A composite thermoelectric nanofiber membrane and its preparation method
The preparation of composite wet thermoelectric nanofiber membranes through electrospinning technology solves the problem of single fiber membrane power generation technology, realizes the dual functions of temperature difference and moisture power generation, and improves electrical and mechanical properties.
Patent Information
- Application Number
- CN202410918449.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-07-10
AI Technical Summary
The existing fiber membranes have single power generation technology and rely on temperature differences, resulting in limited electrical performance and inability to achieve moisture power generation.
The composite wet thermoelectric nanofiber membrane is prepared by electrospinning technology. By combining 3,4-ethylene dioxythiophene and pyrrole with bismuth telluride and other materials, nanoparticles are formed and mixed with polyelectrolyte solution to form porous nanofibers. membrane, achieving temperature difference and moisture power generation.
Under the temperature difference between 5℃-50℃ and humidity of 30%-90%, the output voltage of the fiber membrane is 0.5V-1.2V and the current is 50μA-200μA. It has stable temperature and humidity power generation capabilities, which improves the fiber membrane conductivity and mechanical flexibility.
Smart Images

Figure SMS_4
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of fiber membranes, and in particular to a composite thermoelectric nanofiber membrane and a preparation method thereof. Background Art
[0002] In order to solve the problem of increasing consumption of primary energy such as oil, coal and natural gas and ecological pollution, it is urgent to develop and utilize new energy materials. In the existing technology, screen printing technology, electrodeposition method, spin coating method, drop casting method and other methods are commonly used to prepare a fiber membrane that can realize temperature difference power generation. The principle is to apply thermoelectric materials to fiber films. Thermoelectric materials realize the mutual conversion of heat energy and electrical energy through the transmission of carriers (including electrons e and holes h) inside solid materials, and finally achieve the technical effect of temperature difference power generation. It is a green and environmentally friendly energy conversion product.
[0003] In the prior art, the conversion of heat energy and electrical energy in the fiber membrane is achieved through temperature difference, which not only leads to a single power generation technology for the fiber membrane, but also causes limitations in fiber membrane power generation, making fiber membrane power generation only rely on temperature difference, resulting in limitations in the way the fiber membrane generates electrical properties. Summary of the invention
[0004] In order to solve the above technical problems, the present invention provides a composite wet heat electric nanofiber membrane and a preparation method thereof. The nanofiber membrane obtained by the present invention can simultaneously achieve the technical effects of temperature difference power generation and wet gas power generation, and has good electrical properties.
[0005] The present invention provides a method for preparing a composite thermoelectric nanofiber membrane, comprising the following steps:
[0006] Step S1: dissolving 3,4-ethylenedioxythiophene and pyrrole in a dopant, adding an oxidant dropwise, performing polymerization reaction, solid-liquid separation, and drying to obtain composite nanoparticles;
[0007] Step S2: mixing the solution containing the composite nanoparticles with a bismuth telluride (Bi2Te3) solution to prepare a dispersion for electrostatic spinning to obtain a thermoelectric nanofiber film;
[0008] Step S3: Spraying the polyelectrolyte solution onto the thermoelectric nanofiber film by electrospinning to obtain a composite wet thermoelectric nanofiber membrane.
[0009] Furthermore, the oxidant includes one or more of persulfate and salt containing iron ions.
[0010] Furthermore, the persulfate includes one or more of ammonium persulfate and sodium persulfate.
[0011] Furthermore, the salt containing iron ions includes one or more of ferric chloride and ferric sulfate.
[0012] Furthermore, the dopant includes a compound containing sulfonate ions.
[0013] Furthermore, the compound containing sulfonate ions includes one or more of polystyrene sulfonic acid and p-toluene sulfonic acid.
[0014] Furthermore, the mass ratio of 3,4-ethylenedioxythiophene to pyrrole is 1-3:1.
[0015] Furthermore, the molar concentration of 3,4-ethylenedioxythiophene in the dopant is 0.3 mol / L-0.8 mol / L.
[0016] Furthermore, the polymerization reaction conditions include: temperature of -15°C to -24°C and time of 48h to 96h.
[0017] Furthermore, the polymerization reaction is performed twice. After the first polymerization reaction, the solution after the polymerization reaction is thawed at room temperature for 2.5h-3.5h, and then the second polymerization reaction is performed. The conditions of the second polymerization reaction are the same as those of the first polymerization reaction.
[0018] Furthermore, in order to promote the sufficiency of the polymerization reaction at low temperature, the solution to be subjected to the polymerization reaction may be sufficiently mixed and stirred before the polymerization reaction.
[0019] Furthermore, the drying temperature is 58° C.-62° C., and the drying time is 1 h-2 h.
[0020] Furthermore, considering the effect of solid-liquid separation, those skilled in the art may adopt vacuum filtration.
[0021] Furthermore, the bismuth telluride solution is prepared by dissolving bismuth telluride in anhydrous ethanol.
[0022] Furthermore, the mass concentration of the bismuth telluride solution is 15%-25%, and the mass concentration of the solution containing the composite nanoparticles is 1.5%-3%.
[0023] Furthermore, after the solution containing the composite nanoparticles is mixed with the bismuth telluride solution, the mass ratio of the bismuth telluride to the composite nanoparticles is 1:1-6.
[0024] Furthermore, the parameters of the electrospinning in step S2 are as follows: voltage is 16 kv-24 kv, spinning speed is 1 mL / h-3 mL / h, and receiving distance is 15 cm-20 cm.
[0025] Furthermore, the mass concentration of the polyelectrolyte solution is 10%-30%.
[0026] Furthermore, the method for preparing the polyelectrolyte solution includes: dissolving the polyelectrolyte in deionized water.
[0027] Furthermore, the polyelectrolyte in the polyelectrolyte solution includes one or more of polystyrene sulfonic acid, sodium polystyrene sulfonate, polyacrylic acid, sodium alginate, hydroxymethyl cellulose, and polyethylene imine.
[0028] Furthermore, the polyelectrolyte in the polyelectrolyte solution is sodium alginate.
[0029] Furthermore, the parameters of the electrospinning in step S3 are as follows: voltage is 16 kv-24 kv, spinning speed is 1 mL / h-3 mL / h, and receiving distance is 15 cm-20 cm.
[0030] The present invention also provides a composite moist heat electric nanofiber membrane obtained by the preparation method of the composite moist heat electric nanofiber membrane.
[0031] Furthermore, the specific surface area of the composite thermoelectric nanofiber membrane is 18 m 2 / g-26m 2 / g, porosity is 75%-85%.
[0032] The embodiments of the present invention have the following technical effects:
[0033] 1. First, the composite wet thermoelectric nanofiber membrane obtained by the present invention has a suitable specific surface area and porosity, which ensures the stability of the fiber membrane structure. The fiber membrane of the present invention also has the power generation capacity of wet gas power generation and temperature difference power generation. Under the conditions of a temperature difference of 5°C-50°C and a humidity difference of 30%-90%, the output voltage is 0.5V-1.2V and the current is 50μA-200μA.
[0034] 2. In the present invention, 3,4-ethylenedioxythiophene and pyrrole are dissolved and polymerized to form poly-3,4-ethylenedioxythiophene and polypyrrole, and poly-3,4-ethylenedioxythiophene and polypyrrole have adjustable electrical conductivity; in addition, Bi2Te3 has high electrical conductivity and Seebeck coefficient, which can improve the electrical conductivity, mechanical flexibility and wet thermoelectric power generation capacity of the fiber membrane. The improvement of mechanical flexibility is also beneficial to lay the foundation for the polyelectrolyte solution to form a layer of wet differential power generation structure on the surface of the thermoelectric nanofiber film, which is beneficial to improve the structural stability of the finally obtained composite wet thermoelectric nanofiber membrane, and ensure the stability of the temperature difference power generation and wet differential power generation of the composite wet thermoelectric nanofiber membrane of the present invention.
[0035] 3. In the method of the present invention, in order to realize the composite wet thermoelectric nanofiber membrane of the present invention, on the basis of having a stable structure, it also has the power generation capacity of wet power generation and temperature difference power generation. Therefore, in the invention, the specific surface area and porosity of the fiber membrane are further designed. On the one hand, it is necessary to consider whether a temperature difference and humidity difference can be formed at both ends of the fiber membrane. On the other hand, it is necessary to consider the mechanical strength of the fiber membrane and the stability of the pore structure, so as to facilitate the formation of a stable humidity difference on the fiber membrane. First, the porosity and specific surface area formed by the thermoelectric nanofiber film are adjusted. The thermoelectric nanofiber film is the basis for the formation of wet differential power generation. To ensure the stability of the structure, it requires appropriate mechanical strength and the stability of the pore structure. It is an important component for realizing wet differential power generation of the fiber membrane. Secondly, the polyelectrolyte solution is electrospinned to form a layer of humidity differential power generation structure on the thermoelectric nanofiber film. This structure is first of all an important component of the fiber membrane to achieve humidity differential power generation. The porosity, specific surface area and raw materials forming this structure are selected, which is not only conducive to forming a 30%-90% humidity difference at both ends of the fiber membrane, thereby facilitating the realization of humidity differential power generation; but also enables a higher connection between the two layers of the structure, so that the fiber membrane ultimately has both temperature difference and humidity differential power generation. DETAILED DESCRIPTION
[0036] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work belong to the scope of protection of the present invention.
[0037] In a first aspect, some embodiments of the present invention provide a method for preparing a composite thermoelectric nanofiber membrane, comprising the following steps:
[0038] Step S1: dissolving 3,4-ethylenedioxythiophene and pyrrole in a dopant, adding an oxidant dropwise, performing polymerization reaction, solid-liquid separation, and drying to obtain composite nanoparticles;
[0039] Step S2: mixing the solution containing the composite nanoparticles with the bismuth telluride solution to prepare a dispersion for electrostatic spinning to obtain a thermoelectric nanofiber film;
[0040] Step S3: Spraying the polyelectrolyte solution onto the thermoelectric nanofiber film by electrospinning to obtain a composite wet thermoelectric nanofiber membrane.
[0041] In the method of the present invention, the porosity and specific surface area of the formed thermoelectric nanofiber film and the finally obtained composite moist heat electric nanofiber membrane are regulated by the electrospinning preparation method, which not only enables the two-layer structure in the composite moist heat electric nanofiber membrane to be tightly combined, but also enables the composite moist heat electric nanofiber membrane of the present invention to have the technical effects of temperature difference power generation and humidity difference power generation.
[0042] In some embodiments, the oxidant includes one or more of persulfate and salt containing iron ions.
[0043] In some embodiments, the persulfate includes one or more of ammonium persulfate and sodium persulfate.
[0044] In some embodiments, the salt containing iron ions includes one or more of ferric chloride and ferric sulfate.
[0045] In some embodiments, the dopant includes a compound containing a sulfonate ion.
[0046] In some embodiments, the compound containing sulfonate ions includes one or more of polystyrene sulfonic acid and p-toluene sulfonic acid.
[0047] In some embodiments, the mass ratio of 3,4-ethylenedioxythiophene to pyrrole is 1-3:1.
[0048] In some embodiments, the molar concentration of 3,4-ethylenedioxythiophene in the dopant is 0.3 mol / L-0.8 mol / L.
[0049] In some embodiments, the polymerization reaction conditions include: temperature of -15°C to -24°C, and time of 48h to 96h.
[0050] In some embodiments, the polymerization reaction is performed twice. After the first polymerization reaction, the solution after the polymerization reaction is thawed at room temperature for 2.5h-3.5h, and then a second polymerization reaction is performed. The conditions of the second polymerization reaction are the same as those of the first polymerization reaction.
[0051] In some embodiments, in order to promote the sufficiency of the polymerization reaction at low temperature, the solution to be subjected to the polymerization reaction may be sufficiently and uniformly mixed before the polymerization reaction, and stirring may be adopted.
[0052] In some embodiments, the drying temperature is 58° C.-62° C., and the drying time is 1 h-2 h.
[0053] In some embodiments, considering the effect of solid-liquid separation, those skilled in the art may adopt vacuum filtration.
[0054] In some embodiments, the bismuth telluride solution is prepared by dissolving bismuth telluride in anhydrous ethanol.
[0055] In some embodiments, the mass concentration of the bismuth telluride solution is 15%-25%, and the mass concentration of the solution containing the composite nanoparticles is 1.5%-3%.
[0056] In some embodiments, after the solution containing the composite nanoparticles is mixed with the bismuth telluride solution, the mass ratio of the bismuth telluride to the composite nanoparticles is 1:1-6.
[0057] In some embodiments, the parameters of the electrospinning in step S2 are as follows: voltage is 16 kv-24 kv, spinning speed is 1 mL / h-3 mL / h, and receiving distance is 15 cm-20 cm.
[0058] In some embodiments, the mass concentration of the polyelectrolyte solution is 10%-30%.
[0059] In some embodiments, the polyelectrolyte in the polyelectrolyte solution includes one or more of polystyrene sulfonic acid, sodium polystyrene sulfonate, polyacrylic acid, sodium alginate, hydroxymethyl cellulose, and polyethylene imine.
[0060] In some embodiments, the parameters of the electrospinning in step S3 are as follows: voltage is 16 kv-24 kv, spinning speed is 1 mL / h-3 mL / h, and receiving distance is 15 cm-20 cm.
[0061] In a second aspect, some embodiments of the present invention also provide a composite moist heat electric nanofiber membrane obtained by the preparation method of the composite moist heat electric nanofiber membrane.
[0062] In some embodiments, the specific surface area of the composite thermoelectric nanofiber membrane is 18 m 2 / g-26m 2 / g, porosity is 75%-85%.
[0063] The following is further described in conjunction with specific embodiments:
[0064] Embodiment 1:
[0065] Step S1: Dissolve 3,4-ethylenedioxythiophene (EDOT) and pyrrole (Py) in polystyrene sulfonic acid, add persulfate dropwise, perform polymerization reaction, separate solid and liquid, and dry to obtain composite nanoparticles, wherein the mass ratio of 3,4-ethylenedioxythiophene to pyrrole is 2:1, and the molar concentration of 3,4-ethylenedioxythiophene in polystyrene sulfonic acid is 0.5 mol / L. The mixed solution is placed at -20°C for low-temperature in-situ polymerization for 72 hours. The reacted solution is then taken out and thawed for 3 hours, and then re-frozen at -20°C for 72 hours, vacuum filtered, and dried at 60°C for 1 hour to obtain composite nanoparticles.
[0066] Step S2: Mix the solution containing the composite nanoparticles with the bismuth telluride solution to prepare a dispersion for electrospinning to obtain a thermoelectric nanofiber film. After mixing, the mass ratio of bismuth telluride to the composite nanoparticles is 1:4; the mass concentration of the bismuth telluride solution is 20%, and the mass concentration of the solution containing the composite nanoparticles is 2.3%; the specific parameters of the electrospinning are: voltage of 20 kV, spinning speed of 2 mL / h, and receiving distance of 17 cm.
[0067] Step S3: Spraying the polyelectrolyte solution onto the thermoelectric nanofiber film by electrospinning to obtain a composite wet thermoelectric nanofiber film. The polyelectrolyte is sodium alginate, and the mass concentration of the polyelectrolyte solution is 20%; the specific parameters of electrospinning are: voltage of 20 kV, spinning speed of 2 mL / h, and receiving distance of 17 cm.
[0068] Embodiment 2:
[0069] The step S1 of embodiment 2 is the same as that of embodiment 1;
[0070] Step S2: Mix the solution containing the composite nanoparticles with the bismuth telluride solution to prepare a dispersion for electrostatic spinning to obtain a thermoelectric nanofiber film. After mixing, the mass ratio of bismuth telluride to the composite nanoparticles is 1:4; the mass concentration of the bismuth telluride solution is 20%, and the mass concentration of the solution containing the composite nanoparticles is 2.3%; the specific parameters of the electrostatic spinning are: voltage of 16 kV, spinning speed of 2 mL / h, and receiving distance of 17 cm.
[0071] Step S3: Spraying the polyelectrolyte solution onto the thermoelectric nanofiber film by electrospinning to obtain a composite wet thermoelectric nanofiber film. The polyelectrolyte is sodium alginate, and the mass concentration of the polyelectrolyte solution is 20%; the specific parameters of the electrospinning are: voltage of 24 kV, spinning speed of 2 mL / h, and receiving distance of 17 cm.
[0072] Embodiment 3:
[0073] Embodiment 3 is the same as step S1 of embodiment 1;
[0074] Step S2: Mix the solution containing the composite nanoparticles with the bismuth telluride solution to prepare a dispersion for electrostatic spinning to obtain a thermoelectric nanofiber film. After mixing, the mass ratio of bismuth telluride to the composite nanoparticles is 1:4; the mass concentration of the bismuth telluride solution is 20%, and the mass concentration of the solution containing the composite nanoparticles is 2.3%; the specific parameters of the electrostatic spinning are: voltage of 24kv, spinning speed of 2mL / h, and receiving distance of 17cm.
[0075] Step S3: Spraying the polyelectrolyte solution onto the thermoelectric nanofiber film by electrospinning to obtain a composite wet thermoelectric nanofiber film. The polyelectrolyte is sodium alginate, and the mass concentration of the polyelectrolyte solution is 20%; the specific parameters of the electrospinning are: voltage of 16 kV, spinning speed of 2 mL / h, and receiving distance of 17 cm.
[0076] Embodiment 4:
[0077] The step S1 of embodiment 4 is the same as that of embodiment 1;
[0078] Step S2: Mix the solution containing the composite nanoparticles with the bismuth telluride solution to prepare a dispersion for electrospinning to obtain a thermoelectric nanofiber film. After mixing, the mass ratio of bismuth telluride to the composite nanoparticles is 1:4; the mass concentration of the bismuth telluride solution is 15%, and the mass concentration of the solution containing the composite nanoparticles is 1.5%; the specific parameters of the electrospinning are: voltage of 20 kV, spinning speed of 2 mL / h, and receiving distance of 17 cm.
[0079] Step S3: Spraying the polyelectrolyte solution onto the thermoelectric nanofiber film by electrospinning to obtain a composite wet thermoelectric nanofiber film. The polyelectrolyte is sodium alginate, and the mass concentration of the polyelectrolyte solution is 10%; the specific parameters of the electrospinning are: voltage of 20 kV, spinning speed of 2 mL / h, and receiving distance of 17 cm.
[0080] Embodiment 5:
[0081] Embodiment 5 is the same as step S1 of embodiment 1;
[0082] Step S2: Mix the solution containing the composite nanoparticles with the bismuth telluride solution to prepare a dispersion for electrospinning to obtain a thermoelectric nanofiber film. After mixing, the mass ratio of bismuth telluride to the composite nanoparticles is 1:4; the mass concentration of the bismuth telluride solution is 15%, and the mass concentration of the solution containing the composite nanoparticles is 1.5%; the specific parameters of the electrospinning are: voltage of 20 kV, spinning speed of 2 mL / h, and receiving distance of 17 cm.
[0083] Step S3: Spraying the polyelectrolyte solution onto the thermoelectric nanofiber film by electrospinning to obtain a composite wet thermoelectric nanofiber film. The polyelectrolyte is sodium alginate, and the mass concentration of the polyelectrolyte solution is 25%; the specific parameters of electrospinning are: voltage of 20 kV, spinning speed of 2 mL / h, and receiving distance of 17 cm.
[0084] Embodiment 6:
[0085] The preparation method of Example 6 is the same as that of Example 1, but the polyelectrolyte used in Example 6 is polystyrene sulfonic acid.
[0086] Embodiment 7:
[0087] The preparation method of Example 7 is the same as that of Example 1, but the polyelectrolyte used in Example 6 is hydroxymethyl cellulose.
[0088] Comparative Example 1:
[0089] The step S1 of Comparative Example 1 is the same as that of Example 1;
[0090] Step S2: Mix the solution containing the composite nanoparticles with the bismuth telluride solution to prepare a dispersion for electrostatic spinning to obtain a thermoelectric nanofiber film. After mixing, the mass ratio of bismuth telluride to the composite nanoparticles is 1:4; the mass concentration of the bismuth telluride solution is 20%, and the mass concentration of the solution containing the composite nanoparticles is 2.3%; the specific parameters of the electrostatic spinning are: voltage of 14kv, spinning speed of 2mL / h, and receiving distance of 17cm.
[0091] Step S3: Spraying the polyelectrolyte solution onto the thermoelectric nanofiber film by electrospinning to obtain a composite wet thermoelectric nanofiber film. The polyelectrolyte is sodium alginate, and the mass concentration of the polyelectrolyte solution is 20%; the specific parameters of electrospinning are: voltage of 20 kV, spinning speed of 2 mL / h, and receiving distance of 17 cm.
[0092] Comparative Example 2:
[0093] Comparative Example 2 is the same as step S1 of Example 1;
[0094] Step S2: Mix the solution containing the composite nanoparticles with the bismuth telluride solution to prepare a dispersion for electrostatic spinning to obtain a thermoelectric nanofiber film. After mixing, the mass ratio of bismuth telluride to the composite nanoparticles is 1:4; the mass concentration of the bismuth telluride solution is 20%, and the mass concentration of the solution containing the composite nanoparticles is 2.3%; the specific parameters of the electrostatic spinning are: voltage of 14kv, spinning speed of 2mL / h, and receiving distance of 17cm.
[0095] Step S3: Spraying the polyelectrolyte solution onto the thermoelectric nanofiber film by electrospinning to obtain a composite wet thermoelectric nanofiber film. The polyelectrolyte is sodium alginate, and the mass concentration of the polyelectrolyte solution is 20%; the specific parameters of the electrospinning are: voltage of 25 kV, spinning speed of 2 mL / h, and receiving distance of 17 cm.
[0096] Comparative Example 3:
[0097] An inert metal is sputtered on the PDMS (polydimethylsiloxane) flexible substrate layer to form a current collecting layer on the surface of the flexible substrate (sputtering deposition uses PECVD vapor deposition (plasma enhanced chemical vapor deposition), the vacuum degree reaches 8Pa, argon atmosphere is introduced, and DC sputtering is used with a power of 100W). Then, a PEDOT (poly 3,4-ethylenedioxythiophene) film layer is plated on the surface of the flexible substrate layer / current collecting layer using a three-electrode working system electrodeposition method to obtain an electrode layer. The flexible substrate layer is used as the working electrode, Ag / AgCl is used as the reference electrode, and Pt is used as the counter electrode. The thickness of the flexible substrate layer is 120mm. SDS (sodium dodecyl sulfate) and EDOT (3,4-ethylenedioxythiophene) (the concentration ratio of SDS and EDOT is 1:1) are added to the sulfuric acid solution in sequence, stirred evenly, and then the solution is heated to 60°C in a water bath as an electroplating solution.
[0098] The products obtained in the examples and comparative examples were tested for output voltage and current: the film was cut into 1×1 cm 2 The size of the composite film is then connected to the upper and lower surfaces with wires, and the left and right ends of the film are connected to Boll patches respectively, thereby generating a temperature difference of 30°C; at the same time, N2 carrying water vapor is passed through the upper surface of the composite film, thereby generating a humidity difference of 60°C between the upper and lower surfaces of the film, and finally the Keithley2514 digital source meter is used to test the output voltage and current of the film.
[0099] Testing method for specific surface area: The BSD-PM2 high-performance specific surface and micropore analyzer was used to measure the N2 adsorption-desorption isotherm of the sample under liquid nitrogen, and then the BET method was used to calculate the specific surface area of the fiber membrane.
[0100] The porosity test method is as follows: the prepared nanofiber membrane is cut into square specimens with a side length of 2 cm. The initial fiber membrane is weighed first, and then the fiber membrane is immersed in n-butanol for 20 minutes. Then, the fiber membrane after absorbing n-butanol is taken out, and the excess n-butanol on the surface of the fiber membrane is sucked off. Finally, the nanofiber membrane after absorbing n-butanol is weighed, and the weighing result is put into the following formula to calculate the porosity:
[0101] ;
[0102] Wherein, P is the porosity, unit is %; M o is the initial mass of the fiber membrane, in g; is the fiber membrane density, unit: g / cm 3 ;M b is the mass of n-butanol absorbed by the fiber membrane, in g; is the density of n-butanol, in g / cm 3 In the present invention, the density of n-butanol is 0.81 g / cm 3 ;Fiber membrane density is 1.15g / cm 3 .
[0103] Results and Analysis:
[0104] Table 1 Test results of examples and comparative examples
[0105]
[0106] A nanofiber membrane with both temperature difference power generation and wet power generation was successfully obtained through the electrospinning method of the present invention. As shown in Table 1, when comparing Example 1 to Example 7 with Comparative Example 1 to Comparative Example 3, it was found that the output voltage and current of the nanofiber membrane obtained by the embodiments of the present invention were significantly better than those of Comparative Example 1 to Comparative Example 3. Firstly, this is because the porosity and specific surface area of the nanofiber membrane are taken into consideration in the process of obtaining the nanofiber membrane by the method of the present invention. The nanofiber membrane has a porous structure, and the stability of the porous structure is the basis for realizing the nanofiber membrane. If the porous structure collapses, the fiber membrane cannot realize wet power generation. The selection of the porosity and specific surface area of the fiber membrane is a technical difficulty to further ensure that the fiber membrane can better realize the combination of temperature difference power generation and wet power generation. It can be seen from the comparison between Examples 1 to 7 and Comparative Examples 1 to 3 that in Comparative Examples 1 to 3, due to the significant difference in porosity and specific surface area between the wet differential power generation structure layer formed by the thermoelectric nanofiber film and the polyelectrolyte solution, the output voltage and current of the nanofiber membrane are significantly reduced, especially the output current, which is about 10 times different from that of Examples 1 to 7 and Comparative Examples 1 to 3.
[0107] On this basis, further studies were conducted on Examples 1 to 3, and the output voltage and current of Example 1 were significantly better than those of Examples 2 to 3. When electrospinning is performed, the output voltage and current of the nanofiber membrane can be improved by controlling the electrospinning process parameters so that the porosity and specific surface area of the layer structure formed by the thermoelectric nanofiber film and the polyelectrolyte solution are more compatible.
[0108] In the present invention, in order to further improve the power generation capacity of the nanofiber membrane, the addition amount of composite nanoparticles, bismuth telluride and polyelectrolyte is also studied. Under certain humidity conditions, water molecules dissociate the hydrophilic groups in the polyelectrolyte material to generate mobile charges. The charged ions will spontaneously diffuse in a directional manner under the action of the concentration gradient, thereby generating voltage and current. When the addition amount of polyelectrolyte increases, more charged ions with directional movement are generated, thereby increasing the output voltage and current; and composite nanoparticles and bismuth telluride can increase the conductivity and Seebeck coefficient of the fiber membrane, which is beneficial to temperature difference power generation. For example, Example 1 is compared with Example 4-Example 5. Example 1 is significantly better than Example 4. It can be seen that when the addition amount of composite nanoparticles, bismuth telluride and polyelectrolyte is reduced, the overall power generation capacity of the nanofiber membrane will be reduced. Comparing Example 4 with Example 5, it is found that increasing the addition amount of polyelectrolyte can significantly increase the output voltage and current of the nanofiber. It can be seen that, first, polyelectrolytes can enhance the ability of wet differential power generation, and second, based on the temperature differential power generation of the fiber membrane, the wet electric power generation layer in the present invention can significantly enhance the power generation capacity of the fiber membrane. It can be seen that the fiber membrane in this case can successfully combine temperature differential power generation and wet differential power generation.
[0109] Polyelectrolytes can improve the wet differential power generation capacity of fiber membranes. In the invention, it is further studied whether the selection of polyelectrolytes can further optimize the power generation capacity of nanofiber membranes. Example 1 is further compared with Example 6-Example 7. It is found that the output voltage of Example 1 is not much different from that of Example 6-Example 7, but the current of Example 1 is significantly better than that of Example 6-Example 7. This may be because sodium alginate not only has good hygroscopicity, but also causes the carboxyl groups in sodium alginate to dissociate, thereby improving the current of the fiber membrane. Therefore, sodium alginate is further preferred as the polyelectrolyte.
[0110] In summary, the nanofiber membrane of the present invention achieves the technical effects of power generation by both temperature difference and humidity difference.
[0111] It should be noted that the terms used in the present invention are only for describing specific embodiments, rather than limiting the scope of the present application. As shown in the present specification, unless the context clearly indicates an exception, the words "one", "a", "a kind of" and / or "the" do not specifically refer to the singular, but may also include the plural. The terms "include", "comprise" or any other variant thereof are intended to cover non-exclusive inclusion, so that the process, method or device including a series of elements includes not only those elements, but also includes other elements not explicitly listed, or also includes elements inherent to such process, method or device. In the absence of more restrictions, the elements defined by the sentence "include one..." do not exclude the presence of other identical elements in the process, method or device including the elements.
[0112] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a composite thermoelectric nanofiber membrane, characterized in that: The steps include: Step S1: dissolving 3,4-ethylenedioxythiophene and pyrrole in a dopant, adding an oxidant dropwise, performing polymerization reaction, solid-liquid separation, and drying to obtain composite nanoparticles; Step S2: mixing the solution containing the composite nanoparticles with the bismuth telluride solution to prepare a dispersion for electrostatic spinning to obtain a thermoelectric nanofiber film; Step S3: Spraying the polyelectrolyte solution onto the thermoelectric nanofiber film by electrospinning to obtain a composite thermoelectric nanofiber membrane; the specific surface area of the composite thermoelectric nanofiber membrane is 18 m 2 / g-26m 2 / g, porosity is 75%-85%; The mass concentration of the bismuth telluride solution is 15%-25%; After mixing, the mass concentration of the composite nanoparticles is 1.5%-3%; The mass concentration of the polyelectrolyte solution is 10%-30%; The electrospinning parameters in step S2 are as follows: voltage of 16 kv-24 kv, spinning speed of 1 mL / h-3 mL / h, and receiving distance of 15 cm-20 cm; The specific parameters of the electrospinning in step S3 are: voltage of 16 kv-24 kv, spinning speed of 1 mL / h-3 mL / h, and receiving distance of 15 cm-20 cm.
2. The preparation method according to claim 1, characterized in that: The oxidant includes one or more of persulfate and salt containing iron ions; The dopant includes a compound containing a sulfonate ion.
3. The preparation method according to claim 1, characterized in that: The mass ratio of 3,4-ethylenedioxythiophene to pyrrole is 1-3:1; The molar concentration of 3,4-ethylenedioxythiophene in the dopant is 0.3 mol / L-0.8 mol / L.
4. The preparation method according to claim 1, characterized in that: The polymerization reaction conditions include: temperature of -15°C to -24°C and time of 48h to 96h.
5. The preparation method according to claim 1, characterized in that: The mass ratio of the bismuth telluride to the composite nanoparticles is 1:1-6.
6. The preparation method according to claim 1, characterized in that: The polyelectrolyte in the polyelectrolyte solution includes one or more of polystyrene sulfonic acid, sodium polystyrene sulfonate, polyacrylic acid, sodium alginate, hydroxymethyl cellulose, and polyethylene imine.
7. A composite moist heat electric nanofiber membrane obtained by the method for preparing a composite moist heat electric nanofiber membrane according to any one of claims 1 to 6.