A double-sided deposition battery preparation method, back contact battery and photovoltaic module

By adopting a double-sided deposition method in the preparation process of the back contact battery, and using the gas port set by the quartz boat and the limiter to communicate with the cavity, the simultaneous deposition of the front and back sides of the silicon wafer is achieved, solving the deposition efficiency problem in the existing technology. solve the problems of low and poor economic benefits and improve production efficiency and product quality.

CN118486764BActive Publication Date: 2024-10-18GOLD STONE (FUJIAN) ENERGY CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410939867.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-10-18
Estimated Expiration
2044-07-15

AI Technical Summary

Technical Problem

The existing back-contact battery preparation process requires sequential deposition of the front and back sides of the silicon wafer, resulting in low deposition efficiency, long production cycle, and low economic benefits.

Method used

The battery preparation method of double-sided deposition is adopted, and the first semiconductor layer and the second semiconductor layer are simultaneously deposited on the back and front sides of the silicon wafer through a quartz boat. The gas passage port set by the limiter is connected to the cavity to independently control the reaction gas flow. Achieve deposition of polysilicon layers with different thicknesses and doping concentrations.

Benefits of technology

It improves the deposition efficiency, reduces equipment costs, shortens the production cycle, improves economic benefits, and realizes the deposition of polysilicon layers of different thicknesses on both sides of the silicon wafer, improving product quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118486764B_ABST
    Figure CN118486764B_ABST
Patent Text Reader

Abstract

The invention discloses a double-sided deposition battery preparation method, a back contact battery and a photovoltaic module, and relates to the technical field of back contact batteries. The double-sided deposition battery preparation method is provided with a first gas path opening and a second gas path opening on both sides of a stopper, so that a first airflow channel is connected to a first cavity located on the back side of a silicon wafer through the first gas path opening, and a second airflow channel is connected to a second cavity located on the front side of the silicon wafer through the second gas path opening, and a reaction gas can be introduced to the back side and the front side of the silicon wafer through the first gas path opening at the same time, so as to realize simultaneous deposition on the back side and the front side of the silicon wafer, improve deposition efficiency, reduce equipment cost, and improve economic benefits, and can independently control the flow rate of the reaction gas in the first gas path opening and the second gas path opening, so as to realize the deposition of polysilicon layers with different thicknesses and different doping concentrations on the back side and the front side of the silicon wafer, further reducing equipment cost and improving economic benefits.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of back-contact batteries, and in particular relates to a double-sided deposition battery preparation method, a back-contact battery and a photovoltaic module. Background Art

[0002] At present, in the application of tunneling polycrystalline passivation process, a thinner polysilicon layer is required on the front of the back contact cell to reduce optical absorption and increase current, and a thicker polysilicon layer is required on the back of the back contact cell to ensure the conductivity of the film layer and prevent the back polycrystalline from being damaged by chemical solutions. However, the tunneling polycrystalline is generally prepared by tubular PECVD (plasma enhanced chemical vapor deposition), which can only achieve single-sided deposition each time, so it takes two depositions to complete the coating of the front and back of the silicon wafer, with low deposition efficiency, high equipment cost, long production cycle and low economic benefits.

[0003] It should be noted that this part of the present invention only provides background technology related to the present invention and does not necessarily constitute prior art or known technology. Summary of the invention

[0004] The purpose of the present invention is to overcome the defects of the prior art that the front and back sides of the silicon wafer need to be deposited sequentially during the preparation of the back-contact cell, resulting in low deposition efficiency, long production cycle and low economic benefits. A double-sided deposition cell preparation method, a back-contact cell and a photovoltaic module are provided. The double-sided deposition cell preparation method can simultaneously perform deposition processing on the front and back sides of the silicon wafer, effectively improving the deposition efficiency, reducing equipment costs, shortening the production cycle, and improving economic benefits. The flow rate of the reaction gas to the front and back sides of the silicon wafer can be independently controlled, thereby realizing the deposition of polysilicon layers of different thicknesses on both sides of the silicon wafer, further reducing equipment costs and improving economic benefits.

[0005] In order to achieve the above object, in a first aspect, the present invention provides a method for preparing a double-sided deposited battery, comprising the following steps:

[0006] S1. Provide double-sided polished silicon wafers;

[0007] S2. depositing a protective layer on the back side of the silicon wafer;

[0008] S3. A velvet surface is formed on the front side of the silicon wafer by velvet cleaning, and then the protective layer is removed;

[0009] S4. Using a quartz boat, a first semiconductor layer and a second semiconductor layer are deposited on the back and front of a silicon wafer respectively at the same time, wherein the first semiconductor layer includes a first tunneling oxide layer and a first polysilicon layer which are arranged in sequence, and the second semiconductor layer includes a second tunneling oxide layer and a second polysilicon layer which are arranged in sequence, wherein the first polysilicon layer and the second polysilicon layer have different thicknesses, the quartz boat includes a shell, and a stopper installed in the shell, a first airflow channel, and a second airflow channel, the first airflow channel is provided with a first air path opening on one side of the stopper, and the second airflow channel is provided with a second air path opening on the other side of the stopper, and the stopper is used to limit the silicon wafer so that the first air path opening is connected to a first cavity located on the back of the silicon wafer, and the second air path opening is connected to a second cavity located on the front of the silicon wafer;

[0010] S5. coating a phosphorus source on the first polysilicon layer and the second polysilicon layer respectively, and performing high temperature annealing to form a first doped layer and a second doped layer, wherein the surface doping index of the first doped layer is 6.7e17-4e18, and the surface doping index of the second doped layer is 2.7e17-3.3e18, and the surface doping index is the ratio of the effective doping concentration of the doped layer to the thickness of the doped layer;

[0011] S6. Cleaning and removing the phosphosilicate glass layer on the first doped layer and the second doped layer due to annealing in S5;

[0012] S7. forming a mask layer on the first doped layer, and then forming an anti-reflection layer on the second doped layer;

[0013] S8. Etching an opening on the first tunneling oxide layer, the first doping layer and the mask layer to form a first opening region;

[0014] S9. Cleaning and removing the first tunneling oxide layer, the first doping layer and the mask layer remaining in the first opening region, and then cleaning and removing the mask layer outside the first opening region;

[0015] S10. Depositing a third semiconductor layer on the back side of the silicon wafer so that a portion of the third semiconductor layer covers the side of the first semiconductor layer away from the silicon wafer, and another portion extends into the first opening area and covers the silicon wafer, the third semiconductor layer comprising an intrinsic amorphous silicon layer and a third doped layer arranged in sequence.

[0016] Preferably, the limiting member is provided with a limiting groove, and the silicon chip is embedded in the limiting groove.

[0017] Preferably, the first airflow channel and the second airflow channel are relatively arranged at two ends of the limiting component, the first airflow channel is provided with a first external interface, and the second airflow channel is provided with a second external interface.

[0018] Preferably, there are multiple limit members, which are arranged in parallel and spaced apart, and an air intake gap is formed between two adjacent limit members. The number of first air path openings and second air path openings are both multiple, and the multiple first air path openings and the multiple second air path openings are alternately arranged in sequence and are connected to the multiple air intake gaps one by one.

[0019] Preferably, S4 includes: evacuating the outer shell; introducing oxygen into the first cavity through the first gas outlet, and introducing oxygen into the second cavity through the second gas outlet, until a preset air pressure is reached in the outer shell; maintaining the pressure and stuffing oxygen to form a first tunneling oxide layer on the back side of the silicon wafer, and a second tunneling oxide layer on the front side of the silicon wafer, and the thickness of the first tunneling oxide layer and the second tunneling oxide layer are both 1nm-2nm; introducing a first flow rate of silane into the first cavity through the first gas outlet, and introducing a second flow rate of silane into the second cavity through the second gas outlet, the first flow rate being greater than the second flow rate, so as to react on the first tunneling oxide layer to form a first polysilicon layer, and react on the second tunneling oxide layer to form a second polysilicon layer, the thickness of the first polysilicon layer is 100nm-150nm, and the thickness of the second polysilicon layer is 15nm-30nm.

[0020] Preferably, in S4, the holding conditions are: the preset air pressure is 10000Pa-30000Pa, the holding time is 900s-1800s, and the holding temperature is 550°C-650°C;

[0021] And / or, the reaction conditions for forming the first polysilicon layer and the second polysilicon layer are: the first flow rate is 400sccm-600sccm, the second flow rate is 50sccm-80sccm, the reaction temperature is 550℃-650℃, the reaction gas pressure is 30pa-60pa, and the reaction time is 1300s-1600s.

[0022] Preferably, S5 includes: coating a phosphorus source with a first phosphoric acid concentration on the surface of the first polysilicon layer by spraying, and coating a phosphorus source with a second phosphoric acid concentration on the surface of the second polysilicon layer; introducing nitrogen gas for high temperature annealing to convert the first polysilicon layer into a first doped layer, and converting the second polysilicon layer into a second doped layer, wherein the phosphorus doping concentration in the first doped layer is 1e20cm -3 -4e20cm -3 The phosphorus doping concentration in the second doping layer is 8e18cm -3 -5e19cm -3 .

[0023] Preferably, in S5, the coating conditions are: the first phosphoric acid concentration is 10%-15%, and the second phosphoric acid concentration is 3%-5%;

[0024] And / or, the annealing conditions are: annealing temperature is 850° C.-900° C., nitrogen flow rate is 1000 sccm-3000 sccm, and annealing time is 10 min-30 min.

[0025] Preferably, in S3, the texturing cleaning conditions are: the texturing time is 8min-40min, the texturing temperature is 65℃-85℃, the texturing liquid is a mixture of potassium hydroxide, texturing additives and water, wherein the mass percentage of potassium hydroxide is 1%-5%, and the mass percentage of the texturing additive is 0.5%-1%.

[0026] Preferably, after S10, the method for preparing a double-sided deposition battery further comprises:

[0027] S11. Etching openings on the third semiconductor layer to form second opening regions that are alternately arranged with the first opening regions and spaced apart;

[0028] S12 forming a conductive film layer on the back side of the silicon wafer;

[0029] S13. An isolation groove is formed on the conductive film layer so that a portion of the conductive film layer separated from each other extends into the first opening region and covers the third semiconductor layer, and another portion extends into the second opening region and covers the first semiconductor layer;

[0030] S14. Form a first electrode on the portion of the conductive film layer extending into the first opening region, and form a second electrode on the portion of the conductive film layer extending into the second opening region.

[0031] In a second aspect, the present invention provides a back-contact battery, which is prepared by the above-mentioned double-sided deposition battery preparation method.

[0032] In a third aspect, the present invention provides a photovoltaic module comprising the above-mentioned back contact cell.

[0033] Beneficial effects:

[0034] Through research, it is found that in the application of tunneling polycrystalline passivation process, polycrystalline silicon layers need to be deposited on both the front and back sides of the silicon wafer, and the thickness of the polycrystalline silicon layers on the two sides is different. The thinner polycrystalline silicon layer on the front side can reduce optical absorption and increase current, and the thicker polycrystalline silicon layer on the back side can ensure the conductivity of the film layer and prevent the back polycrystalline from being damaged by chemical solutions. It is well known that the current tubular PECVD can only achieve single-sided deposition, and the deposition efficiency is low. Based on this, further research is conducted to propose the present invention.

[0035] The present invention adopts the above-mentioned technical scheme, especially the first gas path opening and the second gas path opening are respectively arranged on both sides of the limit member, so that the first air flow channel is connected with the first cavity located on the back side of the silicon wafer through the first gas path opening, and the second air flow channel is connected with the second cavity located on the front side of the silicon wafer through the second gas path opening. The reaction gas can be introduced to the back side and the front side of the silicon wafer through the first air flow channel and the second air flow channel at the same time to realize simultaneous deposition on the back side and the front side of the silicon wafer, improve deposition efficiency, reduce equipment cost, shorten production cycle, and improve economic benefits. In addition, the flow rate of the reaction gas in the first air flow channel and the second air flow channel can be independently controlled to realize the deposition of polysilicon layers of different thicknesses and different doping concentrations on the back side and the front side of the silicon wafer, and the surface doping index of the back side and the front side can be controlled at the same time to improve conversion efficiency, further reduce equipment cost, and improve economic benefits.

[0036] The back contact battery prepared by the present invention has a better deposition effect and better product quality. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0038] Figure 1 A schematic structural diagram of a quartz boat applied to S4 in an embodiment of the present invention from one perspective;

[0039] Figure 2 A schematic structural diagram of a quartz boat applied to S4 in another perspective in an embodiment of the present invention;

[0040] Figure 3 This is a schematic diagram of the structure of a quartz boat applied to S4 in an embodiment of the present invention after loading silicon wafers;

[0041] Figure 4 This is a schematic diagram of the structure of a silicon wafer after double-sided polishing and cleaning according to an embodiment of the present invention;

[0042] Figure 5 This is a schematic diagram of the structure of forming a protective layer on the back side of a silicon wafer according to an embodiment of the present invention;

[0043] Figure 6 This is a schematic diagram of the structure in which a velvet surface is formed on the front side of a silicon wafer and a protective layer on the back side is removed according to an embodiment of the present invention;

[0044] Figure 7 This is a schematic diagram of a structure in which a first semiconductor layer is formed on the back side of a silicon wafer and a second semiconductor layer is formed on the front side in an embodiment of the present invention;

[0045] Figure 8 This is a schematic diagram of a structure in which a first doping layer and a mask layer 9 are formed on the back side of a silicon wafer and a second doping layer and an anti-reflection layer are formed on the front side in an embodiment of the present invention;

[0046] Fig. 9 This is a schematic diagram of a structure in which a first opening area is formed on the back side of a silicon wafer according to an embodiment of the present invention;

[0047] Fig.10 This is a schematic diagram of a structure in which a third semiconductor layer and a second opening area are formed on the back side of a silicon wafer according to an embodiment of the present invention;

[0048] Fig.11 This is a schematic diagram of the structure of forming a conductive film layer and an isolation groove on the back side of a silicon wafer according to an embodiment of the present invention;

[0049] Fig.12 This is a schematic diagram of the structure of forming a first electrode and a second electrode on the back side of a silicon wafer according to an embodiment of the present invention.

[0050] Description of Reference Numerals

[0051] 1-silicon wafer; 2-protective layer; 3-first tunneling oxide layer; 4-first polysilicon layer; 5-second tunneling oxide layer; 6-second polysilicon layer; 7-first doping layer; 8-second doping layer; 9-mask layer; 10-anti-reflection layer; 11-intrinsic amorphous silicon layer; 12-third doping layer; 13-conductive film layer; 14-first electrode; 15-second electrode; 100-quartz boat; 110-housing; 120-limiting piece; 121-limiting groove; 122-air inlet gap; 130-first air flow channel; 131-first air path opening; 140-second air flow channel; 141-second air path opening; 150-first cavity; 160-second cavity. DETAILED DESCRIPTION

[0052] In the present invention, unless otherwise specified, directional words such as "upper, lower, left, right" are generally understood in conjunction with the directions shown in the drawings and actual applications.

[0053] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.

[0054] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Moreover, a first feature being "above", "above" or "above" a second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being "below", "below" or "below" a second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.

[0055] The endpoints and any values ​​of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article. Among them, the terms "optional" and "optional" all mean that they may be included or not included (or may be present or not).

[0056] First, please refer to Figures 1 to 12 The present invention provides a double-sided deposition battery preparation method, in which a first gas path opening 131 and a second gas path opening 141 are respectively arranged on both sides of a limiter 120, so that the first gas flow channel 130 is connected to the first cavity 150 located on the back side of the silicon wafer 1 through the first gas path opening 131, and the second gas flow channel 140 is connected to the second cavity 160 located on the front side of the silicon wafer 1 through the second gas path opening 141, and the reaction gas can be introduced to the back side and the front side of the silicon wafer 1 through the first gas flow channel 130 and the second gas flow channel 140 at the same time, so as to realize simultaneous deposition on the back side and the front side of the silicon wafer 1, improve deposition efficiency, reduce equipment cost, shorten production cycle, and improve economic benefits, and can independently control the flow rate of reaction gas in the first gas flow channel 130 and the second gas flow channel 140, so as to realize deposition of polysilicon layers of different thicknesses and different doping concentrations on the back side and the front side of the silicon wafer 1, and control the doping index of the back side and the front side at the same time, improve conversion efficiency, further reduce equipment cost, and improve economic benefits.

[0057] The method for preparing a double-sided deposition battery comprises the following steps:

[0058] S1 provides a double-sided polished silicon wafer 1;

[0059] S2. Depositing a protective layer 2 on the back of the silicon wafer 1;

[0060] S3. By cleaning the velvet surface, a velvet surface is formed on the front side of the silicon wafer 1, and then the protective layer 2 is removed;

[0061] S4. Using a quartz boat 100, a first semiconductor layer and a second semiconductor layer are deposited on the back and front sides of the silicon wafer 1, respectively. The first semiconductor layer includes a first tunneling oxide layer 3 and a first polysilicon layer 4, which are sequentially arranged. The second semiconductor layer includes a second tunneling oxide layer 5 and a second polysilicon layer 6, which are sequentially arranged. The first polysilicon layer 4 and the second polysilicon layer 6 have different thicknesses.

[0062] S5. Coating a phosphorus source on the first polysilicon layer 4 and the second polysilicon layer 6, respectively, and performing high temperature annealing to form a first doping layer 7 and a second doping layer 8, wherein the surface doping index of the first doping layer 7 is 6.7e17-4e18, and the surface doping index of the second doping layer 8 is 2.7e17-3.3e18, and the surface doping index is the ratio of the effective doping concentration of the doping layer to the thickness of the doping layer;

[0063] S6. Cleaning and removing the phosphosilicate glass layer produced by annealing S5 on the first doped layer 7 and the second doped layer 8;

[0064] S7. A mask layer 9 is formed on the first doped layer 7, and then an anti-reflection layer 10 is formed on the second doped layer 8;

[0065] S8. Etching an opening on the first tunneling oxide layer 3, the first doping layer 7 and the mask layer 9 to form a first opening region;

[0066] S9. Cleaning and removing the first tunneling oxide layer 3, the first doping layer 7 and the mask layer 9 remaining in the first opening region, and then cleaning and removing the mask layer 9 outside the first opening region;

[0067] S10. A third semiconductor layer is deposited on the back side of the silicon wafer 1 so that a portion of the third semiconductor layer covers the side of the first semiconductor layer away from the silicon wafer 1, and another portion extends into the first opening area and covers the silicon wafer 1, wherein the third semiconductor layer includes an intrinsic amorphous silicon layer 11 and a third doped layer 12 arranged in sequence.

[0068] like Figures 1 to 3As shown, the quartz boat 100 includes a shell 110, a stopper 120, a first airflow channel 130 and a second airflow channel 140. The stopper 120, the first airflow channel 130 and the second airflow channel 140 are all installed in the shell 110, and the shell 110 is used to carry and position the stopper 120, the first airflow channel 130 and the second airflow channel 140, and a closed cavity is formed in the shell 110 for deposition. Specifically, the first airflow channel 130 is provided with a first air path opening 131 on one side of the stopper 120, and the second airflow channel 140 is provided with a second air path opening 141 on the other side of the stopper 120. The stopper 120 is used to limit the silicon wafer 1 so that the first air path opening 131 is connected to the first cavity 150 located on the back side of the silicon wafer 1, and the second air path opening 141 is connected to the second cavity 160 located on the front side of the silicon wafer 1.

[0069] It is worth noting that the limiting member 120 is provided with a limiting groove 121, and the silicon wafer 1 is embedded in the limiting groove 121. The limiting member 120 can limit and fix the silicon wafer 1 through the limiting groove 121 to prevent the silicon wafer 1 from shifting relative to the limiting member 120 during the deposition process, thereby ensuring the deposition effect of the silicon wafer 1.

[0070] Preferably, the first airflow channel 130 and the second airflow channel 140 are relatively arranged at the two ends of the stopper 120 to realize the staggered arrangement of the first airflow channel 130 and the second airflow channel 140, so as to facilitate the first airflow channel 130 to pass the reaction gas to the first cavity 150 located on the back side of the silicon wafer 1 through the first gas path opening 131, and at the same time facilitate the second airflow channel 140 to pass the reaction gas to the second cavity 160 located on the front side of the silicon wafer 1 through the second gas path opening 141. Specifically, the first airflow channel 130 is provided with a first external interface, and the second airflow channel 140 is provided with a second external interface, and the first external interface and the second external interface are both used to connect to an external gas pipe to facilitate the introduction of the reaction gas.

[0071] Furthermore, there are multiple limiting members 120 , which are arranged in parallel and spaced apart. Each limiting member 120 is used to limit a silicon wafer 1 , and the multiple limiting members 120 work together to allow multiple silicon wafers 1 to be arranged in parallel and spaced apart. Specifically, an air intake gap 122 is formed between two adjacent limit members 120, and the air intake gap 122 is connected to the cavity between two adjacent silicon wafers 1. The number of first air openings 131 and second air openings 141 is multiple, and the multiple first air openings 131 and the multiple second air openings 141 are alternately arranged in sequence and are connected to the multiple air intake gaps 122 one by one, that is, in the arrangement direction of the multiple silicon wafers 1, the first first air opening 131 is connected to the cavity between the first silicon wafer 1 and the second silicon wafer 1 through an air intake gap 122, the first second air opening 141 is connected to the cavity between the second silicon wafer 1 and the third silicon wafer 1 through an air intake gap 122, the second first air opening 131 is connected to the cavity between the third silicon wafer 1 and the fourth silicon wafer 1 through an air intake gap 122, and the second second air opening 141 is connected to the cavity between the fourth silicon wafer 1 and the fifth silicon wafer 1 through an air intake gap 122, and this cycle is repeated. In addition, the first air flow channel 130 is further provided with a first air path opening 131 outside a limiter 120 at one end, and the second air flow channel 140 is further provided with a second air path opening 141 outside a limiter 120 at the other end, so as to realize the deposition function on the outer side surfaces of the two silicon wafers 1 at the end.

[0072] It can be understood that the plurality of silicon wafers 1 are arranged in parallel and spaced apart. In one case, the back surfaces of two adjacent silicon wafers 1 are arranged opposite to each other. In this case, the cavity between the two silicon wafers 1 is a first cavity 150, and the first cavity 150 is connected to a first gas path opening 131 through an air inlet gap 122. In another case, the front surfaces of two adjacent silicon wafers 1 are arranged opposite to each other. In this case, the cavity between the two silicon wafers 1 is a second cavity 160, and the second cavity 160 is connected to a second gas path opening 141 through an air inlet gap 122. In this way, a plurality of first cavities 150 and a plurality of second cavities 160 are formed between the plurality of silicon wafers 1. The plurality of first cavities 150 and the plurality of second cavities 160 are arranged alternately in sequence. The plurality of first cavities 150 correspond to the plurality of first gas paths openings 131 one by one, and the plurality of second cavities 160 correspond to the plurality of second gas paths openings 141 one by one.

[0073] It should be noted that, in S1, the silicon wafer 1 is preferably an N-type single crystal silicon wafer, and the silicon wafer 1 can be a Czochralski single crystal silicon wafer or a cast single crystal silicon wafer.

[0074] In S2, a protective layer 2 is deposited on the back of the silicon wafer 1 by sputtering or chemical vapor doping, wherein the protective layer 2 is a silicon nitride protective layer 2. The silicon nitride protective layer 2 has a strong resistance to corrosion by alkaline solutions and can resist alkaline corrosion in the texturing solution and protect the silicon wafer 1. The thickness of the protective layer 2 is 50nm-100nm. A reasonable thickness of the protective layer 2 can maintain the integrity of the polishing surface and is conducive to improving the passivation level.

[0075] In S3, the silicon wafer 1 is subjected to single-sided texturing to form a pyramid texturing surface on the front side to reduce the reflectivity. In this process, since a protective layer 2 is provided on the back side of the silicon wafer 1, the texturing liquid will not affect the back side of the silicon wafer 1. After the texturing is completed, the protective layer 2 is removed, and the back side of the silicon wafer 1 is a polished surface. The texturing cleaning conditions are: the texturing time is 8min-40min, the texturing temperature is 65℃-85℃, the texturing liquid is an alkaline mixed solution, and the texturing liquid is a mixture of potassium hydroxide, a texturing additive and water, wherein the mass percentage of potassium hydroxide is 1%-5%, the mass percentage of the texturing additive is 0.5%-1%, and the texturing additive contains at least one of benzoic acid, aminotrimethylphosphonic acid, polyepoxysuccinic acid, and polyaspartic acid.

[0076] S4 includes: using LPCVD (low pressure chemical vapor deposition) equipment to deposit silicon wafer 1 through quartz boat 100, first evacuating housing 110; then introducing oxygen into first cavity 150 through first gas port 131, and simultaneously introducing oxygen into second cavity 160 through second gas port 141, until a preset pressure is reached in housing 110; then maintaining the pressure and stuffing oxygen to form a first tunneling oxide layer 3 on the back side (velvet surface) of silicon wafer 1, and forming a second tunneling oxide layer 5 on the front side (polished surface) of silicon wafer 1, the thickness of first tunneling oxide layer 3 and second tunneling oxide layer 5 are both 1nm-2nm ( In this process, since the oxygen flow rate into the first cavity 150 is the same as the oxygen flow rate into the second cavity 160, the thickness of the first tunnel oxide layer 3 and the second tunnel oxide layer 5 are the same); then, a first flow rate of silane is introduced into the first cavity 150 through the first gas path port 131 of the first gas flow channel 130, and a second flow rate of silane is introduced into the second cavity 160 through the second gas path port 141 of the second gas flow channel 140, and the first flow rate is greater than the second flow rate, so as to react and form a first polysilicon layer 4 on the first tunnel oxide layer 3, and react and form a second polysilicon layer 6 on the second tunnel oxide layer 5. Among them, the thickness of the first polysilicon layer 4 is 100nm-150nm, and the thickness of the second polysilicon layer 6 is 15nm-30nm. A reasonable thickness of the first polysilicon layer 4 can improve the passivation level, which is conducive to improving the open circuit voltage, and a reasonable thickness of the second polysilicon layer 6 can reduce the parasitic absorption of the film layer, which is conducive to improving the short circuit current. In this way, the deposition of polysilicon layers of different thicknesses on the back and front sides of the silicon wafer 1 is achieved simultaneously, which greatly improves the deposition efficiency, reduces the equipment cost, shortens the production cycle, and improves the economic benefits.

[0077] Preferably, in S4, the pressure holding conditions are: the preset air pressure is 10000Pa-30000Pa, the pressure holding time is 900s-1800s, and the pressure holding temperature is 550℃-650℃.

[0078] Preferably, in S4, the reaction conditions for forming the first polysilicon layer 4 and the second polysilicon layer 6 are: the first flow rate is 400sccm-600sccm, the second flow rate is 50sccm-80sccm, the reaction temperature is 550℃-650℃, the reaction gas pressure is 30pa-60pa, and the reaction time is 1300s-1600s.

[0079] S5 includes: firstly, coating a phosphorus source with a first phosphoric acid concentration on the surface of the first polysilicon layer 4 by spraying, and coating a phosphorus source with a second phosphoric acid concentration on the surface of the second polysilicon layer 6; then introducing nitrogen gas for high temperature annealing to convert the first polysilicon layer 4 into a first doped layer 7, and convert the second polysilicon layer 6 into a second doped layer 8. Among them, the surface doping index of the first doped layer 7 is 6.7e17-4e18, and the surface doping index of the second doped layer 8 is 2.7e17-3.3e18. A reasonable surface doping index of the first doped layer 7 can improve the field passivation effect, reduce the contact resistance, and help to improve the open circuit voltage and short circuit current. A reasonable surface doping index of the second doped layer 8 can improve the field passivation effect and help to improve the open circuit voltage; the phosphorus doping concentration in the first doped layer 7 is 1e20cm -3 -4e20cm -3 The phosphorus doping concentration in the second doping layer 8 is 8e18cm -3 -5e19cm -3 A reasonable phosphorus doping concentration in the first doping layer 7 can improve the field passivation effect, reduce the contact resistance, and help improve the open circuit voltage and short circuit current. A reasonable phosphorus doping concentration in the second doping layer 8 can improve the field passivation effect and help improve the open circuit voltage.

[0080] Preferably, in S5, the coating conditions are: the first phosphoric acid concentration is 10%-15%, and the second phosphoric acid concentration is 3%-5%.

[0081] Preferably, in S5, the annealing conditions are: annealing temperature is 850° C.-900° C., nitrogen flow rate is 1000 sccm-3000 sccm, and annealing time is 10 min-30 min.

[0082] In S6, the cleaning conditions are: cleaning time is 3 min-5 min, cleaning temperature is 20° C.-30° C., and the cleaning solution is a hydrofluoric acid solution, wherein the mass percentage of hydrofluoric acid is 5%-10%, and the mass percentage of deionized water is 90%-95%.

[0083] In S7, a mask layer 9 is deposited on the first doped layer 7 on the back of the silicon wafer 1 by using a tubular PECVD (plasma enhanced chemical vapor deposition) method, and then an anti-reflection layer 10 is deposited on the second doped layer 8 on the front of the silicon wafer 1. The mask layer 9 and the anti-reflection layer 10 are both silicon nitride layers, the thickness of the mask layer 9 is 60nm-90nm, and the thickness of the anti-reflection layer 10 is 100nm-150nm. The reaction conditions for forming the mask layer 9 are: introducing a mixed gas of silane and ammonia, turning on the glow, the reaction temperature is 400℃-450℃, the silane flow rate is 1200sccm-1600sccm, the ammonia flow rate is 3000sccm-5000sccm, the reaction time is 400s-800s, the reaction pressure is 500mtorr-3000mtorr, and the reaction power is 4000W-6000W. The reaction conditions for forming the anti-reflection layer 10 are: introducing a mixed gas of silane and ammonia, turning on the glow, the reaction temperature is 400°C-450°C, the silane flow rate is 1200sccm-1600sccm, the ammonia flow rate is 5000sccm-8000sccm, the reaction time is 1000s-1500s, the reaction pressure is 500mtorr-3000mtorr, and the reaction power is 4000W-6000W.

[0084] In S8, laser or mask etching is used to etch an opening on the mask layer 9, the first doping layer 7 and the first tunneling oxide layer 3 on the back of the silicon wafer 1 to form a first opening area, and the mask layer 9, the first doping layer 7 and the first tunneling oxide layer 3 in the first opening area are etched away. The width of the first opening area W1 is 0.3 mm-0.6 mm. Laser etching is preferred, and the laser used for etching is an ultraviolet laser or a green laser, and the pulse width is less than 100 ns.

[0085] In S9 , the first tunneling oxide layer 3 , the first doping layer 7 and the mask layer 9 remaining in the first opening region are removed by water rinsing; and then the mask layer 9 outside the first opening region is cleaned and removed.

[0086] In S10, a third semiconductor layer is deposited on the back side of the silicon wafer 1 by PECVD (plasma enhanced chemical vapor deposition), wherein the intrinsic amorphous silicon layer 11 has a thickness of 5nm-15nm, the third doped layer 12 is a P-type doped amorphous or microcrystalline silicon layer, the thickness of the third doped layer 12 is 10nm-35nm, and the boron doping concentration in the third doped layer 12 is 1e19cm -3 -4e20cm -3 .

[0087] Preferably, after S10, the method for preparing a double-sided deposition battery further comprises:

[0088] S11. Etching openings on the third semiconductor layer to form second opening regions that are alternately arranged with the first opening regions and spaced apart;

[0089] S12 forming a conductive film layer 13 on the back side of the silicon wafer 1;

[0090] S13. An isolation groove is formed on the conductive film layer 13 so that a portion of the conductive film layer 13 separated from each other extends into the first opening region and covers the third semiconductor layer, and another portion extends into the second opening region and covers the first semiconductor layer;

[0091] S14. Form a first electrode 14 on the portion of the conductive film layer 13 extending into the first opening region, and form a second electrode 15 on the portion of the conductive film layer 13 extending into the second opening region.

[0092] It should be noted that in S11, an opening is etched on the third semiconductor layer on the back of the silicon wafer 1 by laser or mask etching to form a second opening area, and the third semiconductor layer in the second opening area is etched away. The width of the second opening area W2 is 0.1 mm-0.3 mm. Laser etching is preferred, and the etching laser is an ultraviolet laser or a green laser, and the pulse width is less than 50 ns.

[0093] In S12, a conductive film layer 13 is deposited on the back side of the silicon wafer 1 by physical vapor deposition technology (PVD) or activated plasma deposition technology (RPD). The thickness of the conductive film layer 13 is 40nm-80nm. The material of the conductive film layer 13 can be an indium oxide film doped with tin oxide, titanium oxide, zinc oxide or gallium oxide, or a zinc oxide film doped with aluminum oxide, gallium oxide or boron oxide.

[0094] In S13, an isolation groove is formed on the conductive film layer 13 by laser or etching. The isolation groove is used to achieve the insulation function between two adjacent parts of the conductive film layer 13. The isolation groove is located between the first opening area and the second opening area. The width of the isolation groove W3 is 30μm-200μm.

[0095] In S14, a silver gate electrode may be formed by screen printing and low temperature sintering, or a gate line electrode may be formed by electroplating. Preferably, the gate line electrode is formed by electroplating (the first electrode 14 and the second electrode 15 are both formed by electroplating).

[0096] In a second aspect, the present invention provides a back-contact battery, which is prepared by the above-mentioned double-sided deposition battery preparation method.

[0097] In a third aspect, the present invention provides a photovoltaic module comprising the above-mentioned back contact cell.

[0098] The embodiments of the present invention are described in detail below, which are exemplary and are only used to explain the present invention, and should not be construed as limiting the present invention.

[0099] Example 1

[0100] A back contact battery is prepared by the following steps:

[0101] S1. Figure 4 As shown, the N-type single crystal silicon wafer 1 is double-sided polished and cleaned, and the silicon wafer 1 is a Czochralski single crystal silicon wafer.

[0102] S2. Figure 5 As shown, a protection layer 2 is deposited on the back side of the silicon wafer 1 by sputtering, and the thickness of the protection layer 2 is 70 nm.

[0103] S3. Figure 6 As shown, a textured surface is formed on the front side of the silicon wafer 1 through textured cleaning, and then the protective layer 2 is removed, wherein the textured cleaning conditions are: the textured time is 20 minutes, the textured temperature is 75°C, the textured liquid is an alkaline mixed solution, and the textured liquid is a mixture of potassium hydroxide, a textured additive and water, wherein the mass percentage of potassium hydroxide is 3%, the mass percentage of the textured additive is 0.75%, and the textured additive contains benzoic acid and aminotri(methylene)phosphoric acid.

[0104] S4. Figure 7 As shown, a quartz boat 100 is used to simultaneously deposit a first semiconductor layer and a second semiconductor layer on the back and front sides of a silicon wafer 1, respectively. The deposition process is as follows:

[0105] In the first stage, vacuum is first drawn, and then oxygen is introduced until the pressure reaches 20000 Pa, and then the oxygen is stopped, and the pressure is maintained for 2200 seconds. The pressure maintenance temperature is 600°C, and the thickness of the first tunneling oxide layer 3 and the second tunneling oxide layer 5 formed are both 1.5 nm;

[0106] In the second stage, silane is introduced, the first flow rate into the first air flow channel 130 is 500sccm, the second flow rate into the second air flow channel 140 is 60sccm, the reaction temperature is 600°C, the pressure is 40pa, the reaction time is 1400s, and the thickness of the formed first polysilicon layer 4 is 120nm, and the thickness of the second polysilicon layer 6 is 20nm.

[0107] S5. Figure 8 As shown, a phosphorus source is coated on the first polysilicon layer 4 and the second polysilicon layer 6, respectively, and high temperature annealing is performed to form a first doping layer 7 and a second doping layer 8. The surface doping index of the first doping layer 7 is 6.9e17, the surface doping index of the second doping layer 8 is 3.1e18, and the phosphorus doping concentration in the first doping layer 7 is 3e20cm -3 The phosphorus doping concentration in the second doping layer 8 is 4e19cm -3The coating conditions are as follows: the first phosphoric acid concentration is 12%, the second phosphoric acid concentration is 4%; the annealing conditions are as follows: the annealing temperature is 880° C., the nitrogen flow rate is 2000 sccm, and the annealing time is 20 min.

[0108] S6. Clean and remove the phosphosilicate glass layer produced by annealing in S5 on the first doping layer 7 and the second doping layer 8, wherein the cleaning conditions are: cleaning time is 5 minutes, cleaning temperature is 20° C., and the cleaning solution is a hydrofluoric acid solution, wherein the mass percentage of hydrofluoric acid is 5%, and the mass percentage of deionized water is 95%.

[0109] S7. Figure 8 As shown, a mask layer 9 is formed on the first doping layer 7, and then an anti-reflection layer 10 is formed on the second doping layer 8. The thickness of the mask layer 9 is 80 nm, and the thickness of the anti-reflection layer 10 is 120 nm. The reaction conditions for forming the mask layer 9 are: reaction temperature of 420°C, silane flow rate of 1400 sccm, ammonia flow rate of 4000 sccm, reaction time of 600 s, reaction pressure of 1500 mtorr, and reaction power of 5000 W. The reaction conditions for forming the anti-reflection layer 10 are: reaction temperature of 420°C, silane flow rate of 1400 sccm, ammonia flow rate of 6000 sccm, reaction time of 1200 s, reaction pressure of 1500 mtorr, and reaction power of 5000 W.

[0110] S8. Fig. 9 As shown, an opening is etched on the first tunneling oxide layer 3, the first doping layer 7 and the mask layer 9 to form a first opening area. The width of the first opening area W1 is 0.4 mm. The laser used for etching is a green laser with a pulse width of 50 ns.

[0111] S9. Clean and remove the first tunneling oxide layer 3, the first doping layer 7 and the mask layer 9 remaining in the first opening region, and then clean and remove the mask layer 9 outside the first opening region.

[0112] S10. Fig.10 As shown, a third semiconductor layer is deposited on the back of the silicon wafer 1. The third semiconductor layer includes an intrinsic amorphous silicon layer 11 and a third doped layer 12 arranged in sequence. The intrinsic amorphous silicon layer 11 has a thickness of 10 nm, the third doped layer 12 has a thickness of 20 nm, and the boron doping concentration in the third doped layer 12 is 3e20 cm -3 .

[0113] S11. Fig.10 As shown, an opening is etched on the third semiconductor layer to form a second opening area that is alternately arranged with the first opening area and spaced apart. The width of the second opening area W2 is 0.2 mm. The laser used for etching is a green laser with a pulse width of 20 ns.

[0114] S12. Fig.11 As shown, a conductive film layer 13 is formed on the back side of the silicon wafer 1. The thickness of the conductive film layer 13 is 60 nm. The material of the conductive film layer 13 is a tin oxide-doped indium oxide thin film.

[0115] S13. Fig.11 As shown, an isolation groove W3 is opened on the conductive film layer 13, and the width of the isolation groove W3 is 100 μm.

[0116] S14. Fig.12 As shown, a first electrode 14 is formed on a portion of the conductive film layer 13 extending into the first opening region, and a second electrode 15 is formed on a portion of the conductive film layer 13 extending into the second opening region by electroplating.

[0117] Example 2

[0118] The method of Example 1 is referred to, except that the thickness of the first polysilicon layer 4 is adjusted to 100 nm, the surface doping index is adjusted to 3e18, and the thickness of the second polysilicon layer 6 is adjusted to 15 nm, the surface doping index is adjusted to 2.7e18.

[0119] Example 3

[0120] The method of Example 1 is followed, except that the phosphorus doping concentration in the first doping layer 7 is adjusted to 1e20 cm -3 , the surface doping index is 8.3e17, and the phosphorus doping concentration in the second doping layer 8 is 8e18cm -3 , the surface doping index is 4e17.

[0121] Example 4

[0122] The method of Example 1 is followed, except that the conditions for forming the first polysilicon layer 4 and the second polysilicon layer 6 in S4 are adjusted so that the first flow rate into the first gas flow channel 130 is 600 sccm, the second flow rate into the second gas flow channel 140 is 80 sccm, the reaction temperature is 610°C, the pressure is 60 Pa, and the reaction time is 1600 s.

[0123] Example 5

[0124] The method of Example 1 is referred to, except that the annealing conditions in S5 are adjusted so that the annealing temperature is 900° C., the nitrogen flow rate is 3000 sccm, and the annealing time is 30 min.

[0125] Comparative Example 1

[0126] The method of Example 1 is referred to, except that the thickness of the first polysilicon layer 4 is adjusted to 50 nm, the surface doping index is 1e19, and the thickness of the second polysilicon layer 6 is adjusted to 50 nm, the surface doping index is 1e19.

[0127] Comparative Example 2

[0128] The method of Example 1 is followed, except that the phosphorus doping concentration in the first doping layer 7 is adjusted to 6e19cm -3 , the surface doping index is 5e17, and the phosphorus doping concentration in the second doping layer 8 is 1e18cm -3 , the surface doping index is 5e16.

[0129] Comparative Example 3

[0130] The method of Example 1 is followed, except that the conditions for forming the first polysilicon layer 4 and the second polysilicon layer 6 in S4 are adjusted so that the first flow rate into the first gas flow channel 130 is 300 sccm, the second flow rate into the second gas flow channel 140 is 0 sccm, the reaction temperature is 540°C, the pressure is 20 Pa, and the reaction time is 800 s.

[0131] Comparative Example 4

[0132] The method of Example 1 is referred to, except that the annealing conditions in S5 are adjusted so that the annealing temperature is 800° C., the nitrogen flow rate is 500 sccm, and the annealing time is 5 min.

[0133] Test Case

[0134] The back contact cells obtained in the above examples and comparative examples were subjected to performance tests, and the results are shown in the following performance index comparison table.

[0135] Performance index comparison table:

[0136]

[0137] It can be seen from the above performance index comparison table that, relative to the comparative example, the embodiment scheme of the present invention is adopted, by respectively setting the first gas path opening 131 and the second gas path opening 141 on both sides of the limiter 120, so that the first air flow channel 130 is connected with the first cavity 150 located on the back side of the silicon wafer 1 through the first gas path opening 131, and the second air flow channel 140 is connected with the second cavity 160 located on the front side of the silicon wafer 1 through the second gas path opening 141, and the reaction gas can be introduced to the back side and the front side of the silicon wafer 1 through the first air flow channel 130 and the second air flow channel 140 at the same time, so as to realize the simultaneous deposition on the back side and the front side of the silicon wafer 1, improve the deposition efficiency, reduce the equipment cost, shorten the production cycle, and improve the economic benefit, and can independently control the flow rate of the reaction gas in the first air flow channel 130 and the second air flow channel 140, so as to realize the deposition of polysilicon layers of different thicknesses and different doping concentrations on the back side and the front side of the silicon wafer 1, and control the surface doping index of the back side and the front side at the same time, further reduce the equipment cost and improve the economic benefit.

[0138] Furthermore, according to Example 1 and Examples 2-5, it can be seen that the preferred battery structure of the present invention is more conducive to reducing optical absorption while ensuring conductivity, increasing current, and improving battery conversion efficiency.

[0139] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A method for preparing a double-sided deposition battery, characterized in that: The following steps are involved: S1. Provide double-sided polished silicon wafers; S2. depositing a protective layer on the back side of the silicon wafer; S3. By cleaning the velvet surface, a velvet surface is formed on the front side of the silicon wafer, and then the protective layer is removed; S4. Using a quartz boat, a first semiconductor layer and a second semiconductor layer are deposited on the back and front sides of the silicon wafer respectively, wherein the first semiconductor layer includes a first tunneling oxide layer and a first polysilicon layer arranged in sequence, and the second semiconductor layer includes a second tunneling oxide layer and a second polysilicon layer arranged in sequence, wherein the first polysilicon layer and the second polysilicon layer have different thicknesses, and the quartz boat includes a shell and a limiter installed in the shell, a first airflow channel and a second airflow channel, the first airflow channel has a first air path opening on one side of the limiter, and the second airflow channel has a second air path opening on the other side of the limiter, and the The limiting member is used to limit the silicon wafer; a first cavity is formed between two adjacent silicon wafers arranged opposite to each other on the back side, the first cavity is communicated with the first gas path port, and a second cavity is formed between two adjacent silicon wafers arranged opposite to each other on the front side, the second cavity is communicated with the second gas path port; a first flow rate of silane is introduced into the first cavity through the first gas path port, and a second flow rate of silane is introduced into the second cavity through the second gas path port, the first flow rate being greater than the second flow rate, so as to react on the first tunneling oxide layer to form the first polysilicon layer, and react on the second tunneling oxide layer to form the second polysilicon layer; S5. coating a phosphorus source on the first polysilicon layer and the second polysilicon layer respectively, and performing high temperature annealing to form a first doping layer and a second doping layer, wherein the surface doping index of the first doping layer is 6.7e17-4e18, and the surface doping index of the second doping layer is 2.7e17-3.3e18, and the surface doping index is the ratio of the effective doping concentration of the doping layer to the thickness of the doping layer; S6. Cleaning and removing the phosphosilicate glass layer produced by annealing in S5 on the first doped layer and the second doped layer; S7. forming a mask layer on the first doped layer, and then forming an anti-reflection layer on the second doped layer; S8. Etching an opening on the first tunneling oxide layer, the first doping layer and the mask layer to form a first opening region; S9. Cleaning and removing the first tunneling oxide layer, the first doping layer and the mask layer remaining in the first opening region, and then cleaning and removing the mask layer outside the first opening region; S10. Depositing a third semiconductor layer on the back side of the silicon wafer so that a portion of the third semiconductor layer covers the side of the first semiconductor layer away from the silicon wafer, and another portion extends into the first opening area and covers the silicon wafer, wherein the third semiconductor layer includes an intrinsic amorphous silicon layer and a third doping layer arranged in sequence.

2. The method for preparing a double-sided deposited battery according to claim 1, characterized in that: The limiting member is provided with a limiting groove, and the silicon chip is embedded in the limiting groove.

3. The method for preparing a double-sided deposition battery according to claim 1, characterized in that: The first airflow channel and the second airflow channel are relatively arranged at two ends of the limiting component, the first airflow channel is provided with a first external interface, and the second airflow channel is provided with a second external interface.

4. The method for preparing a double-sided deposition battery according to any one of claims 1 to 3, characterized in that: There are multiple limit members, and the multiple limit members are arranged in parallel and spaced apart, and an air intake gap is formed between two adjacent limit members. There are multiple first air path openings and multiple second air path openings, and the multiple first air path openings and the multiple second air path openings are alternately arranged in sequence and are connected to the multiple air intake gaps in a one-to-one correspondence.

5. The method for preparing a double-sided deposition battery according to claim 1, characterized in that: S4 includes: evacuating the shell; introducing oxygen into the first cavity through the first gas port, and introducing oxygen into the second cavity through the second gas port until a preset air pressure is reached in the shell; maintaining the pressure and stuffing oxygen to form the first tunneling oxide layer on the back side of the silicon wafer and the second tunneling oxide layer on the front side of the silicon wafer, wherein the thickness of the first tunneling oxide layer and the second tunneling oxide layer are both 1nm-2nm; the thickness of the first polysilicon layer is 100nm-150nm, and the thickness of the second polysilicon layer is 15nm-30nm.

6. The method for preparing a double-sided deposition battery according to claim 5, characterized in that: In S4, the holding conditions are: the preset air pressure is 10000Pa-30000Pa, the holding time is 900s-1800s, and the holding temperature is 550°C-650°C; And / or, the reaction conditions for forming the first polysilicon layer and the second polysilicon layer are: the first flow rate is 400sccm-600sccm, the second flow rate is 50sccm-80sccm, the reaction temperature is 550℃-650℃, the reaction gas pressure is 30pa-60pa, and the reaction time is 1300s-1600s.

7. The method for preparing a double-sided deposition battery according to claim 1, characterized in that: S5 includes: coating a phosphorus source with a first phosphoric acid concentration on the surface of the first polycrystalline silicon layer by spraying, and coating a phosphorus source with a second phosphoric acid concentration on the surface of the second polycrystalline silicon layer; introducing nitrogen gas for high temperature annealing to convert the first polycrystalline silicon layer into the first doped layer, and converting the second polycrystalline silicon layer into the second doped layer, wherein the phosphorus doping concentration in the first doped layer is 1e20cm -3 -4e20cm -3 The phosphorus doping concentration in the second doping layer is 8e18cm -3 -5e19cm -3 .

8. The method for preparing a double-sided deposition battery according to claim 7, characterized in that: In S5, the coating conditions are: the first phosphoric acid concentration is 10%-15%, and the second phosphoric acid concentration is 3%-5%; And / or, the annealing conditions are: annealing temperature is 850° C.-900° C., nitrogen flow rate is 1000 sccm-3000 sccm, and annealing time is 10 min-30 min.

9. The method for preparing a double-sided deposition battery according to claim 1, characterized in that: In S3, the texturing cleaning conditions are: the texturing time is 8min-40min, the texturing temperature is 65℃-85℃, the texturing liquid is a mixture of potassium hydroxide, texturing additives and water, wherein the mass percentage of potassium hydroxide is 1%-5%, and the mass percentage of the texturing additive is 0.5%-1%.

10. The method for preparing a double-sided deposition battery according to claim 1, characterized in that: After S10, the double-sided deposition battery preparation method further includes: S11. Etching openings on the third semiconductor layer to form second opening regions that are alternately and spaced apart from the first opening regions; S12 forming a conductive film layer on the back side of the silicon wafer; S13. An isolation groove is formed on the conductive film layer so that a portion of the conductive film layer separated from each other extends into the first opening area and covers the third semiconductor layer, and another portion extends into the second opening area and covers the first semiconductor layer; S14. Form a first electrode on the portion of the conductive film layer extending into the first opening region, and form a second electrode on the portion of the conductive film layer extending into the second opening region.

11. A back contact battery, characterized in that: The battery is prepared by the double-sided deposition method as described in any one of claims 1 to 10.

12. A photovoltaic module, characterized in that: Comprising a back contact cell as claimed in claim 11.

Citation Information

Patent Citations

  • Thin-film deposition device and thin-film deposition method

    CN103898476A

  • Preparation method of Al2O3 films with different thicknesses on front surface and back surface of silicon wafer

    CN116682893A

  • Method for simultaneously growing polycrystalline silicon with different thicknesses on front and back surfaces of battery and back contact battery

    CN116936684A

  • Post-texturing manufacturing method of combined passivation back contact battery

    CN118099290A

  • Back contact battery, manufacturing method thereof and photovoltaic module

    CN118281087A