example... Figure 14 As shown in Figure i, compared with CN and BiOBr, the Nyquist plot of R4 has the smallest arc radius, indicating that the introduction of carbon dots improves the dissociation and charge transfer characteristics of charge carriers, making it easier to generate more electrons and holes in the photocatalytic degradation reaction. In summary, PL spectroscopy, photoelectrochemical tests, and EIS show that the introduction of CQDs has a good regulating effect on the separation efficiency and carrier mobility of the catalyst.
[0082] The catalytic mechanism of R4 and B1 was analyzed, and the characterization results are as follows: Figure 16 As shown.
[0083] To further elucidate the mechanism of photocatalytic degradation of RhB, electron spin trapping (ESR) was used to detect the contribution of active substances to the photocatalytic process. Figure 16 Figures a and b show the ·OH and ·O produced by catalyst R4 during the reaction. 2- ESR spectra of active free radicals. No free radicals were detected in the dark, but after illumination, the catalyst produced significant ·OH and ·O radicals. 2- A free radical signal peak was observed. The peak value then increased with time. Free radical capture experiments were performed to further verify the generation of active substances during the catalytic reaction. To further verify the generation of active species during the catalytic process, silver nitrate (AgNO3), isopropanol (IPA), ammonium oxalate (AO), and 1,4-benzoquinone (BQ) were selected as electrons (electrons). - A scavenger of hydroxyl (·OH) radicals, photogenerated vacancies (h+) and superoxide radicals (·O2). 2- ). Figure 16 Figure c shows the radical capture curves of the R4 catalyst. After the addition of AO, the degradation rate of RhB decreased from 98.65% to 41.95%. Simultaneously, after the addition of BQ, the degradation rate decreased to 37.84%. These results indicate that h + and O 2- It plays a major role in photocatalytic reactions. Therefore, free radical experiments and ESR analysis show that O 2- h + ·OH species play a key role in the photocatalytic oxidation of Rhb.
[0084] By combining the band structure of the catalyst with free radical testing, the mechanism of catalytic reaction can be revealed. For example... Figure 16As shown in Figure d, firstly, the valence band of BiOBr is irradiated to generate photogenerated electrons, thus forming a hole that oxidizes OH- to produce hydroxyl radicals. The photogenerated electrons migrate to the conduction band. Then, the carbon dots transfer the electrons generated by BiOBr to the valence band of CN. Finally, the electrons in the CN valence band jump to the conduction band to generate superoxide radicals to degrade RhB. Based on the above results, two main factors contribute to the high photocatalytic activity of R4. On the one hand, the carbon quantum dot loading greatly increases the specific surface area of the material, generating abundant active sites and making the photocatalytic process more efficient. On the other hand, R4 forms an effective charge collection and separation system for the z-shaped heterostructure between CN and BiOBr, not only forming a Schottky barrier to promote electron separation but also inducing the generation of highly active radicals. All the above results indicate that the sample prepared by the process route provided in this invention is a tea-derived carbon quantum dot-supported carbon nitride / bismuth oxybromide.
[0085] Using the method of Example 5, the catalytic performance of rhodamine and tetracycline was tested with R4 and B1. The test results are as follows: Figures 17-18 As shown. To evaluate the photocatalytic activity of the prepared material, RhB was photodegraded under a mercury lamp. First, Figure 17 The ad-α plot shows the photocatalytic degradation curves of CN / BiOBr loaded with RCD and BCD at different concentrations. R4 and B1 exhibit the best photocatalytic performance, with reaction rate constants of -0.2653 min⁻¹. -1 and -0.1068min -1 This is because a lower carbon dot loading limits the improvement in catalytic activity, while excessive carbon dots can lead to self-aggregation, which is detrimental to light and electron transfer. Furthermore, compared to BCD, sheet-like RCDs have more conjugated structures and stronger light absorption, resulting in a significantly higher catalytic rate for R4 than for B1. Figure 18 As shown in Figure a, pure SCN exhibits poor degradation of RhB. For pristine BiOBr and CN / BiOBr, only approximately 75% and 70% of RhB were degraded after 20 min of UV irradiation, respectively. The catalytic activity of RhB was significantly enhanced with the modulation of the band structure by the carbon dots. The catalytic rate of R4 was 4.07 and 3.15 times that of BiOBr and CN / BiOBr, respectively. Figure 18 (See Figure b). Reaction conditions are a crucial factor limiting catalytic reactions. Generally, the amount of catalyst used is related to the adsorption of light for the dark reaction and the absorption of light during photocatalysis. With an RhB concentration of 30 mg / L and a solution pH of 7, changing the catalyst dosage, such as... Figure 18 As shown in Figure c, with the increase of catalyst dosage, the adsorption performance of R4 on RhB also increases, making the adsorption effect much greater than the catalytic performance, which is not conducive to the reasonable disclosure of the process. When the catalyst dosage is 10 mg, it is obvious that the material has reached adsorption equilibrium. Figure 18 The d-plot shows the degradation curves for different RhB concentrations. With a catalyst dosage of 10 mg and a solution pH of 7, changing the RhB concentration revealed that the dark reaction was more likely to reach adsorption equilibrium with increasing RhB concentration. However, as the degradation time required for photocatalysis increased, insufficient RhB led to a greater adsorption effect than catalysis. Therefore, a RhB concentration of 30 mg / L was chosen as the optimal choice. The initial pH of the pollutants is an important variable to consider when striving to improve system efficiency. With an RhB concentration of 30 mg / L and a catalyst dosage of 10 mg, changing the pH... Figure 18 As shown in the e-plot, the catalyst exhibits good stability and minimal variation when the pH is between 3 and 9. On one hand, low or high pH can promote the adsorption of RhB on the catalyst surface; on the other hand, it can effectively suppress the recombination of electrons and holes, thereby promoting the catalytic reaction. When the pH is 1, H... + Dark reaction adsorption of RhB was inhibited, but under light intervention, the degradation rate reached 97.7% within 5 minutes. It is speculated that this rapid degradation may be due to the high H₂ content. + Electron-hole recombination at different concentrations. Table 4 shows the photocatalytic degradation data of RhB by different catalysts. It can be seen from Table 4 that R4 exhibits good catalytic performance. The doi of the references in Table 4 are shown below:
[0086] [1]http: / / doi.org / 10.1039 / c4dt01702a.
[0087] [2]http: / / doi.org / 10.1016 / j.optmat.2022.113035.
[0088] [3]http: / / doi.org / 10.12030 / j.cjee.202203135.
[0089] [4]http: / / doi.org / 10.11896 / cldb.21060126.
[0090] [5]http: / / doi.org / 10.1016 / j.molstruc.2022.132768.
[0091] Table 4. Photocatalytic degradation data of RhB by different catalysts
[0092]
[0093] To expand the application of the catalyst, a 300W Xe lamp was used for the catalytic degradation of RhB (…). Figure 18(See Figure f). The CN / BiOBr heterojunction plays a crucial role in catalysis, and the introduction of carbon dots further enhances the photocatalytic performance of the composite material. At 20 min, the degradation rates of RhB by R4 and B1 were 99.0% and 98.5%, respectively. The photocatalytic degradation of tetracycline by R4 was also tested; under a 300 W Xe lamp, 82.45% of tetracycline was degraded within 70 min. The tests demonstrate that they possess good light absorption properties and catalytic versatility. The cyclic catalytic performance of R4 and B1 for Rhodamine was tested using the method described in Example 5, and the test results are as follows: Figure 19 As shown. Figure 19 Figure a shows the catalyst sample during and after the reaction, clearly demonstrating the strong adsorption of RhB on the catalyst surface. To verify the cyclic catalytic performance of this material, R4 was used to catalyze the degradation of RhB, as shown in Figure a. Figure 19 As shown in Figure b, after four rounds of catalysis, the decomposition rate of RhB decreased from 99.54% to 98.87%, indicating that the material has good cycling performance. Furthermore, as... Figure 19 As shown in Figures c and d, the FTIR and XRD spectra of the catalyst before and after the four reactions did not show significant changes, indicating that the material structure has good stability. Therefore, the modulation of the band structure by carbon dots is key to improving the catalyst's cycle performance.
[0094] The intermediates of the catalytic reaction of R4 with rhodamine were tested, and the results are as follows: Figures 20-21 As shown. HPLC-MS is an important analytical method for studying intermediates generated during the degradation process. Figure 20 The results showed that RhB exhibited high efficiency during photocatalytic degradation at 0 minutes ( Figure 20 (Figure a-1), 10 minutes ( Figure 20 (Figure b-1) and 20 minutes ( Figure 20 The UPLC-MS spectrum of (c-1 figure). Figure 20 As shown, the retention time of the RhB solution in the unreacted state was 9.52 minutes ( Figure 20 The peak values were observed at 0.00–3.00 min and 9.80 min, as shown in Figure a-2. MS analysis revealed that the degradation primarily involved RhB dechlorination (m / z = 443) and removal of one molecule of ethyl group (m / z = 415). When the catalytic degradation proceeded for 10 min, the peak values were observed in the UPLC spectrum at 0.00–3.00 min and 7.70 min. Figure 20An absorption peak was observed at 10.00 min (Figure b-2). In the mass spectrometry with retention times of 7.70–10.00 min, the product (m / z = 415) showed that the ethyl group was successively removed, forming molecules at m / z = 387, m / z = 359, and m / z = 210. Then, the compound (m / z = 210) formed a diphenyl ether (m / z = 170) by removing the two amino groups on both sides and breaking the double bond. Finally, when the catalytic time reached 20 min (…),… Figure 20 When the c-1 graph is used, the retention time is mostly around 0.00-3.00 minutes, but at 7.70 ( Figure 20 The retention time (as shown in Figure c-2) still exhibits a peak at m / z = 195 after 1 minute, indicating that the formation of diphenyl ether is the main catalytic step. Further cleavage of the diphenyl ether forms phenol (m / z = 88). Simultaneously, benzoic acid stripped from m / z = 359 undergoes hydrogenation (m / z = 126), hydroxylation (m / z = 444), bond breaking, carboxylation, and decarboxylation (m / z = 1.58) to form a small molecule compound. The final product further degrades into CO2 and H2O, with reaction intermediates such as... Figure 21 As shown.
[0095] Although preferred embodiments of the invention have been described, those skilled in the art, upon learning the basic inventive concept, can make other changes and modifications to these embodiments. Therefore, the appended claims are intended to be interpreted as including both the preferred embodiments and all changes and modifications falling within the scope of the invention. Clearly, those skilled in the art can make various alterations and modifications to the invention without departing from its spirit and scope. Thus, if these modifications and modifications of the invention fall within the scope of the claims and their equivalents, the invention is also intended to include these modifications and modifications.
Claims
1. A preparation method of carbon nitride / bismuth oxybromide / carbon quantum dot photocatalyst, characterized in that, Includes the following steps: Step 1: Using ethanol as a solvent, perform Soxhlet extraction on tea powder. After extraction, solution A and residue A are obtained. Step 2: The supernatant after centrifugation of solution A is subjected to hydrothermal treatment at 150-180℃ to obtain solution B. Solution B is then post-processed to obtain tea-derived red light emitting carbon quantum dots. Step 3: Using water as a solvent and ethylenediamine as a passivating agent, add residue A and perform hydrothermal treatment at 180-200℃ to obtain solution C. Post-process solution C to obtain tea-derived blue light emitting carbon quantum dots. Step 4: Add carbon nitride, bismuth nitrate pentahydrate, and tea-derived red-emitting carbon quantum dots or tea-derived blue-emitting carbon quantum dots to ethylene glycol, and sonicate to obtain solution D. Dissolve potassium bromide and sodium hydroxide in water, and sonicate to obtain solution E. Add solution E dropwise to solution D, stir and mix evenly, and let stand for 2-6 hours to obtain tea-derived red-emitting carbon dots / carbon nitride / bismuth oxybromide or tea-derived blue-emitting carbon dots / carbon nitride / bismuth oxybromide. Carbon nitride is prepared by the following steps: melamine and thiourea are added to methanol, stirred evenly, and dried to obtain a mixed product. The mixed product is then reacted at 550-650℃ for 4-6 hours to obtain carbon nitride. 2.The method for preparing a carbon nitride / bismuth oxybromide / carbon quantum dot photocatalyst according to claim 1, characterized in that, In step 1, the ratio of tea powder to ethanol is 1-3g:30mL, the extraction temperature is 80-90℃, and the extraction time is 18-20h.
3. The method for preparing a carbon nitride / bismuth oxybromide / carbon quantum dot photocatalyst according to claim 1, characterized in that, In step 2, the hydrothermal treatment time is 4 to 8 hours. 4.The method for preparing a carbon nitride / bismuth oxybromide / carbon quantum dot photocatalyst according to claim 1, characterized in that, In step 3, the ratio of residue A, water, and ethylenediamine is 3-4 g: 60 mL: 0.5-1 mL; the hydrothermal time is 12-14 h.
5. The method for preparing a carbon nitride / bismuth oxybromide / carbon quantum dot photocatalyst according to claim 1, characterized in that, In step 4, the ratio of carbon nitride, bismuth nitrate pentahydrate, and ethylene glycol is 0.136–0.146 g: 1.58–1.70 g: 40 mL; The amount of red-emitting carbon quantum dots derived from tea leaves added is 5-25% of the total mass of carbon nitride, bismuth nitrate pentahydrate, and ethylene glycol; the amount of blue-emitting carbon quantum dots derived from tea leaves added is 5-10% of the total mass of carbon nitride, bismuth nitrate pentahydrate, and ethylene glycol. The ratio of potassium bromide, sodium hydroxide, and water is 0.476–0.556 g: 0.16–0.20 g: 20 mL; The volume ratio of solution D to solution E is 2:
1. 6.The method for preparing a carbon nitride / bismuth oxybromide / carbon quantum dot photocatalyst according to claim 1, characterized in that, In step 4, the ratio of melamine, thiourea, and methanol is 1g:1-2g:40mL.
7. A carbon nitride / bismuth oxybromide / carbon quantum dot photocatalyst prepared by the preparation method according to any one of claims 1 to 6.
8. The application of the carbon nitride / bismuth oxybromide / carbon quantum dot photocatalyst according to claim 7 in the photocatalytic degradation of organic pollutants.
9. Use of the carbon nitride / bismuth oxybromide / carbon quantum dots photocatalyst according to claim 8 for photocatalytic degradation of organic pollutants, characterized in that, The organic pollutants are rhodamine B or tetracycline.
10. Use of the carbon nitride / bismuth oxybromide / carbon quantum dots photocatalyst according to claim 9 for photocatalytic degradation of organic pollutants, characterized in that, The catalyst addition amount is 5-25g, the organic pollutant concentration is 10-90mg / L, and the pH is 1-9.
Citation Information
Patent Citations
Preparation method of fluorescent carbon point based on tea leaves and fluorescent carbon point prepared according to preparation method
CN109095453A