Electrolyte additive, electrolyte and electrochemical device
By using specific electrolyte additives in electrochemical devices to form a stable interface film, the problem of electrolyte decomposition reaction under high pressure is solved, the growth of internal resistance is significantly reduced, and the high-temperature performance of the electrochemical device is improved.
Patent Information
- Application Number
- CN202410910196.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2044-07-09
AI Technical Summary
Traditional electrolyte systems are prone to decomposition reactions under high pressure, causing the internal resistance of the electrochemical device to increase and affecting its high-temperature cycle performance and high-temperature storage performance.
An electrolyte additive is used, including a specific compound combination, to form a stable solid electrolyte interface film (SEI film and CEI film) at the positive and negative electrode interface to reduce side reactions between the electrolyte and the electrode active material, and inhibit the electrolyte Decomposition and gas generation, regulating the mass ratio and content of compounds to optimize interface stability.
Effectively reduce the internal resistance growth rate of electrochemical devices, improve high-temperature cycle performance and high-temperature storage performance, and extend battery life.
Smart Images

Figure CN118486898B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of electrochemical technology, and in particular to an electrolyte additive, an electrolyte and an electrochemical device. Background Art
[0002] Rechargeable electrochemical devices are considered to be one of the most attractive energy storage systems due to their advantages such as high operating voltage, long life, and green environmental protection. Nowadays, electrochemical devices, such as lithium-ion batteries, have been widely used in consumer electronics, power batteries, and energy storage batteries.
[0003] With the rapid development of the electrochemical device industry, the market has put forward higher requirements on the energy density and service life of electrochemical devices. At present, in order to improve the energy density of electrochemical devices, the upper limit voltage of the charge of the electrochemical device can be increased or the content of nickel in the positive electrode material can be increased. However, the traditional electrolyte system is prone to decomposition reaction under high pressure, and the positive electrode material and the electrolyte are prone to side reactions, which affect the structural stability of the positive electrode active material, and also cause excessive consumption of the electrolyte and generate gas, increase the internal resistance of the electrochemical device, and seriously affect the high temperature cycle performance and high temperature storage performance of the electrochemical device. Therefore, how to reduce the internal resistance growth rate of the electrochemical device and improve the high temperature cycle performance and high temperature storage performance of the electrochemical device has become an urgent problem to be solved. Summary of the invention
[0004] The purpose of this application is to provide an electrolyte additive, an electrolyte and an electrochemical device to reduce the internal resistance growth rate of the electrochemical device and improve the high temperature cycle performance and high temperature storage performance of the electrochemical device. The specific technical solution is as follows:
[0005] The first aspect of the present application provides an electrolyte additive, which includes a compound shown in Formula 1 and a compound shown in Formula 2, wherein the compound in Formula 2 is selected from at least one of the compounds shown in Formula 2-A and the compounds shown in Formula 2-B:
[0006] ;
[0007] wherein m and n are each independently selected from integers from 0 to 3, and m and n are not both 0, p is selected from integers from 1 to 5, R0 is selected from a single bond or a methylene group, R1 is selected from hydrogen, halogen, a C1-C5 hydrocarbon group or a C1-C5 halogenated hydrocarbon group, and R2, R3, and R4 are each independently selected from , , , , or R5 and R6 are each independently selected from substituted or unsubstituted phenyl, substituted or unsubstituted imidazolyl, substituted or unsubstituted C1~C5 alkyl, substituted or unsubstituted C2~C5 alkenyl, C1~C5 alkoxy, substituted or unsubstituted C2~C5 alkoxyalkyl, substituted or unsubstituted C1~C5 carbonyl, substituted or unsubstituted C1~C5 cyano, and halogen. When substituted, the substituents are each independently selected from halogen and C1~C5 alkyl. R7 and R9 are each independently selected from halogen, substituted or unsubstituted C1~C5 alkyl, and R8 is selected from substituted or unsubstituted phenylene, substituted or unsubstituted C1~C5 alkylene, C2~C5 alkenylene, C2~C5 alkynylene, and C2~C5 alkyleneoxyalkylene. When substituted, the substituents are each independently selected from halogen, hydroxyl, and phenyl. The compound of Formula 1 of the present application can form an interface film at the interface of the positive and negative electrodes when used as an electrolyte additive. In order to obtain a stable solid electrolyte interface film (SEI film) and a positive electrode electrolyte interface film (CEI film), a large amount of the compound of Formula 1 needs to be added, but the film formation process is difficult to control. Adding too much of the compound of Formula 1 can easily cause a large initial film formation impedance, and as the electrolyte interface film impedance increases during the battery cycle, it causes the internal resistance of the electrochemical device to increase, affecting the cycle life. To address this problem, the present application selects the compound of Formula 1 and the compound of Formula 2 as an electrolyte additive. The compound of Formula 2 takes precedence over the compound of Formula 1 and other components of the electrolyte in the negative electrode. The surface is reduced, and a solid electrolyte interface film (SEI film) rich in alkyl sulfonate is formed on the surface of the negative electrode, thereby improving the stability of the negative electrode interface. In addition, the preferential reduction of the compound of formula 2 is beneficial to inhibiting the further reduction of the compound shown in formula 1 and other components of the electrolyte at the negative electrode, thereby forming a stable solid electrolyte interface film (SEI film) at the negative electrode interface, and at the same time, it is also beneficial to form a stable positive electrode electrolyte interface film (CEI film) at the positive electrode interface, thereby improving the stability of the positive and negative electrode interfaces, reducing the side reactions between the electrolyte and the electrode active materials, effectively inhibiting the further decomposition of the electrolyte, reducing gas production, reducing the internal resistance growth rate of the electrochemical device, and improving the high temperature cycle performance and high temperature storage performance of the electrochemical device.
[0008] In some embodiments of the present application, the mass ratio of the compound of Formula 1 to the compound of Formula 2 is (0.1-16): 1. By regulating the mass ratio of the compound of Formula 1 to the compound of Formula 2 within the scope of the present application, it is beneficial to exert the synergistic effect of the compound of Formula 1 and the compound of Formula 2, further improve the stability of the positive electrode and negative electrode interface, further reduce the side reaction between the electrolyte and the electrode material, reduce gas production, further reduce the internal resistance growth rate of the electrochemical device, and improve the high temperature cycle performance and high temperature storage performance of the electrochemical device.
[0009] In some embodiments of the present application, the compound represented by Formula 1 is selected from at least one of the following compounds:
[0010] , , , , , , , , , .
[0011] The electrolyte additive includes the compound represented by Formula 1 within the above range, which is conducive to forming a stable CEI film at the positive electrode interface, improving the stability of the positive electrode interface, thereby further improving the high-temperature cycle performance and high-temperature storage performance of the electrochemical device and reducing the internal resistance.
[0012] In some embodiments of the present application, the compound represented by Formula 1 is selected from the compound represented by Formula 1-1.
[0013] In some embodiments of the present application, the compound represented by formula 2-A is selected from at least one of the following compounds:
[0014] .
[0015] In some embodiments of the present application, the compound represented by formula 2-B is selected from at least one of the following compounds:
[0016] .
[0017] The electrolyte additive includes at least one of the compounds represented by formula 2-A or the compounds represented by formula 2-B within the above range. During the first charging process of the electrochemical device, it is beneficial for the compound represented by formula 2 to be reduced on the negative electrode surface in priority to the compound represented by formula 1 and other components of the electrolyte, and a solid electrolyte interface film (SEI film) rich in alkyl sulfonates is formed on the negative electrode surface, thereby improving the stability of the negative electrode interface. In addition, the preferential reduction of the compound represented by formula 2 is beneficial to inhibiting the further reduction of the compound represented by formula 1 and other components of the electrolyte at the negative electrode. The compound represented by formula 2 and the compound represented by formula 1 cooperate with each other to form a stable interface protection film at both the positive electrode and the negative electrode, thereby further improving the high-temperature cycle performance and high-temperature storage performance of the electrochemical device, and reducing the internal resistance growth rate of the electrochemical device.
[0018] In some embodiments of the present application, the compound represented by Formula 2 is selected from the compound represented by Formula 2-A10.
[0019] The second aspect of the present application provides an electrolyte, which includes a solvent, an electrolyte and the electrolyte additive provided in the first aspect of the present application.
[0020] In some embodiments of the present application, based on the mass of the electrolyte, the mass percentage of the compound represented by Formula 1 is C1%, 0.05≤C1≤8; and / or, based on the mass of the electrolyte, the mass percentage of the compound represented by Formula 2 is C2%, 0.1≤C2≤5. By regulating the mass percentage of the compound represented by Formula 1 and / or the mass percentage of the compound represented by Formula 2 in the electrolyte within the scope of the present application, it is advantageous for the compound represented by Formula 2 to be reduced on the negative electrode surface in preference to the compound represented by Formula 1 and other components of the electrolyte, forming a solid electrolyte interface film (SEI film) rich in alkyl sulfonates on the negative electrode surface, improving the stability of the negative electrode interface, and inhibiting the compound represented by Formula 1 and other components of the electrolyte from being further reduced at the negative electrode, thereby facilitating the compound represented by Formula 1 to form a stable CEI film at the positive electrode interface, improving the stability of the positive electrode interface, effectively inhibiting further decomposition of the electrolyte, stabilizing the structural stability of the positive electrode material, inhibiting the dissolution of transition metals in the positive electrode material layer, and the compound represented by Formula 2 and the compound represented by Formula 1 cooperate with each other to form a stable interface protection film at both the positive electrode and the negative electrode, further improving the high temperature cycle performance and high temperature storage performance of the electrochemical device, and reducing the internal resistance growth rate of the electrochemical device.
[0021] In some embodiments of the present application, the solvent is selected from at least one of cyclic carbonates, linear carbonates and linear carboxylates; the cyclic carbonate is selected from at least one of ethylene carbonate and propylene carbonate; the linear carbonate is selected from at least one of dimethyl carbonate, diethyl carbonate and ethyl methyl carbonate; the linear carboxylates are selected from at least one of ethyl acetate, ethyl butyrate, ethyl propionate, methyl propionate, propyl propionate and propyl acetate; based on the mass of the electrolyte, the mass percentage of the solvent is C3%, 60≤C3≤89; and / Or, the electrolyte is selected from lithium salt or sodium salt; the lithium salt is selected from at least one of lithium hexafluorophosphate, lithium bisfluorosulfonyl imide and bistrifluoromethanesulfonyl imide; the sodium salt is selected from at least one of sodium hexafluorophosphate, sodium tetrafluoroborate, sodium bisfluorosulfonyl imide, sodium bistrifluoromethanesulfonyl imide, sodium bisoxalate borate, sodium difluorobisoxalate borate, sodium difluorobisoxalate phosphate, sodium tetrafluorooxalate phosphate and sodium 4,5-dicyano-2-trifluoromethyl-imidazole; based on the mass of the electrolyte, the mass percentage of the electrolyte is C4%, 10≤C4≤18. The electrolyte includes a solvent within the above range and the mass percentage of the solvent is regulated within the scope of the present application and / or the electrolyte includes an electrolyte within the above range and the mass percentage of the electrolyte is regulated within the scope of the present application, so that the electrolyte has a suitable viscosity, a high ionic conductivity and good electrochemical stability, and can further improve the high temperature cycle performance and high temperature storage performance of the electrochemical device.
[0022] In some embodiments of the present application, the electrolyte may further include other electrolyte additives, and the other electrolyte additives are selected from at least one of lithium tetrafluoroborate and 1,3-propane sultone; based on the mass of the electrolyte, the mass percentage of the other electrolyte additives is C5%, 0.1≤C5≤20. The electrolyte includes other electrolyte additives within the above range, and the mass percentage of other electrolyte additives is regulated within the scope of the present application, which is conducive to forming a stable interface film at the positive electrode and / or the negative electrode, and further improving the high temperature cycle performance of the electrochemical device.
[0023] The third aspect of the present application provides an electrochemical device, which includes a positive electrode sheet, a negative electrode sheet, a separator and the electrolyte provided by the second aspect of the present application; in some embodiments of the present application, the negative electrode sheet includes a negative electrode current collector and a negative electrode material layer disposed on at least one surface of the negative electrode current collector, the negative electrode material layer includes a negative electrode active material, a negative electrode conductive agent and a negative electrode binder, and the electrochemical device satisfies the relationship I:
[0024] ,
[0025] Among them, D 50 is the particle size corresponding to 50% of the volume accumulation measured from the small particle size in the volume-based particle size distribution of the negative electrode active material particles, in μm; m is the bonding force between the negative electrode material layer and the negative electrode current collector, in N / m; C2% is the mass percentage of the compound shown in Formula 2 based on the mass of the electrolyte. By adjusting the particle size D of the negative electrode active material particles 50 , the bonding force m between the negative electrode material layer and the negative electrode current collector and the mass percentage C2 of the compound shown in Formula 2 satisfy the relationship I, which is beneficial to improving the electronic and ion conductivity of the negative electrode, and is beneficial to the compound of Formula 2 to form a stable SEI film at the negative electrode, thereby improving the stability of the negative electrode interface, thereby further reducing the internal resistance growth rate of the electrochemical device and improving the high temperature cycle performance and high temperature expansion performance of the electrochemical device.
[0026] In some embodiments of the present application, the electrochemical device satisfies at least one of the following conditions: (1) 7 μm ≤ D 50 ≤15μm; (2) 3N / m≤m≤30N / m. When the electrochemical device meets at least one of the above conditions, it is beneficial to further reduce the internal resistance growth rate of the electrochemical device and improve the high temperature cycle performance and high temperature expansion performance of the electrochemical device.
[0027] Beneficial effects of this application:
[0028] The present application provides an electrolyte additive, an electrolyte and an electrochemical device, wherein the electrolyte additive includes a compound shown in Formula 1 and a compound shown in Formula 2, wherein the compound shown in Formula 2 is selected from at least one of the compounds shown in Formula 2-A and the compounds shown in Formula 2-B. Through the above configuration, when the compounds shown in Formula 1 and the compounds shown in Formula 2 of the present application are used as electrolyte additives, it is beneficial to form a stable solid electrolyte interface film (SEI film) at the negative electrode interface, and it is also beneficial to form a stable positive electrode electrolyte interface film (CEI film) at the positive electrode interface, improve the stability of the positive and negative electrode interfaces, reduce the side reactions between the electrolyte and the electrode active material, effectively inhibit the further decomposition of the electrolyte, reduce gas production, reduce the internal resistance growth rate of the electrochemical device, and improve the high temperature cycle performance and high temperature storage performance of the electrochemical device.
[0029] Of course, implementing any product or method of the present application does not necessarily require achieving all of the advantages described above at the same time. DETAILED DESCRIPTION
[0030] The technical solutions in the embodiments of the present application are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all the embodiments. All other embodiments obtained by those skilled in the art based on the present application belong to the scope of protection of the present application.
[0031] It should be noted that in the specific embodiments of the present application, lithium-ion batteries and sodium-ion batteries are used as examples of electrochemical devices to explain the present application, but the electrochemical devices of the present application are not limited to lithium-ion batteries and sodium-ion batteries.
[0032] The first aspect of the present application provides an electrolyte additive, which includes a compound shown in Formula 1 and a compound shown in Formula 2, wherein the compound in Formula 2 is selected from at least one of the compounds shown in Formula 2-A and the compounds shown in Formula 2-B:
[0033] ;
[0034] wherein m and n are each independently selected from integers from 0 to 3, and m and n are not both 0, p is selected from integers from 1 to 5, R0 is selected from a single bond or a methylene group, R1 is selected from hydrogen, halogen, a C1-C5 hydrocarbon group or a C1-C5 halogenated hydrocarbon group, and R2, R3, and R4 are each independently selected from , , , , or R5 and R6 are each independently selected from substituted or unsubstituted phenyl, substituted or unsubstituted imidazolyl, substituted or unsubstituted C1~C5 alkyl, substituted or unsubstituted C2~C5 alkenyl, C1~C5 alkoxy, substituted or unsubstituted C2~C5 alkoxyalkyl, substituted or unsubstituted C1~C5 carbonyl, substituted or unsubstituted C1~C5 cyano, and halogen. When substituted, the substituents are each independently selected from halogen and C1~C5 alkyl. R7 and R9 are each independently selected from halogen, substituted or unsubstituted C1~C5 alkyl, and R8 is selected from substituted or unsubstituted phenylene, substituted or unsubstituted C1~C5 alkylene, C2~C5 alkenylene, C2~C5 alkynylene, and C2~C5 alkyleneoxyalkylene. When substituted, the substituents are each independently selected from halogen, hydroxyl, and phenyl. The halogen is selected from at least one of fluorine, chlorine and bromine, and is preferably fluorine.
[0035] The inventors have found that the electrolyte additive includes the compound shown in Formula 1 and the compound shown in Formula 2 at the same time. During the first charging process of the electrochemical device, the compound shown in Formula 2 is reduced on the negative electrode surface before the compound shown in Formula 1 and other components of the electrolyte, and a solid electrolyte interface film (SEI film) rich in sulfonate is formed on the negative electrode surface, which improves the stability of the negative electrode interface and can effectively inhibit the compound shown in Formula 1 and other components of the electrolyte from being further reduced on the negative electrode surface. During the further charging process of the electrochemical device, the compound shown in Formula 1 can be oxidized on the positive electrode surface, and a stable positive electrode electrolyte interface film (CEI film) is formed on the positive electrode surface, which is conducive to inhibiting the further decomposition of the electrolyte, improving the structural stability of the positive electrode material, and inhibiting the dissolution of transition metals in the positive electrode material layer. Therefore, the synergistic effect of the compound shown in Formula 1 and the compound shown in Formula 2 can significantly improve the high-temperature cycle performance and high-temperature storage performance of the electrochemical device, and reduce the internal resistance growth rate of the electrochemical device.
[0036] In some embodiments of the present application, the mass ratio of the compound of Formula 1 to the compound of Formula 2 is (0.1~16):1. For example, the mass ratio of the compound of Formula 1 to the compound of Formula 2 can be 0.1:1, 0.5:1, 0.8:1, 1:1, 3:1, 5:1, 8:1, 10:1, 12:1, 15:1, 16:1 or a range consisting of any two of these values. By regulating the mass ratio of the compound of Formula 1 to the compound of Formula 2 within the scope of the present application, it is beneficial to exert the synergistic effect of the compound of Formula 1 and the compound of Formula 2, further improve the stability of the positive and negative electrode interfaces, further reduce the side reactions between the electrolyte and the electrode materials, reduce gas production, further reduce the internal resistance growth rate of the electrochemical device, and improve the high temperature cycle performance and high temperature storage performance of the electrochemical device.
[0037] In some embodiments of the present application, the compound represented by Formula 1 is selected from at least one of the following compounds:
[0038] , , , , , , , , , .
[0039] The electrolyte additive includes the compound represented by formula 1 within the above range, which is conducive to forming a stable CEI film at the positive electrode interface, improving the stability of the positive electrode interface, effectively inhibiting the further decomposition of the electrolyte, stabilizing the structural stability of the positive electrode material, and inhibiting the dissolution of transition metals in the positive electrode material layer, thereby further improving the high-temperature cycle performance and high-temperature storage performance of the electrochemical device, and reducing the internal resistance growth rate of the electrochemical device.
[0040] In some embodiments of the present application, the compound shown in Formula 1 is selected from the compound shown in Formula 1-1. The electrolyte additive includes the compound shown in Formula 1-1, which is more conducive to forming a stable CEI film at the positive electrode interface, improving the stability of the positive electrode interface, effectively inhibiting further decomposition of the electrolyte, stabilizing the structural stability of the positive electrode material, and inhibiting the dissolution of transition metals in the positive electrode material layer, thereby further improving the high temperature cycle performance and high temperature storage performance of the electrochemical device, and reducing the internal resistance growth rate of the electrochemical device.
[0041] In some embodiments of the present application, the compound represented by formula 2-A is selected from at least one of the following compounds:
[0042] .
[0043] In some embodiments of the present application, the compound represented by formula 2-B is selected from at least one of the following compounds:
[0044] .
[0045] The electrolyte additive includes at least one of the compounds shown in Formula 2-A or the compounds shown in Formula 2-B within the above range. During the first charging process of the electrochemical device, since the compound shown in Formula 2 has smaller steric hindrance and some electron-withdrawing groups, it is beneficial for the compound shown in Formula 2 to be reduced on the negative electrode surface in priority to the compound shown in Formula 1 and other components of the electrolyte, and a solid electrolyte interface film (SEI film) rich in alkyl sulfonates is formed on the negative electrode surface. Compared with the ring structure, the compound shown in Formula 2 has a chain structure, which can avoid the formation of sulfonates containing unsaturated bonds (C=C and C≡C) and low stability SEI film during reduction, and the alkyl sulfonate lithium component is beneficial to improving the stability of the negative electrode interface, improving high-temperature cycle performance and high-temperature storage performance; in addition, the preferential reduction of the compound shown in Formula 2 is beneficial to inhibiting the compound shown in Formula 1 and other components of the electrolyte from being further reduced at the negative electrode, and the compound shown in Formula 2 and the compound shown in Formula 1 cooperate with each other to form a stable interface protection film at both the positive and negative electrodes, further improving the high-temperature cycle performance and high-temperature storage performance of the electrochemical device, and reducing the internal resistance growth rate of the electrochemical device.
[0046] In some embodiments of the present application, the compound shown in Formula 2 is selected from the compound shown in Formula 2-A10. The electrolyte additive includes the compound shown in Formula 2-A10, which is more conducive to the formation of a solid electrolyte interface film (SEI film) rich in alkyl sulfonates on the surface of the negative electrode, improves the stability of the negative electrode interface, and inhibits the compound shown in Formula 1 and other components of the electrolyte from being further reduced at the negative electrode. The compound shown in Formula 2 and the compound shown in Formula 1 cooperate with each other to form a stable interface protection film at both the positive and negative electrodes, further improving the high-temperature cycle performance and high-temperature storage performance of the electrochemical device, and reducing the internal resistance growth rate of the electrochemical device. At the same time, the imidazole group of the compound of Formula 2-A10 contains a nitrogen atom with a lone electron pair, which makes the compound exhibit weak Lewis basicity in the electrolyte, which can effectively inhibit the increase in electrolyte acidity and water content.
[0047] The second aspect of the present application provides an electrolyte, which includes a solvent, an electrolyte and the electrolyte additive provided in the first aspect of the present application. The electrolyte includes the electrolyte additive within the scope of the present application and is applied to an electrochemical device, which is beneficial to improving the stability of the positive electrode and negative electrode interface, reducing the side reactions between the electrolyte and the electrode active material, effectively inhibiting the excessive consumption of the electrolyte, reducing gas production, reducing the internal resistance growth rate of the electrochemical device, and improving the high temperature cycle performance and high temperature storage performance of the electrochemical device.
[0048] In some embodiments of the present application, based on the mass of the electrolyte, the mass percentage of the compound shown in Formula 1 is C1%, 0.05≤C1≤8. For example, the mass percentage C1% of the compound shown in Formula 1 can be 0.05%, 0.1%, 0.5%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8% or a range consisting of any two of the values. By regulating the mass percentage of the compound shown in Formula 1 in the electrolyte within the scope of the present application, it is beneficial to form a stable CEI film at the positive electrode interface, improve the stability of the positive electrode interface, effectively inhibit further decomposition of the electrolyte, stabilize the structural stability of the positive electrode material, inhibit the dissolution of transition metals in the positive electrode material layer, further improve the high temperature cycle performance and high temperature storage performance of the electrochemical device, and reduce the internal resistance growth rate of the electrochemical device.
[0049] In some embodiments of the present application, based on the mass of the electrolyte, the mass percentage of the compound shown in Formula 2 is C2%, 0.1≤C2≤5. For example, the mass percentage of the compound shown in Formula 2 C2% can be 0.1%, 0.5%, 1%, 2%, 3%, 4%, 5% or a range consisting of any two of these values. By regulating the mass percentage of the compound shown in Formula 2 in the electrolyte within the scope of the present application, it is beneficial for the compound shown in Formula 2 to be reduced on the surface of the negative electrode in preference to the compound shown in Formula 1 and other components of the electrolyte, forming a solid electrolyte interface film (SEI film) rich in alkyl sulfonates on the surface of the negative electrode, improving the stability of the negative electrode interface, and having a small impedance, and can also effectively inhibit the compound shown in Formula 1 and other components of the electrolyte from being further reduced at the negative electrode, and the compound shown in Formula 2 and the compound shown in Formula 1 cooperate with each other to form a stable interface protection film at both the positive and negative electrodes, further improving the high temperature cycle performance and high temperature storage performance of the electrochemical device, and reducing the internal resistance growth rate of the electrochemical device.
[0050] In some embodiments of the present application, based on the mass of the electrolyte, the mass percentage of the compound represented by Formula 1 is C1%, 0.05≤C1≤8; based on the mass of the electrolyte, the mass percentage of the compound represented by Formula 2 is C2%, 0.1≤C2≤5. By regulating the mass percentage of the compound represented by Formula 1 and the mass percentage of the compound represented by Formula 2 in the electrolyte within the scope of the present application, it is advantageous for the compound represented by Formula 2 to be reduced on the negative electrode surface in preference to the compound represented by Formula 1 and other components of the electrolyte, forming a solid electrolyte interface film (SEI film) rich in alkyl sulfonates on the negative electrode surface, improving the stability of the negative electrode interface, and inhibiting the compound represented by Formula 1 and other components of the electrolyte from being further reduced at the negative electrode, thereby facilitating the compound represented by Formula 1 to form a stable CEI film at the positive electrode interface, improving the stability of the positive electrode interface, effectively inhibiting further decomposition of the electrolyte, stabilizing the structural stability of the positive electrode material, inhibiting the dissolution of transition metals in the positive electrode material layer, and the compound represented by Formula 2 and the compound represented by Formula 1 cooperate with each other to form a stable interface protection film at both the positive electrode and the negative electrode, further improving the high-temperature cycle performance and high-temperature storage performance of the electrochemical device, and reducing the internal resistance growth rate of the electrochemical device.
[0051] In some embodiments of the present application, the solvent is selected from at least one of cyclic carbonates, linear carbonates and linear carboxylates; cyclic carbonates are selected from at least one of ethylene carbonate and propylene carbonate; linear carbonates are selected from at least one of dimethyl carbonate, diethyl carbonate and ethyl methyl carbonate; linear carboxylates are selected from at least one of ethyl acetate, ethyl butyrate, ethyl propionate, methyl propionate, propyl propionate and propyl acetate; based on the mass of the electrolyte, the mass percentage of the solvent is C3%, 60≤C3≤89. For example, the mass percentage of the solvent C3% can be 60%, 65%, 70%, 75%, 80%, 85%, 89% or a range consisting of any two of the values. The electrolyte includes a solvent within the above range, and the mass percentage of the solvent is regulated within the scope of the present application, so that the electrolyte has a suitable viscosity, a high ionic conductivity and good electrochemical stability, and can further improve the high temperature cycle performance and high temperature storage performance of the electrochemical device.
[0052] In some embodiments of the present application, the electrolyte is selected from lithium salt or sodium salt; the lithium salt is selected from at least one of lithium hexafluorophosphate, lithium bisfluorosulfonyl imide and bistrifluoromethanesulfonyl imide; the sodium salt is selected from at least one of sodium hexafluorophosphate, sodium tetrafluoroborate, sodium bisfluorosulfonyl imide, sodium bistrifluoromethanesulfonyl imide, sodium bisoxalate borate, sodium difluorobisoxalate borate, sodium difluorobisoxalate phosphate, sodium tetrafluorooxalate phosphate and sodium 4,5-dicyano-2-trifluoromethyl-imidazole; based on the mass of the electrolyte, the mass percentage of the electrolyte is C4%, 10≤C4≤18. For example, the mass percentage of the electrolyte C4% can be 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18% or a range consisting of any two of the values. The electrolyte includes an electrolyte within the above range, and the mass percentage of the electrolyte is regulated within the scope of the present application, so that the electrolyte has higher ionic conductivity and good electrochemical stability, which can further improve the high-temperature cycle performance and high-temperature storage performance of the electrochemical device.
[0053] In some embodiments of the present application, the solvent is selected from at least one of cyclic carbonates, linear carbonates and linear carboxylates; the cyclic carbonate is selected from at least one of ethylene carbonate and propylene carbonate; the linear carbonate is selected from at least one of dimethyl carbonate, diethyl carbonate and ethyl methyl carbonate; the linear carboxylates are selected from at least one of ethyl acetate, ethyl butyrate, ethyl propionate, methyl propionate, propyl propionate and propyl acetate; based on the mass of the electrolyte, the mass percentage of the solvent is C3%, 60≤C3≤89; The electrolyte is selected from lithium salt or sodium salt; the lithium salt is selected from at least one of lithium hexafluorophosphate, lithium bisfluorosulfonyl imide and bistrifluoromethanesulfonyl imide; the sodium salt is selected from at least one of sodium hexafluorophosphate, sodium tetrafluoroborate, sodium bisfluorosulfonyl imide, sodium bistrifluoromethanesulfonyl imide, sodium bisoxalate borate, sodium difluorobisoxalate borate, sodium difluorobisoxalate phosphate, sodium tetrafluorooxalate phosphate and sodium 4,5-dicyano-2-trifluoromethyl-imidazole; based on the mass of the electrolyte, the mass percentage of the electrolyte is C4%, 10≤C4≤18. The electrolyte includes the solvent within the above range and the mass percentage of the solvent is regulated within the scope of the present application, and the electrolyte includes the electrolyte within the above range and the mass percentage of the electrolyte is regulated within the scope of the present application, so that the electrolyte has a suitable viscosity, a high ionic conductivity and good electrochemical stability, and can further improve the high temperature cycle performance and high temperature storage performance of the electrochemical device.
[0054] In some embodiments of the present application, the electrolyte may further include other electrolyte additives, and the other electrolyte additives are selected from at least one of lithium tetrafluoroborate and 1,3-propane sultone; based on the mass of the electrolyte, the mass percentage of the other electrolyte additives is C5%, 0.1≤C5≤20. For example, the mass percentage C5% of other additives can be 0.1%, 1%, 2%, 3%, 5%, 8%, 10%, 13%, 15%, 18%, 20% or a range consisting of any two of the values. The electrolyte includes other electrolyte additives within the above range, and regulating the mass percentage of other electrolyte additives within the scope of the present application is conducive to forming a stable interface film at the positive and negative electrodes, and further improving the high temperature cycle performance of the electrochemical device.
[0055] The third aspect of the present application provides an electrochemical device, which includes a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte provided in the second aspect of the present application. The electrochemical device includes an electrolyte within the scope of the present application, which is conducive to improving the stability of the positive and negative electrode interfaces, reducing the side reactions between the electrolyte and the electrode active materials, effectively inhibiting the excessive consumption of the electrolyte, reducing gas production, reducing the internal resistance growth rate of the electrochemical device, and improving the high temperature cycle performance and high temperature storage performance of the electrochemical device.
[0056] In some embodiments of the present application, the negative electrode sheet includes a negative electrode current collector and a negative electrode material layer disposed on at least one surface of the negative electrode current collector, the negative electrode material layer includes a negative electrode active material, a negative electrode conductive agent and a negative electrode binder, and the electrochemical device satisfies the relationship I:
[0057] ,
[0058] Among them, D 50 is the particle size corresponding to 50% of the volume accumulation measured from the small particle size in the volume-based particle size distribution of the negative electrode active material particles, in μm; m is the bonding force between the negative electrode material layer and the negative electrode current collector, in N / m; C2% is the mass percentage of the compound shown in Formula 2 based on the mass of the electrolyte. The value of relational formula I can be 0.02, 0.05, 0.1, 0.3, 0.5, 0.8, 1, 1.2, 1.3, 1.5 or a range consisting of any two of these values. By adjusting D 50 , m and C2 satisfy the relationship I, which is beneficial to improving the electronic and ion conductivity of the negative electrode plate, and is beneficial to the compound of formula 2 to form a stable SEI film at the negative electrode, thereby improving the stability of the negative electrode interface, thereby further reducing the internal resistance growth rate of the electrochemical device and improving the high-temperature cycle performance and high-temperature expansion performance of the electrochemical device.
[0059] In some embodiments of the present application, 7 μm ≤ D 50≤15μm. For example, D 50 The value of can be 7 μm, 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm, 14 μm, 15 μm or a range consisting of any two of these values. By adjusting the particle size D of the negative electrode active material 50 Within the scope of the present application and satisfying Relationship I, the negative electrode active material has suitable active sites, active metal ions (such as Li + 、Na + ) The transmission path inside the negative electrode active material particles is shorter, and there are fewer side reactions between the negative electrode active material and the electrolyte, which is beneficial to reducing the internal resistance growth rate of the electrochemical device and improving the high-temperature cycle performance and high-temperature storage performance of the electrochemical device.
[0060] In some embodiments of the present application, 3N / m≤m≤30N / m. For example, the value of m can be 3N / m, 5N / m, 10N / m, 13N / m, 15N / m, 18N / m, 20N / m, 23N / m, 25N / m, 28N / m, 30N / m, or a range consisting of any two of these values. The value of the bonding force m between the negative electrode material layer and the negative electrode current collector is within the range of the present application and satisfies the relationship I, the active metal ion (e.g., Li + 、Na + ) has a shorter transmission path and the negative electrode has good electron and ion conductivity, which improves the kinetic and cycle performance of the electrochemical device.
[0061] In some embodiments of the present application, 7 μm ≤ D 50 ≤15μm, 3N / m≤m≤30N / m. By adjusting D 50 The values of m and m are within the scope of the present application and satisfy the relationship I, which can further improve the electronic and ion conductivity of the negative electrode plate, and is conducive to the formation of a stable SEI film at the negative electrode by the compound of formula 2, thereby improving the stability of the negative electrode interface, thereby further reducing the internal resistance growth rate of the electrochemical device and improving the high temperature cycle performance and high temperature expansion performance of the electrochemical device.
[0062] In some embodiments of the present application, based on the mass of the negative electrode material layer, the mass percentage X% of the negative electrode binder is 1% to 4%.
[0063] Generally, the magnitude of the bonding force m between the negative electrode material layer and the negative electrode current collector can be adjusted by changing the mass percentage of the negative electrode binder in the negative electrode material layer. When other conditions remain unchanged, increasing the mass percentage of the negative electrode binder increases the bonding force m between the negative electrode material layer and the negative electrode current collector; decreasing the mass percentage of the negative electrode binder decreases the bonding force m between the negative electrode material layer and the negative electrode current collector.
[0064] The present application has no particular restrictions on the type of negative electrode active material, as long as the purpose of the present application can be achieved. For example, the negative electrode active material may include but is not limited to graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, lithium titanate, etc. Graphite may include but is not limited to at least one of natural graphite or artificial graphite; the above silicon-based material may include but is not limited to at least one of elemental silicon, silicon oxide compounds, silicon-carbon composites, silicon-nitrogen composites, or silicon alloys; the above tin-based material may include at least one of elemental tin, tin oxide compounds, or tin alloys.
[0065] In the present application, the negative electrode active material can be purchased, and in combination with the "test of particle size D50 of negative electrode active material" provided in the present application, the negative electrode active material with the required D50 is selected.
[0066] In the present application, the negative electrode plate includes a negative electrode current collector and a negative electrode material layer disposed on at least one surface of the negative electrode current collector. The above-mentioned "negative electrode material layer is disposed on at least one surface of the negative electrode current collector" means that the negative electrode material layer can be disposed on one surface of the negative electrode current collector along its own thickness direction, or it can be disposed on two surfaces of the negative electrode current collector along its own thickness direction. It should be noted that the "surface" here can be the entire area of the surface of the negative electrode current collector, or it can be a partial area of the surface of the negative electrode current collector. This application has no special restrictions, as long as the purpose of this application can be achieved. This application has no special restrictions on the negative electrode current collector, as long as the purpose of this application can be achieved. For example, the negative electrode current collector can be copper foil, copper alloy foil, nickel foil, stainless steel foil, titanium foil, foam nickel or foam copper, aluminum foil or a composite negative electrode current collector. The composite negative electrode current collector may be a polymer material base layer and a metal layer formed on at least one surface of the polymer material substrate. The material of the polymer material base layer may include but is not limited to at least one of polypropylene (PP), polyethylene terephthalate (PET) or polybutylene terephthalate (PBT), and the material of the metal layer may include but is not limited to at least one of copper, copper alloy, nickel or nickel alloy. The present application has no particular restrictions on the thickness of the negative electrode material layer and the negative electrode current collector, as long as the purpose of the present application can be achieved. For example, the thickness of the single-sided negative electrode material layer is 50μm to 180μm, and the thickness of the negative electrode current collector is 3μm to 10μm.
[0067] The present application does not particularly limit the types of negative electrode conductors and negative electrode binders, as long as the purpose of the present application can be achieved. For example, the negative electrode conductor may include but is not limited to at least one of superconducting carbon black (Super P), acetylene black, Ketjen black, carbon nanotubes, graphene or carbon fibers. The above-mentioned carbon nanotubes may include but are not limited to single-walled carbon nanotubes and / or multi-walled carbon nanotubes. The above-mentioned carbon fibers may include but are not limited to vapor-grown carbon fibers (VGCF) and / or nano-carbon fibers. For example, the negative electrode binder may include but is not limited to at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), sodium carboxymethyl cellulose (CMC), polymethacrylic acid (PMAA) or carboxymethyl chitosan (CMCS).
[0068] In the present application, the electrochemical device includes a positive electrode plate, and the positive electrode plate includes a positive electrode collector and a positive electrode material layer disposed on at least one surface of the positive electrode collector. The above-mentioned "positive electrode material layer disposed on at least one surface of the positive electrode collector" means that the positive electrode material layer can be disposed on one surface of the positive electrode collector along the thickness direction of itself, or on two surfaces of the positive electrode collector along the thickness direction of itself. It should be noted that the "surface" here can be the entire area of the surface of the positive electrode collector, or it can be a partial area of the surface of the positive electrode collector. This application has no special restrictions, as long as the purpose of this application can be achieved. This application has no special restrictions on the positive electrode collector, as long as the purpose of this application can be achieved. For example, the positive electrode collector can be aluminum foil, aluminum alloy foil or a composite positive electrode collector. The composite positive electrode current collector may be a polymer material base layer and a metal layer formed on at least one surface of the polymer material substrate. The material of the polymer material base layer may include but is not limited to at least one of polypropylene (PP), polyethylene terephthalate (PET) or polybutylene terephthalate (PBT), and the material of the metal layer may include but is not limited to at least one of aluminum, aluminum alloy, nickel or nickel alloy. The present application has no particular restrictions on the thickness of the positive electrode material layer and the positive electrode current collector, as long as the purpose of the present application can be achieved. For example, the thickness of the single-sided positive electrode material layer is 50μm to 250μm, and the thickness of the positive electrode current collector is 7μm to 15μm.
[0069] The positive electrode material layer includes a positive electrode active material. The present application has no particular limitation on the positive electrode active material as long as the purpose of the present application can be achieved. For example, the positive electrode active material may include but is not limited to lithium iron phosphate, lithium iron manganese phosphate, LiCoO2, LiNi x Co y Mn zO2 (0≤x,y,z≤1,x+y+z=1), lithium-rich manganese-based materials (xLi2MnO3•(1-x)LiAO2, A can be Ni, Co, Mn), lithium nickel manganese oxide (LiNi 0.5 Mn 1.5 O4)、Na 0.44 At least one of MnO2, P2 layered NaMO2 (M is one, two or three of Ni, Mn, Fe), NaFePO4, Na4Fe3(PO4)2P2O7, Na3V2(PO4)3, Na3V2(PO4)2F3, Na2Fe(CN)6 or Na2MnFe(CN)6.
[0070] The positive electrode material layer may also include a positive electrode conductor and a positive electrode binder. The present application does not particularly limit the types of the positive electrode conductor and the positive electrode binder, as long as the purpose of the present application can be achieved. For example, the positive electrode conductor may include but is not limited to at least one of superconducting carbon black (Super P), acetylene black, Ketjen black, carbon nanotubes, graphene or carbon fiber. For example, the positive electrode binder may include but is not limited to polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer or fluorine-containing acrylate resin. The present application does not particularly limit the mass ratio of the positive active material, the conductive agent, and the binder in the positive electrode material layer. Those skilled in the art can choose according to actual needs, as long as the purpose of the present application can be achieved.
[0071] In the present application, the electrochemical device also includes a diaphragm. The present application has no particular restrictions on the diaphragm, as long as the purpose of the present application can be achieved. For example, the material of the diaphragm may include, but is not limited to, at least one of polyethylene (PE), polypropylene (PP), glass fiber, polyester (e.g., polyethylene terephthalate (PET) film), cellulose, polyimide (PI), and polyamide (PA). The type of diaphragm may include at least one of a woven membrane, a non-woven fabric, a microporous membrane, a composite membrane, a rolled membrane, or a spun membrane. In the present application, the thickness of the diaphragm is not particularly limited, as long as the purpose of the present application can be achieved. For example, the thickness of the diaphragm may be 4 μm to 20 μm.
[0072] In the present application, the electrochemical device also includes a housing for accommodating a positive electrode plate, a separator, a negative electrode plate and an electrolyte, as well as other components known in the field of secondary batteries, and the present application does not limit the above-mentioned other components. The present application has no particular restrictions on the housing, and it can be a housing known in the art, as long as the purpose of the present application can be achieved. For example, the housing can be a hard shell housing or a flexible housing. The material of the hard shell housing can be metal, and the present application does not limit the type of metal, and a metal hard shell housing known in the art can be used, as long as the purpose of the present application can be achieved. The flexible housing can be a metal plastic film, such as an aluminum plastic film, a steel plastic film, etc.
[0073] The electrochemical device of the present application is not particularly limited, and may include any device that generates an electrochemical reaction. In one embodiment of the present application, the electrochemical device may include, but is not limited to, a lithium ion secondary battery (lithium ion battery), a sodium ion secondary battery (sodium ion battery), and the like.
[0074] The preparation process of the electrochemical device of the present application is well known to those skilled in the art, and there is no particular limitation in the present application. For example, the preparation process of the electrochemical device may include but is not limited to the following steps: stacking the positive electrode sheet, the separator and the negative electrode sheet in order, and winding, folding and other operations as needed to obtain an electrode assembly of a winding structure, placing the electrode assembly in a shell, injecting the electrolyte into the shell and sealing it to obtain a secondary battery. Alternatively, stacking the positive electrode sheet, the separator and the negative electrode sheet in order, and then fixing the four corners of the entire laminated structure with tape to obtain an electrode assembly of a laminated structure, placing the electrode assembly in a shell, injecting the electrolyte into the shell and sealing it to obtain an electrochemical device. In addition, overcurrent protection elements, guide plates, etc. may also be placed in the shell as needed to prevent the pressure inside the secondary battery from rising and overcharging and discharging.
[0075] Example
[0076] Hereinafter, the embodiments of the present application will be described in more detail with reference to Examples and Comparative Examples. Various tests and evaluations were performed according to the following methods. In addition, unless otherwise specified, "parts" and "%" are by mass.
[0077] Test methods and equipment:
[0078] Negative electrode active material particle size D 50 Test
[0079] 1% ethylphenyl polyethylene glycol (Nonidet p40) dispersant and the negative electrode active material to be tested were ultrasonicated for 1 minute, and then the particle size distribution was tested using a laser particle size tester (instrument model: Malvern MS300). In the volume-based particle size distribution of the negative electrode active material, the particle size that reaches 50% of the volume accumulation starting from the small particle size is D50.
[0080] Test of the bonding force m between the negative electrode material layer and the negative electrode current collector
[0081] After formation, shaping and capacity division, the lithium-ion battery was completely discharged to 2V at a constant current of 0.5C and then disassembled to obtain the negative electrode sheet. After washing with dimethyl carbonate (DMC) three times, the negative electrode sheet was placed in an oven at 80°C for 24 hours, and then a 180° peel test was performed using a tensile machine to measure the bonding force between the negative electrode material layer and the negative electrode current collector. The specific test was carried out according to the national standard GB / T2790-1995 Adhesive 180° Peel Strength Test Method.
[0082] High temperature cycle performance test and internal resistance growth rate test
[0083] Place the lithium-ion battery in a 45°C constant temperature box and let it stand for 30 minutes. Then charge the lithium-ion battery at a constant current of 1C to a voltage of 3.6V, then charge it at a constant voltage of 3.6V to a current of 0.05C, and then discharge it at a constant current of 1C to a voltage of 2V. This is a charge and discharge cycle, and repeat the above charge and discharge cycles to 2000 times. Record the maximum discharge capacity of the first three charge and discharge cycles as Q1 and the AC internal resistance ACR1 of the lithium-ion battery after the third cycle discharge, and then record the discharge capacity of the lithium-ion battery after 2000 cycles as Q2 and the AC internal resistance ACR2. The charge and discharge cycle test instrument is the Xinwei BTS, and the AC internal resistance test instrument is the battery internal resistance tester.
[0084] Capacity retention rate (%) = Q2 / Q1×100%; The capacity retention rate is used to evaluate the high temperature cycle performance of lithium-ion batteries. The greater the capacity retention rate, the better the high temperature cycle performance of lithium-ion batteries.
[0085] Internal resistance growth rate (%) = [(ACR2 / ACR1)-1] × 100%.
[0086] High temperature storage performance test
[0087] The lithium-ion battery was placed in a 25°C environment, charged at a constant current of 1C to 3.6V, and then charged at a constant voltage of 3.6V to a current of 0.05C. The thickness of the lithium-ion battery was tested and recorded as d0. The lithium-ion battery was then placed in a 70°C constant temperature box and left to stand for 15 days to observe the surface state of the lithium-ion battery.
[0088] Judgment standard: When the lithium-ion battery cell is separated from the aluminum-plastic film packaging bag, that is, it is not in a vacuum state, it is determined that the lithium-ion battery produces gas.
[0089] The test methods for high temperature cycle performance, internal resistance growth rate and high temperature storage performance of sodium ion batteries in Examples 1-26 are the same as the above-mentioned lithium ion battery test methods.
[0090] Example 1-1
[0091] <Preparation of Electrolyte>
[0092] In an inert atmosphere with a water content of less than 0.1 ppm and an oxygen content of less than 1 ppm, ethylene carbonate (EC), ethyl methyl carbonate (EMC), and ethyl acetate (EA) are mixed in a mass ratio of 3:6:1 to obtain a basic solvent, and then lithium hexafluorophosphate (LiPF6), lithium bis(fluorosulfonyl)imide salt (LiFSI), the compound shown in Formula 1-1, and the compound shown in Formula 2-A10 are added to the basic solvent and mixed evenly to obtain an electrolyte. Based on the mass of the electrolyte, the mass percentage of LiPF6 is 9%, the mass percentage of LiFSI is 5%, the mass percentage of the compound shown in Formula 1-1 is 1%, the mass percentage of the compound shown in Formula 2-A10 is 0.5%, and the remaining base solvent is 84.5%.
[0093] <Preparation of negative electrode sheet>
[0094] The negative electrode active material graphite, the conductive agent acetylene black, the binder sodium carboxymethyl cellulose (CMC) and styrene butadiene rubber (SBR) were mixed in a mass ratio of 95:2:2:1 (based on the mass of the negative electrode material layer, the mass percentage X of the negative electrode binder sodium carboxymethyl cellulose (CMC) was 2%), and deionized water was added as a solvent to prepare a slurry with a solid content of 49wt%, and the negative electrode slurry was obtained after stirring evenly with a vacuum mixer. The negative electrode slurry was evenly coated on one surface of a negative electrode current collector copper foil with a thickness of 9μm, and dried at 90°C to obtain a negative electrode sheet with a single-sided coating of a negative electrode material layer, and the coating weight of the negative electrode material layer was 8mg / mm 2 Then repeat the above steps on the other surface of the copper foil to obtain a negative electrode sheet with a negative electrode material layer coated on both sides. After drying at 85°C, roll pressing, slitting and welding the tabs, a negative electrode sheet with a specification of 74mm×59mm is obtained for standby use. The thickness of the single-sided negative electrode material layer is 111μm.
[0095] <Preparation of positive electrode sheet>
[0096] The positive electrode active material lithium iron phosphate (LiFePO4), the positive electrode conductive agent acetylene black and the positive electrode binder polyvinylidene fluoride (PVDF) were mixed in a mass ratio of 96:2:2, and N-methylpyrrolidone (NMP) was added as a solvent to prepare a slurry with a solid content of .55wt%, and the positive electrode slurry was obtained after vacuum stirring. The positive electrode slurry was evenly coated on one surface of a positive electrode current collector aluminum foil with a thickness of 12μm, and dried at 90°C to obtain a positive electrode sheet with a single-sided coating of a positive electrode material layer. The coating weight of the positive electrode material layer was 17mg / mm 2Then repeat the above steps on the other surface of the aluminum foil to obtain a positive electrode sheet coated with a positive electrode material layer on both sides. After drying at 85°C, roll pressing, slitting and welding the tabs, a positive electrode sheet with a specification of 70mm×55mm is obtained for standby use. The thickness of the single-sided positive electrode material layer is 158μm.
[0097] <Preparation of Separator>
[0098] A polyethylene (PE) porous membrane with a thickness of 10 µm (provided by Shenzhen Xingyuan Material Technology Co., Ltd.) was used as the separator.
[0099] <Preparation of lithium-ion batteries>
[0100] The positive electrode sheet, separator and negative electrode sheet prepared above are stacked in order, so that the separator is placed between the positive electrode sheet and the negative electrode sheet to play an isolating role, and the electrode assembly is wound. The electrode assembly is placed in an aluminum-plastic film packaging bag, and the water is removed at 85°C, and the prepared electrolyte is injected. After vacuum packaging, standing, forming, shaping and other processes, a lithium-ion battery with a rated capacity of 2Ah is obtained. Among them, the upper limit voltage of the formation is 3.6V, the formation temperature is 45°C, and the formation pressure is 300kgf after standing for 48 hours.
[0101] Example 1-2 to Example 1-25
[0102] Except that the type of the compound represented by Formula 1 or the compound represented by Formula 2 is adjusted according to Table 1 in <Preparation of Electrolyte>, the rest is the same as Example 1-1.
[0103] Examples 1-26
[0104] In addition to replacing electrolyte lithium hexafluorophosphate (LiPF6) and lithium bis(fluorosulfonyl)imide (LiFSI) with sodium hexafluorophosphate (NaPF6) in <Preparation of electrolyte>, the mass percentage of electrolyte NaPF6 is 14% based on the mass of electrolyte, and in <Preparation of negative electrode sheet>, the negative electrode active material graphite is replaced with hard carbon, and in <Preparation of positive electrode sheet>, the positive electrode active material is replaced with NaFePO4 to prepare a sodium ion battery, and the rest is the same as Example 1-1.
[0105] Example 2-1 to Example 2-11
[0106] Except that the mass percentage of the compound represented by Formula 1 or the compound represented by Formula 2 in <Preparation of Electrolyte> is adjusted according to Table 2, the rest is the same as Example 1-1. When the content of the compound represented by Formula 1 or the compound represented by Formula 2 changes, the mass percentage of the base solvent changes accordingly, and the mass percentage of the electrolyte remains unchanged.
[0107] Example 2-12 to Example 2-15
[0108] Except that in <Preparation of Negative Electrode Sheet>, the negative electrode active material with the corresponding particle size D50 is selected according to Table 2, the rest is the same as Example 1-1.
[0109] Example 2-16 to Example 2-19
[0110] Except that the mass percentage of the negative electrode binder is adjusted in <Preparation of Negative Electrode Sheet>, the mass percentage of the negative electrode active material is changed accordingly, the rest is the same as Example 1-1.
[0111] Example 2-20 to Example 2-24
[0112] Except for adjusting the relevant parameters according to Table 2, the rest is the same as Example 1-1. In the <Preparation of Negative Electrode Sheet>, when the mass percentage of the negative electrode binder changes, the mass percentage of the negative electrode active material changes accordingly; when the content of the compound represented by Formula 1 or the compound represented by Formula 2 changes, the mass percentage of the base solvent changes accordingly, and the mass percentage of the electrolyte remains unchanged.
[0113] Example 2-25 to Example 2-28
[0114] Except for adjusting the mass percentage C5% and type of other electrolyte additives in <Preparation of Electrolyte> according to Table 2, the rest is the same as Example 1-1. Among them, when the content of other electrolyte additives C5% changes, the mass percentage of the base solvent changes accordingly, and the mass percentage of the electrolyte remains unchanged. In Table 2, LiBF4 is lithium tetrafluoroborate, and PS is 1,3-propane sultone.
[0115] Example 2-29
[0116] Except for the fact that in <Preparation of Electrolyte>, lithium bis(fluorosulfonyl)imide (LiFSI) is replaced by lithium hexafluorophosphate (LiPF6), and the total mass percentage of lithium hexafluorophosphate (LiPF6) is 14% based on the mass of the electrolyte, the rest is the same as Example 1-1.
[0117] Example 2-30
[0118] Except for the addition amount of bis(fluorosulfonyl)imide lithium salt (LiFSI) in <Preparation of electrolyte>, the mass percentage of bis(fluorosulfonyl)imide lithium salt (LiFSI) is adjusted to 1% based on the mass of the electrolyte, and the rest is the same as Example 1-1. Among them, when the mass percentage of bis(fluorosulfonyl)imide lithium salt (LiFSI) changes, the mass percentage of the base solvent changes accordingly, and the mass percentage of lithium hexafluorophosphate (LiPF6) remains unchanged, that is, the mass percentage of the electrolyte C4% is 10%.
[0119] Example 2-31
[0120] Except for adjusting the amount of lithium hexafluorophosphate (LiPF6) added in <Preparation of Electrolyte>, the mass percentage of lithium hexafluorophosphate (LiPF6) is 13% based on the mass of the electrolyte, and the rest is the same as Example 1-1. Among them, when the mass percentage of lithium hexafluorophosphate (LiPF6) changes, the mass percentage of the base solvent changes accordingly, and the mass percentage of lithium bis(fluorosulfonyl)imide (LiFSI) remains unchanged, that is, the mass percentage of the electrolyte C4% is 18%.
[0121] Example 2-32
[0122] Except that in <Preparation of Electrolyte>, the solvent was adjusted to propylene carbonate (PC), dimethyl carbonate (DMC), and ethyl butyrate (EB) in a mass ratio of 3:6:1, the rest was the same as Example 1-1.
[0123] Comparative Examples 1 to 5
[0124] Except that the content of the compound shown in Formula 1 and / or the compound shown in Formula 2 is adjusted according to Table 1 in <Preparation of Electrolyte>, the rest is the same as Example 1-1. Wherein, when the content of the compound shown in Formula 1 or the compound shown in Formula 2 changes, the mass percentage of the base solvent changes accordingly, and the mass percentage of the electrolyte remains unchanged. In Table 1, vinyl sulfate is abbreviated as DTD, and 1,3-propane sultone is abbreviated as PS.
[0125] The preparation parameters and performance parameters of each embodiment and comparative example are shown in Tables 1 and 2.
[0126] Table 1
[0127]
[0128] Note: “ / ” in Table 1 indicates that there is no corresponding preparation parameter or substance.
[0129] It can be seen from Examples 1-1 to 1-26 and Comparative Examples 1 to 5 that the electrochemical devices of the embodiments of the present application, the electrolyte includes the compound represented by Formula 1 and the compound represented by Formula 2 within the scope of the present application, while the electrochemical devices in the comparative examples do not simultaneously meet the above characteristics. The electrochemical devices obtained in the embodiments have a higher capacity retention rate, a smaller internal resistance growth rate, and no gas is produced during storage, indicating that the electrochemical devices have good high-temperature cycle performance, high-temperature storage performance and a smaller internal resistance growth rate.
[0130] The type of compound represented by Formula 1 usually affects the high-temperature cycle performance, high-temperature storage performance and internal resistance growth rate of the electrochemical device. It can be seen from Examples 1-1 to 1-10 and Comparative Example 2 that when the electrolyte includes the compound represented by Formula 1 within the scope of the present application, the obtained electrochemical device has a higher capacity retention rate, a smaller internal resistance growth rate, and no gas is generated during storage, indicating that the electrochemical device has good high-temperature cycle performance, high-temperature storage performance and a smaller internal resistance growth rate.
[0131] The type of compound represented by Formula 2 usually affects the high-temperature cycle performance, high-temperature storage performance and internal resistance growth rate of the electrochemical device. It can be seen from Example 1-1, Example 1-11 to Example 1-25, Comparative Example 1, Comparative Example 4 to Comparative Example 5 that when the electrolyte includes the compound represented by Formula 2 within the scope of the present application, the obtained electrochemical device has a higher capacity retention rate, a smaller internal resistance growth rate, and no gas is generated during storage, indicating that the electrochemical device has good high-temperature cycle performance, high-temperature storage performance and a smaller internal resistance growth rate.
[0132] Table 2
[0133]
[0134] The mass ratio of the compound represented by Formula 1 to the compound represented by Formula 2 usually affects the high-temperature cycle performance, high-temperature storage performance and internal resistance growth rate of the electrochemical device. It can be seen from Examples 1-1, 2-1 to 2-11 that by regulating the mass ratio of the compound represented by Formula 1 to the compound represented by Formula 2 in the electrolyte within the scope of this application, the obtained electrochemical device has a higher capacity retention rate, a smaller internal resistance growth rate, and storage without gas production, indicating that the electrochemical device has good high-temperature cycle performance, high-temperature storage performance and a smaller internal resistance growth rate. Compared with Examples 1-1, 2-2 to 2-4, the mass ratio of the compound represented by Formula 1 to the compound represented by Formula 2 in Example 2-1 is less than 0.1, its capacity retention rate is slightly smaller, and the internal resistance growth rate is slightly larger, and the improvement of the high-temperature cycle performance and high-temperature storage performance of the electrochemical device is weak. Compared with Example 1-1 and Example 2-2 to Example 2-4, the mass ratio of the compound represented by Formula 1 to the compound represented by Formula 2 in Example 2-5 is greater than 16, its capacity retention rate is slightly smaller, the internal resistance growth rate is slightly larger, and the improvement of the high temperature cycle performance and high temperature storage performance of the electrochemical device is weak.
[0135] The value of the mass percentage C1% of the compound represented by Formula 1 usually affects the high-temperature cycle performance, high-temperature storage performance and internal resistance growth rate of the electrochemical device. It can be seen from Example 1-1 and Example 2-1 to Example 2-5 that by regulating the value of the mass percentage C1% of the compound represented by Formula 1 within the scope of the present application, the obtained electrochemical device has a higher capacity retention rate, a smaller internal resistance growth rate, and no gas is produced during storage, indicating that the electrochemical device has good high-temperature cycle performance, high-temperature storage performance and a smaller internal resistance growth rate.
[0136] The mass percentage C2% value of the compound shown in Formula 2 usually affects the high-temperature cycle performance, high-temperature storage performance and internal resistance growth rate of the electrochemical device. It can be seen from Implementation 1-1 and Example 2-6 to Example 2-11 that by regulating the mass percentage C2% value of the compound shown in Formula 2 within the scope of the present application, the obtained electrochemical device has a higher capacity retention rate, a smaller internal resistance growth rate, and no gas is produced during storage, indicating that the electrochemical device has good high-temperature cycle performance, high-temperature storage performance and a smaller internal resistance growth rate.
[0137] The relationship between the particle size D50 of the negative electrode active material, the bonding force m between the negative electrode material layer and the negative electrode current collector, and the mass percentage C2% of the compound shown in Formula 2 will affect the high temperature cycle performance, high temperature storage performance and internal resistance growth rate of the electrochemical device. It can be seen from Examples 1-1, 2-6 to 2-24 that by adjusting the values of D50, m, and C2 to satisfy the relationship I, the obtained electrochemical device has a higher capacity retention rate, a smaller internal resistance growth rate, and no gas is produced during storage, indicating that the electrochemical device has good high temperature cycle performance, high temperature storage performance and a smaller internal resistance growth rate. It can be seen from Examples 2-21 to 2-24 that the values of D50, m, and C2 do not satisfy the relationship I, and the obtained electrochemical device has a lower capacity retention rate, a higher internal resistance growth rate, and gas is produced during storage, indicating that the improvement of the high temperature cycle performance and high temperature storage performance of the electrochemical device is weak.
[0138] The mass percentage and type of other electrolyte additives usually affect the high-temperature cycle performance, high-temperature storage performance and internal resistance growth rate of the electrochemical device. It can be seen from Example 1-1 and Example 2-25 to Example 2-28 that the electrolyte includes other additives within the scope of the present application, and the mass percentage is regulated within the scope of the present application. The obtained electrochemical device has a higher capacity retention rate, a smaller internal resistance growth rate, and no gas is produced during storage, indicating that the electrochemical device has good high-temperature cycle performance, high-temperature storage performance and a smaller internal resistance growth rate.
[0139] The type and mass percentage of the electrolyte usually affect the high-temperature cycle performance, high-temperature storage performance and internal resistance growth rate of the electrochemical device. It can be seen from Examples 1-1 and 2-29 to 2-31 that the electrolyte includes electrolytes within the scope of the present application, and its mass percentage is regulated within the scope of the present application. The obtained electrochemical device has a higher capacity retention rate, a smaller internal resistance growth rate, and no gas is produced during storage, indicating that the electrochemical device has good high-temperature cycle performance, high-temperature storage performance and a smaller internal resistance growth rate.
[0140] The type and mass percentage of the solvent usually affect the high-temperature cycle performance, high-temperature storage performance and internal resistance growth rate of the electrochemical device. It can be seen from Examples 1-1 and 2-1 to 2-32 that the electrolyte includes a solvent within the scope of the present application, and its mass percentage is regulated within the scope of the present application. The obtained electrochemical device has a higher capacity retention rate, a smaller internal resistance growth rate, and no gas is produced during storage, indicating that the electrochemical device has good high-temperature cycle performance, high-temperature storage performance and a smaller internal resistance growth rate.
[0141] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present application shall be included in the scope of protection of the present application.
Claims
1. An electrolyte additive, comprising a compound of Formula 1 and a compound of Formula 2, wherein the compound of Formula 2 is selected from at least one of a compound of Formula 2-A and a compound of Formula 2-B: ; wherein m and n are each independently selected from integers from 0 to 3, and m and n are not both 0, p is selected from integers from 1 to 5, R0 is selected from a single bond or a methylene group, R1 is selected from hydrogen, halogen, a C1-C5 hydrocarbon group or a C1-C5 halogenated hydrocarbon group, and R2, R3, and R4 are each independently selected from or One of; R5 and R6 are each independently selected from substituted or unsubstituted phenyl, substituted or unsubstituted imidazolyl, substituted or unsubstituted C1-C5 alkyl, substituted or unsubstituted C2-C5 alkenyl, C1-C5 alkoxy, substituted or unsubstituted C2-C5 alkoxyalkyl, substituted or unsubstituted C1-C5 carbonyl, substituted or unsubstituted C1-C5 cyano, halogen. When substituted, the substituents are each independently selected from halogen and C1-C5 alkyl; R7 and R9 are each independently selected from halogen, substituted or unsubstituted C1-C5 alkyl, R8 is selected from substituted or unsubstituted phenylene, substituted or unsubstituted C1-C5 alkylene, C2-C5 alkenylene, C2-C5 alkynylene, C2-C5 alkyleneoxyalkylene, and when substituted, the substituents are each independently selected from halogen, hydroxyl, and phenyl; in, The mass ratio of the compound represented by Formula 1 to the compound represented by Formula 2 is (0.1-16):1; Based on the mass of the electrolyte, the mass percentage of the compound represented by Formula 1 is C1%, 0.05≤C1≤8, or, based on the mass of the electrolyte, the mass percentage of the compound represented by Formula 2 is C2%, 0.1≤C2≤5.
2. The electrolyte additive according to claim 1, wherein The compound represented by Formula 1 is selected from at least one of the following compounds: 。 3. The electrolyte additive according to claim 2, wherein The compound represented by Formula 1 is selected from the compound represented by Formula 1-1.
4. The electrolyte additive according to claim 1, wherein The compound represented by formula 2-A is selected from at least one of the following compounds: 。 5. The electrolyte additive according to claim 1, wherein The compound represented by formula 2-B is selected from at least one of the following compounds: 。 6. The electrolyte additive according to claim 4, wherein The compound represented by Formula 2 is selected from the compound represented by Formula 2-A10. 7 . An electrolyte comprising a solvent, an electrolyte and the electrolyte additive according to claim 1 .
8. The electrolyte according to claim 7, wherein Based on the mass of the electrolyte, the mass percentage of the compound represented by Formula 1 is C1%, 0.05≤C1≤8; and / or, based on the mass of the electrolyte, the mass percentage of the compound represented by Formula 2 is C2%, 0.1≤C2≤5.
9. The electrolyte according to any one of claims 7 to 8, wherein The solvent is selected from at least one of cyclic carbonates, linear carbonates and linear carboxylates; the cyclic carbonate is selected from at least one of ethylene carbonate and propylene carbonate; the linear carbonate is selected from at least one of dimethyl carbonate, diethyl carbonate and ethyl methyl carbonate; the linear carboxylates are selected from at least one of ethyl acetate, ethyl butyrate, ethyl propionate, methyl propionate, propyl propionate and propyl acetate; based on the mass of the electrolyte, the mass percentage of the solvent is C3%, 60≤C3≤89; and / or the electrolyte The mass is selected from lithium salt or sodium salt; the lithium salt is selected from at least one of lithium hexafluorophosphate, bisfluorosulfonyl imide lithium salt and bistrifluoromethanesulfonyl imide; the sodium salt is selected from at least one of sodium hexafluorophosphate, sodium tetrafluoroborate, bisfluorosulfonyl imide sodium salt, bistrifluoromethylsulfonyl imide sodium, sodium bisoxalate borate, sodium difluorobisoxalate borate, sodium difluorobisoxalate phosphate, sodium tetrafluorooxalate phosphate and 4,5-dicyano-2-trifluoromethyl-imidazole sodium; based on the mass of the electrolyte, the mass percentage of the electrolyte is C4%, 10≤C4≤18.
10. The electrolyte according to any one of claims 7 to 8, further comprising other electrolyte additives, wherein the other electrolyte additives are selected from at least one of lithium tetrafluoroborate and 1,3-propane sultone; based on the mass of the electrolyte, the mass percentage of the other electrolyte additives is C5%, 0.1≤C5≤20.
11. An electrochemical device comprising a positive electrode sheet, a negative electrode sheet, a separator and the electrolyte according to any one of claims 7 to 10; The negative electrode sheet includes a negative electrode current collector and a negative electrode material layer disposed on at least one surface of the negative electrode current collector, the negative electrode material layer includes a negative electrode active material, a negative electrode conductive agent and a negative electrode binder, and the electrochemical device satisfies the relational formula I: , in, D 50 is the particle size corresponding to 50% volume accumulation measured from the small particle size in the volume-based particle size distribution of the negative electrode active material particles, in μm; m is the bonding force between the negative electrode material layer and the negative electrode current collector, in N / m; C2% is the mass percentage of the compound represented by Formula 2 based on the mass of the electrolyte.
12. The electrochemical device according to claim 11, which satisfies at least one of the following conditions: (1) 7μm≤D 50 ≤15μm; (2) 3N / m≤m≤30N / m.