A nano-precipitation strengthened high-strength and high-corrosion-resistant copper alloy and its preparation method and application

By uniformly distributing nanoscale precipitates in copper-nickel alloys, combined with specific heat treatment methods, the problem of insufficient strength and corrosion resistance of copper-nickel alloys in marine environments is solved, and high strength and corrosion resistance are improved, which is suitable for Optimized design of copper-nickel alloys for marine engineering and marine applications.

CN118497548BActive Publication Date: 2024-10-18GRIMAT ENG INST CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410976952.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-10-18
Estimated Expiration
2044-07-22

AI Technical Summary

Technical Problem

Existing copper-nickel alloys have insufficient strength and corrosion resistance in complex marine environments and cannot meet the development needs of large-scale ocean engineering and ship equipment.

Method used

Using nano-precipitation-strengthened high-strength and high-corrosion-resistant copper alloy, the nano-scale Cr2Ni phase and/or Cr2Fe phase is evenly dispersed in the copper alloy, combined with homogenization treatment, hot extrusion, cold drawing and annealing treatment to form a high-density and Uniformly distributed nano-precipitated phases improve the strength and corrosion resistance of the alloy.

Benefits of technology

Significantly improve the tensile strength, yield strength and corrosion resistance of copper-nickel alloy, reduce the corrosion rate in marine environment, and enhance the service reliability in marine environment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118497548B_ABST
    Figure CN118497548B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of copper alloys, and specifically relates to a nano-precipitation-strengthened high-strength and high-corrosion-resistant copper alloy, and a preparation method and application thereof. The nano-precipitation-strengthened high-strength and high-corrosion-resistant copper alloy provided by the present invention comprises the following elements in percentage by mass: 8-16wt% of Ni element, 1-2wt% of the sum of Fe element and Cr element, the mass ratio of Fe element and Cr element ≥3:1, 1-2wt% of Mn element, 1-3wt% of Al element, 0.01-0.03wt% of Ce element, and the remainder of Cu element. The present invention achieves a uniformly dispersed precipitation phase in the alloy matrix by optimizing the types and content of copper alloy elements, and realizes the nano-precipitation-strengthened high-strength and high-corrosion-resistant copper alloy to synergistically improve the strength and corrosion performance of the copper-nickel alloy, and effectively improves the service reliability of the copper-nickel alloy in the marine environment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of copper alloys, and in particular relates to a nano-precipitation strengthened high-strength and high-corrosion-resistant copper alloy and a preparation method and application thereof. Background Art

[0002] Copper-nickel alloy is a key material for ships and marine engineering due to its good seawater corrosion resistance, anti-fouling performance and excellent cold and hot processing performance. It is widely used in cooling water pipelines for main and auxiliary engines of ships, fire water pipelines for offshore oil production platforms, heat exchangers in coastal power plants, and seawater cooling systems such as brine heaters for multi-stage flash evaporation devices for seawater desalination. Complex marine environments such as high-salinity, high-humidity and high-pressure seawater environments, alternating dry and wet splash zones and tidal range zones, as well as deep-sea high hydrostatic pressure and ocean currents place stringent requirements on copper-nickel alloys for marine engineering and ships. The materials should have comprehensive properties such as high strength, corrosion resistance and high toughness. With the development of large-scale marine engineering and ship equipment, the most important needs and challenges come from reducing overall weight and increasing safety. Therefore, the research and development of high-strength and high-corrosion-resistant copper-nickel alloys for marine engineering and ships is the current development trend.

[0003] Copper-nickel alloy is a type of copper alloy with Ni as the main added element. It is generally believed that copper-nickel alloy is a solid solution and does not contain a second phase in the matrix. Its strength is mainly due to solid solution strengthening. With the development of large-scale marine engineering and ship equipment, higher requirements are placed on the strength and corrosion resistance of copper-nickel alloys. At present, the strength of copper-nickel alloys has reached its limit only by solid solution strengthening, and its corrosion resistance is unstable in the complex marine service environment. Corrosion failure is still inevitable, which cannot meet the development requirements of large-scale marine engineering and ship equipment. Summary of the invention

[0004] The purpose of the present invention is to provide a nano-precipitation strengthened high-strength and high-corrosion-resistant copper alloy and a preparation method and application thereof. The nano-precipitation strengthened high-strength and high-corrosion-resistant copper alloy provided by the present invention synergistically improves the strength and corrosion performance of the copper-nickel alloy, thereby effectively improving the service reliability of the copper-nickel alloy in the marine environment.

[0005] In order to achieve the above object, the present invention provides the following technical solutions:

[0006] The present invention provides a nano-precipitation strengthened high-strength and high-corrosion resistant copper alloy, comprising the following elements in percentage by weight: 8-16wt% of Ni element, 1-2wt% of the sum of Fe element and Cr element, the mass ratio of Fe element to Cr element being ≥3:1, 1-2wt% of Mn element, 1-3wt% of Al element, 0.01-0.03wt% of Ce element, and the remainder of Cu element and unavoidable impurity elements;

[0007] The nano-precipitation strengthened high-strength and high-corrosion resistant copper alloy comprises a matrix and a second phase dispersedly distributed inside the matrix; the second phase comprises a Cr2Ni phase and / or a Cr2Fe phase, and the second phase is nanoscale.

[0008] Preferably, the average grain size of the nano-precipitation strengthened high-strength and high-corrosion resistant copper alloy is 50~100μm; the percentage of low ΣCSL grain boundaries in the nano-precipitation strengthened high-strength and high-corrosion resistant copper alloy is ≥30%; and the average grain size of the second phase is 10~50nm.

[0009] The present invention provides a method for preparing the nano-precipitation strengthened high-strength and high-corrosion-resistant copper alloy described in the above technical solution, comprising the following steps:

[0010] The raw materials for preparing the nano-precipitation-strengthened high-strength and high-corrosion-resistant copper alloy are melted, and the obtained melt is cast to obtain an ingot;

[0011] The ingot is heated and homogenized to obtain a homogenized copper alloy billet;

[0012] The homogenized copper alloy billet is subjected to hot extrusion treatment and then water-cooled to obtain a first deformed copper alloy billet;

[0013] cold drawing the first deformed copper alloy billet to obtain a second deformed copper alloy billet;

[0014] The second deformed copper alloy billet is annealed to obtain the nano-precipitation strengthened high-strength and high-corrosion resistant copper alloy.

[0015] Preferably, the raw materials for preparing the nano-precipitation strengthened high-strength and high-corrosion-resistant copper alloy include: copper element, nickel element, manganese element, aluminum element, copper-iron master alloy, copper-chromium master alloy and copper-cerium master alloy; the mass percentage of iron element in the copper-iron master alloy is 10~20wt%; the mass percentage of chromium element in the copper-chromium master alloy is 10~20wt%; the mass percentage of cerium element in the copper-cerium master alloy is 10~20wt%.

[0016] Preferably, the smelting temperature is 1150-1400°C.

[0017] Preferably, the temperature of the homogenization treatment is 900-1000° C., and the insulation time is 2-8 hours.

[0018] Preferably, the extrusion deformation amount of the hot extrusion treatment is 40-90%, the initial temperature of the homogenized copper alloy billet during the hot extrusion treatment is 900-1000°C, and the temperature of the extrusion barrel and the die used in the hot extrusion treatment is 400-700°C.

[0019] Preferably, the deformation amount of the cold drawing process is 50-99%.

[0020] Preferably, the annealing treatment temperature is 700-850° C., the holding time is 0.5-2 h, and the cooling method is furnace cooling.

[0021] The present invention provides the application of the nano-precipitation strengthened high-strength and high-corrosion-resistant copper alloy described in the above technical scheme or the nano-precipitation strengthened high-strength and high-corrosion-resistant copper alloy prepared by the preparation method described in the above technical scheme in marine engineering and ship seawater cooling systems.

[0022] The present invention provides a nano precipitation-strengthened high-strength and high-corrosion-resistant copper alloy, comprising the following elements in percentage by weight: 8-16wt% Ni element, 1-2wt% of the sum of Fe element and Cr element, the mass ratio of Fe element and Cr element ≥3:1, 1-2wt% Mn element, 1-3wt% Al element, 0.01-0.03wt% Ce element, and the remainder of Cu element and inevitable impurity elements; the nano precipitation-strengthened high-strength and high-corrosion-resistant copper alloy comprises a matrix and a second phase dispersedly distributed inside the matrix; the second phase comprises a Cr2Ni phase and / or a Cr2Fe phase, and the second phase is nanoscale. At present, the strengthening methods of alloy materials include fine grain strengthening, solid solution strengthening, work hardening and second phase (precipitation phase) strengthening. However, for corrosion-resistant alloy materials, due to the different potentials between the precipitation phase and the matrix, phase selection corrosion may occur around the precipitation phase, thereby accelerating the corrosion of the alloy material. Therefore, the precipitation of the second phase is usually avoided when designing the corrosion-resistant alloy. The present invention overcomes the above-mentioned technical prejudices and achieves a uniformly dispersed nanoscale precipitated phase (Cr2Ni phase and / or Cr2Fe phase) in the alloy matrix by optimizing the types and contents of copper alloy elements, so that the copper alloy provided by the present invention obtains a uniform microstructure with a good strengthening mechanism; at the same time, the uniformly dispersed nanoscale precipitated phase can improve the electrochemical uniformity of the copper alloy and the overall potential of the copper alloy matrix, thereby reducing the micro-galvanic corrosion between the second phase and the matrix. Since the second phase is nanoscale, the galvanic corrosion can be ignored, and it is beneficial to form a uniform oxide film and improve the oxide film repair ability, thereby achieving the nano-precipitation-strengthened high-strength and high-corrosion-resistant copper alloy to synergistically improve the strength and corrosion performance of the copper-nickel alloy, and effectively improve the service reliability of the copper-nickel alloy in the marine environment.

[0023] The present invention provides a method for preparing a nano-precipitation-strengthened high-strength and high-corrosion-resistant copper alloy as described in the above technical solution, comprising the following steps: smelting the raw materials for preparing the nano-precipitation-strengthened high-strength and high-corrosion-resistant copper alloy, casting the obtained melt, and obtaining an ingot; heating the ingot for homogenization treatment to obtain a homogenized copper alloy billet; hot extruding the homogenized copper alloy billet and then water cooling it to obtain a first deformed copper alloy billet; cold drawing the first deformed copper alloy billet to obtain a second deformed copper alloy billet; annealing the second deformed copper alloy billet to obtain the nano-precipitation-strengthened high-strength and high-corrosion-resistant copper alloy. The present invention adopts alloying and a deformation heat treatment method of "homogenization treatment → hot extrusion treatment → cold drawing deformation treatment → annealing treatment" to finely control the microscopic morphology and distribution of the second phase of the copper alloy, so as to achieve the precipitation of a uniformly dispersed precipitation phase inside the copper alloy matrix, and effectively improve the strength and corrosion resistance of the copper-nickel alloy.

[0024] The results of the embodiment show that the tensile strength of the nano-precipitation-strengthened high-strength and high-corrosion-resistant copper alloy provided by the present invention is ≥400MPa, the yield strength is ≥200MPa, the elongation after fracture is ≥30%, the static seawater immersion uniform corrosion rate is <0.015mm / a at room temperature, and the clean artificial seawater (wherein the chemical composition of the clean artificial seawater is shown in Table 1) at a flow rate of 3m / s at room temperature is ≤0.035mm / a. The nano-precipitation-strengthened high-strength and high-corrosion-resistant copper alloy provided by the present invention can be widely used in cooling water pipelines of main and auxiliary engines of ships, fire water pipelines of offshore oil production platforms, heat exchangers of coastal power plants, and brine heaters of multi-stage flash evaporation devices for seawater desalination, etc. Seawater cooling systems provide a theoretical basis for the optimized design of high-strength and high-corrosion-resistant copper-nickel alloys for marine engineering and ships and their service reliability in marine environments.

[0025] Table 1 Chemical composition of clean artificial seawater

[0026]

[0027] Furthermore, in the present invention, the average grain size of the nano-precipitation-strength high-strength and high-corrosion-resistant copper alloy is 50-100 μm; the percentage of low ΣCSL grain boundaries in the nano-precipitation-strength high-corrosion-resistant copper alloy is ≥30%. The present invention controls the average grain size of the nano-precipitation-strength high-strength and high-corrosion-resistant copper alloy to 50-100 μm, and at the same time, the percentage of low ΣCSL grain boundaries in the nano-precipitation-strength high-strength and high-corrosion-resistant copper alloy is ≥30%. While having a large number of high-density and dispersedly distributed precipitation phases in the matrix of the nano-precipitation-strength high-strength and high-corrosion-resistant copper alloy, the occurrence of intergranular corrosion is reduced, and the corrosion resistance and strength of the copper alloy are further improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 This is a statistical diagram of special grain boundaries and grain sizes of samples prepared in Example 1 of the present invention;

[0029] Figure 2 This is a statistical diagram of special grain boundaries and grain sizes of samples prepared in Example 2 of the present invention;

[0030] Figure 3 This is a statistical diagram of special grain boundaries and grain sizes of samples prepared in Example 3 of the present invention;

[0031] Figure 4 This is a statistical diagram of special grain boundaries and grain sizes of samples prepared in Example 4 of the present invention;

[0032] Figure 5 This is a statistical diagram of special grain boundaries and grain sizes of the samples prepared in comparative example 1 of the present invention. DETAILED DESCRIPTION

[0033] The present invention provides a nano-precipitation strengthened high-strength and high-corrosion resistant copper alloy, comprising the following elements in percentage by weight: 8-16wt% of Ni element, 1-2wt% of the sum of Fe element and Cr element, the mass ratio of Fe element to Cr element being ≥3:1, 1-2wt% of Mn element, 1-3wt% of Al element, 0.01-0.03wt% of Ce element, and the remainder of Cu element and unavoidable impurity elements;

[0034] The nano-precipitation strengthened high-strength and high-corrosion resistant copper alloy comprises a matrix and a second phase uniformly dispersed in the matrix; the second phase comprises a Cr2Ni phase and / or a Cr2Fe phase, and the second phase is nanoscale.

[0035] In the present invention, unless otherwise specified, all preparation raw materials / components are commercially available products well known to those skilled in the art.

[0036] In terms of mass percentage, the nano-precipitation strengthened high-strength and high-corrosion resistant copper alloy provided by the present invention includes 8-16wt% of Ni element, preferably 8.5-15.5wt%, and specifically preferably 8.8wt%, 11wt% or 15wt%.

[0037] In the present invention, the Ni element can be infinitely soluble in the Cu matrix. The addition of Ni can improve the overall corrosion potential of the copper alloy on the one hand, and on the other hand, during the corrosion process, Ni ions will fill the defective positions of the corrosion product film to make the film layer complete and dense, thereby improving the corrosion resistance of the copper alloy.

[0038] In terms of mass percentage, the nano-precipitation strengthened high-strength and high-corrosion resistant copper alloy provided by the present invention includes 1-2wt% of the sum of Fe and Cr elements, and the mass ratio of Fe and Cr elements is ≥3:1. In the present invention, the sum of the Fe and Cr elements is preferably 1.1-2wt%, and specifically preferably 1.1wt%, 1.2wt%, 1.3wt%, 1.4wt%, 1.7wt%, 1.8wt%, 1.9wt% or 2wt%. The mass ratio of the Fe and Cr elements is preferably (4-19):1, and specifically preferably 4:1, 5:1, 17:3 or 19:1.

[0039] In terms of mass percentage, the nano-precipitation strengthened high-strength and high-corrosion resistant copper alloy provided by the present invention preferably includes 1-1.9wt% of Fe element, and specifically preferably 1.9wt%, 1.7wt%, 1.6wt% or 1wt%.

[0040] In the present invention, the addition of Fe element can not only refine the grains, but also affect the composition and structure of the copper-nickel alloy corrosion film, thereby improving the corrosion resistance of the copper-nickel alloy.

[0041] In terms of mass percentage, the nano-precipitation strengthened high-strength and high-corrosion resistant copper alloy provided by the present invention preferably includes 0.1-0.4wt% of Cr element, and specifically preferably 0.1wt%, 0.3wt%, 0.4wt% or 0.2wt%.

[0042] In the present invention, the Cr element, as a corrosion inhibition element, can replace part of the role of Fe, and the addition of the Cr element will precipitate a nanometer second phase inside the grains.

[0043] In terms of mass percentage, the nano-precipitation strengthened high-strength and high-corrosion resistant copper alloy provided by the present invention includes 1-2wt% of Mn element, preferably 1-1.5wt%, and specifically preferably 1wt%, 1.5wt% or 1.3wt%.

[0044] In the present invention, Mn element is added to the copper-nickel alloy together with Fe element. Mn element can supplement the effect of Fe element to a certain extent. A proper amount of Mn element can significantly improve the strength and erosion corrosion resistance of the copper-nickel alloy.

[0045] In terms of mass percentage, the nano-precipitation strengthened high-strength and high-corrosion resistant copper alloy provided by the present invention includes 1-3wt% of Al element, preferably 1-2.5wt%, and specifically preferably 1wt%, 2wt% or 2.5wt%.

[0046] In the present invention, the Al element can promote the formation of a tough and dense Al2O3 protective film on the surface of the copper-nickel alloy, reduce the surface activity of the copper alloy, and at the same time, the Al element can greatly improve the strength of the alloy.

[0047] Calculated by mass percentage, the nano-precipitation strengthened high-strength and high-corrosion-resistant copper alloy provided by the present invention includes 0.01-0.03wt% of Ce element, and specifically preferably 0.01wt%, 0.02wt% or 0.03wt%.

[0048] In the present invention, the Ce element plays a role in purifying the matrix of the copper alloy and improving the corrosion resistance.

[0049] Measured in percentage by mass, the nano-precipitation strengthened high-strength and high-corrosion resistant copper alloy provided by the present invention includes a balance of Cu elements and unavoidable impurity elements.

[0050] The nano-precipitation-strength high-corrosion-resistant copper alloy provided by the present invention includes a matrix and a second phase uniformly dispersed inside the matrix; the second phase includes a Cr2Ni phase and / or a Cr2Fe phase, and the second phase is nanoscale. In the present invention, the matrix of the nano-precipitation-strength high-corrosion-resistant copper alloy is a copper-nickel solid solution. The average grain size of the nano-precipitation-strength high-corrosion-resistant copper alloy is preferably 50-100 μm, more preferably 53-80 μm, and specifically preferably 53.7 μm, 57.2 μm, 76.4 μm or 70.6 μm. The percentage of low ΣCSL grain boundaries in the nano-precipitation-strength high-corrosion-resistant copper alloy is preferably ≥30%, preferably 31-55%, and specifically preferably 53%, 49.3%, 43.9% or 31%. In the present invention, the percentage of low ΣCSL grain boundaries in the nano-precipitation strengthened high-strength and high-corrosion resistant copper alloy is obtained by computer software statistics, and the percentage of special grain boundaries to all grain boundaries is calculated according to the length ratio.

[0051] In the present invention, the average particle size of the second phase is preferably 10 to 50 nm.

[0052] In the present invention, the corrosion of the nano-precipitation-strength high-strength and high-corrosion-resistant copper alloy often occurs at the grain boundary and gradually expands into the grain. In order to reduce the occurrence of intergranular corrosion, the average grain size of the nano-precipitation-strength high-corrosion-resistant copper alloy is preferably 50-100 μm.

[0053] The tensile strength of the nano-precipitation strengthened high-strength and high-corrosion-resistant copper alloy provided by the present invention is ≥400 MPa, preferably 405-460 MPa, and specifically preferably 406 MPa, 440 MPa, 435 MPa or 455 MPa.

[0054] The yield strength of the nano-precipitation strengthened high-strength and high-corrosion-resistant copper alloy provided by the present invention is ≥200MPa.

[0055] The nano-precipitation strengthened high-strength and high-corrosion-resistant copper alloy provided by the present invention has an elongation after fracture of ≥30%, preferably 35-40%, and specifically preferably 40%, 38%, 36% or 37%.

[0056] The nano-precipitation strengthened high-strength and high-corrosion-resistant copper alloy provided by the present invention has a uniform corrosion rate of less than 0.015 mm / a, preferably less than 0.02 mm / a, and specifically preferably 0.0112 mm / a, 0.0102 mm / a, 0.0124 mm / a or 0.0115 mm / a, when immersed in static seawater at room temperature.

[0057] The nano-precipitation strengthened high-strength and high-corrosion resistant copper alloy provided by the present invention has a uniform corrosion rate of ≤0.035 mm / a, preferably ≤0.034 mm / a, and specifically preferably 0.0334 mm / a, 0.0247 mm / a, 0.0276 mm / a or 0.023 mm / a, when washed with clean artificial seawater (wherein the chemical composition of the clean artificial seawater is shown in Table 1) at a flow rate of 3 m / s under room temperature conditions.

[0058] The present invention provides a method for preparing the nano-precipitation strengthened high-strength and high-corrosion-resistant copper alloy described in the above technical solution, comprising the following steps:

[0059] The raw materials for preparing the nano-precipitation-strengthened high-strength and high-corrosion-resistant copper alloy are melted, and the obtained melt is cast to obtain an ingot;

[0060] The ingot is heated and homogenized to obtain a homogenized copper alloy billet;

[0061] The homogenized copper alloy billet is subjected to hot extrusion treatment and then water-cooled to obtain a first deformed copper alloy billet;

[0062] cold drawing the first deformed copper alloy billet to obtain a second deformed copper alloy billet;

[0063] The second deformed copper alloy billet is annealed to obtain the nano-precipitation strengthened high-strength and high-corrosion resistant copper alloy.

[0064] The present invention melts the raw materials for preparing the nano precipitation-strengthened high-strength and high-corrosion-resistant copper alloy, and casts the obtained melt to obtain an ingot. In the present invention, the raw materials for preparing the nano precipitation-strengthened high-strength and high-corrosion-resistant copper alloy preferably include: copper element, nickel element, manganese element, aluminum element, copper-iron master alloy, copper-chromium master alloy and copper-cerium master alloy. The copper element is preferably electrolytic copper. The nickel element is preferably electrolytic nickel. The purity of the manganese element is preferably ≥99.9%. The purity of the aluminum element is preferably ≥99.9%. The mass percentage of iron in the copper-iron master alloy is preferably 10~20wt%, and the remainder is copper and unavoidable impurity elements. In a specific embodiment of the present invention, the mass percentage of iron in the copper-iron master alloy is preferably 20wt%, recorded as Cu-20Fe. The mass percentage of chromium in the copper-chromium master alloy (recorded as Cu-20Cr) is 10~20wt%, and the remainder is copper and unavoidable impurity elements. In a specific embodiment of the present invention, the mass percentage of chromium in the copper-chromium master alloy is 20wt%, which is recorded as Cu-20Cr. The mass percentage of cerium in the copper-cerium master alloy is 10-20wt%, and the remainder is copper and unavoidable impurity elements. In a specific embodiment of the present invention, the mass percentage of cerium in the copper-cerium master alloy is 20wt%, which is recorded as Cu-20Ce.

[0065] In the present invention, the smelting is preferably carried out using a three-high graphite crucible. The smelting temperature is preferably 1150-1400°C, preferably 1200-1300°C, and specifically preferably 1250°C, 1200°C or 1300°C. In the present invention, after the smelting obtains the melt and before the casting, the present invention preferably stirs the melt evenly and covers it with charcoal, and performs heat preservation smelting in a protective gas atmosphere, and the heat preservation smelting time is preferably 1-4h. The protective gas is preferably an inert gas. The casting method is preferably a non-vacuum method.

[0066] After obtaining the ingot, the present invention heats the ingot for homogenization treatment to obtain a homogenized copper alloy billet. In the present invention, the temperature of the homogenization treatment is preferably 900-1000°C, more preferably 900-980°C, specifically preferably 900°C, 950°C or 980°C; the holding time is preferably 2-8h, specifically preferably 6h, 3h, 2h or 8h. In the present invention, the homogenization treatment is preferably carried out in a box-type resistance furnace. The present invention preferably removes the oxide skin from the ingot before carrying out the homogenization treatment. The thickness of the removed oxide skin is preferably 2-3mm, and the removal method is preferably a lathe.

[0067] After obtaining the homogenized copper alloy billet, the present invention performs hot extrusion treatment on the homogenized copper alloy billet and then water cools it to obtain a first deformed copper alloy billet. In the present invention, the extrusion deformation amount of the hot extrusion treatment is preferably 40-90%, more preferably 50-90%, further preferably 60-90%, and specifically preferably 75%, 87% or 90%. The temperature of the homogenized copper alloy billet during the hot extrusion treatment is preferably 900-1000°C, more preferably 900-980°C, specifically preferably 900°C, 950°C or 980°C. The hot extrusion treatment is preferably carried out in an extruder. The temperature of the extrusion barrel and the mold used in the hot extrusion treatment is preferably 400-700°C, more preferably 450-700°C, and specifically preferably 480°C, 550°C, 620°C or 700°C.

[0068] After obtaining the first deformed copper alloy billet, the present invention performs a cold drawing process on the first deformed copper alloy billet to obtain a second deformed copper alloy billet. In the present invention, the deformation amount of the cold drawing process is preferably 50-99%, and specifically preferably 65%, 99%, 85% or 50%. The present invention has no special requirements for the specific implementation process of the cold drawing process.

[0069] After obtaining the second deformed copper alloy billet, the present invention performs annealing treatment on the second deformed copper alloy billet to obtain the nano-precipitation strengthened high-strength and high-corrosion resistant copper alloy. In the present invention, the annealing temperature is preferably 700-850°C, and is specifically preferably 800°C, 850°C, 830°C or 700°C; the holding time is preferably 0.5-2h, and is specifically preferably 50min, 40min, 60min or 120min. The cooling is preferably furnace cooling.

[0070] The present invention adopts a method combining homogenization treatment → hot extrusion → cold deformation → annealing treatment to prepare a nano-precipitation-strength high-corrosion-resistant copper alloy with good grain size uniformity, and contains high-density and diffusely distributed nano-precipitated phases inside the grains, which synergistically improves the strength and corrosion resistance of the copper-nickel alloy. At the same time, by controlling the steps and parameters of the preparation method, the present invention obtains a nano-precipitation-strength high-corrosion-resistant copper alloy with an average grain size of 50~100μm, a percentage of special grain boundaries (low ΣCSL) ≥30%, and a large number of high-density and diffusely distributed nano-precipitated phases are precipitated inside the grains. Compared with traditional copper-nickel alloys, the nano-precipitation-strength high-corrosion-resistant copper alloy provided by the present invention has excellent mechanical and corrosion resistance matching.

[0071] The present invention provides the application of the nano-precipitation strengthened high-strength and high-corrosion-resistant copper alloy described in the above technical scheme or the nano-precipitation strengthened high-strength and high-corrosion-resistant copper alloy prepared by the preparation method described in the above technical scheme in marine engineering and ship seawater cooling systems.

[0072] In the present invention, the marine engineering and marine seawater cooling system preferably includes cooling water pipelines of ship main and auxiliary engines, fire water pipelines of offshore oil production platforms, heat exchangers of coastal power plants or brine heaters of seawater desalination multi-stage flash evaporation devices.

[0073] In order to further illustrate the present invention, the technical solutions provided by the present invention are described in detail below in conjunction with embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0074] Example 1

[0075] This embodiment provides a method for preparing a precipitation-strengthened high-strength and high-corrosion-resistant copper alloy for marine engineering and shipbuilding, which specifically comprises the following steps: (1) casting, (2) homogenization, (3) hot extrusion, (4) cold drawing, and (5) annealing.

[0076] In step (1), electrolytic copper, electrolytic nickel, pure manganese, pure aluminum, Cu-20Fe master alloy, Cu-20Cr master alloy, Cu-20Ce master alloy are used as raw materials, and the mass percentage (wt%) of each element is: Ni 8.5%, Fe 1.9%, Mn 1%, Cr 0.1%, Al 1%, Ce 0.01% and the balance of Cu and unavoidable impurity elements. The raw materials are added to a melting furnace. In order to control the content of impurity elements, a three-high graphite crucible is selected, and the temperature is raised to 1250°C. After the above raw materials are completely melted, they are stirred evenly, covered with charcoal, and inert gas is passed through the melting furnace for protection. After that, the obtained liquid alloy is placed in a mold for cooling by non-vacuum casting to cast the required ingot.

[0077] In step (2), the outer skin of the ingot in step (1) is turned off by 2 mm and then homogenized in a box-type resistance furnace. The homogenization temperature is 900° C. and the time is 6 hours.

[0078] In step (3), the extrusion barrel and the die are first preheated to a temperature of 480° C., and then the sample homogenized in step (2) is taken out and quickly sent to an extruder for hot extrusion. The hot extrusion deformation is 75%, and the copper rod blank after extrusion is water-cooled in water.

[0079] In step (4), the copper rod blank prepared in step (3) is cold drawn, and the total deformation is 65%.

[0080] In step (5), the copper rod in step (4) is annealed at a temperature of 800° C. for 50 min and a cooling method of furnace cooling to obtain a nano-precipitation-strengthened high-strength and high-corrosion-resistant copper alloy sample.

[0081] Figure 1This is a statistical diagram of special grain boundaries and grain sizes of the nano-precipitation strengthened high-strength and high-corrosion resistant copper alloy sample prepared in Example 1. Figure 1 The upper left and upper right figures are the percentages of special grain boundaries. Figure 1 The lower left and lower right figures in the figure are grain size distribution diagrams of the copper alloy. The results show that the average grain size of the nano-precipitation strengthened high-strength and high-corrosion resistant copper alloy sample obtained in this embodiment is 53.7μm, and the percentage of special grain boundaries (low ΣCSL) is 53%.

[0082] The nano-precipitation-strengthened high-strength and high-corrosion-resistant copper alloy sample obtained in Example 1 was subjected to performance tests, including room temperature tensile properties, room temperature yield strength properties, elongation after fracture, uniform corrosion rate of static seawater immersion under room temperature conditions, and uniform corrosion rate under clean artificial seawater (chemical composition as shown in Table 1) flushing conditions with a flow rate of 3 m / s at room temperature. Its performance is shown in Table 2. In Table 2: room temperature tensile strength, room temperature yield strength and elongation after fracture were tested in accordance with GB / T228.1-2010 "Metallic Material Tensile Test Part 1: Room Temperature Test Method". The uniform corrosion rate of static seawater immersion under room temperature conditions was tested in accordance with GB / T 6384-2008 "Seawater Corrosion Test Method for Metal Materials for Ships and Marine Engineering in Natural Environments". Determination of uniform corrosion rate under clean artificial seawater (chemical composition as shown in Table 1) flushing conditions with a flow rate of 3 m / s at room temperature The copper alloy sample was flushed with clean artificial seawater with the chemical composition shown in Table 1 at a speed of 3 m / s. The traditional B10 alloy in Table 2 is a commercially available product.

[0083] Table 2 Performance test results of nano-precipitation strengthened high-strength and high-corrosion-resistant copper alloy samples prepared in Example 1

[0084]

[0085] Example 2

[0086] The present embodiment provides a method for preparing a novel corrosion-resistant white copper alloy that is resistant to high-velocity seawater erosion, comprising the following steps: (1) casting, (2) homogenization, (3) hot extrusion, (4) cold drawing, and (5) annealing.

[0087] In step (1), electrolytic copper, electrolytic nickel, pure manganese, pure aluminum, Cu-20Fe master alloy, Cu-20Cr master alloy, and Cu-20Ce master alloy are used as raw materials, and their composition and the mass percentage content (wt%) of each element are: Ni 11%, Fe 1.7%, Mn 1.5%, Cr 0.3%, Al 2%, Ce 0.02%, and the remaining amount of Cu and inevitable impurity elements. The raw materials are added to the melting furnace. In order to control the content of impurity elements, a three-high graphite crucible is selected, and the temperature is raised to 1200°C. After the above raw materials are completely melted, they are stirred evenly, covered with charcoal, and inert gas is passed through the melting furnace for protection. After that, the obtained liquid alloy is placed in a mold for cooling by non-vacuum casting to cast the required ingot.

[0088] In step (2), the outer skin of the ingot in step (1) is turned off by 3 mm and then homogenized in a box-type resistance furnace. The homogenization temperature is 950° C. and the time is 3 hours.

[0089] In step (3), the extrusion barrel and the die are first preheated to a temperature of 550° C., and then the sample homogenized in step (2) is taken out and quickly sent to an extruder for extrusion, with an extrusion deformation of 87%. The extruded copper rod blank is water-cooled in water.

[0090] In step (4), the copper rod blank prepared in step (3) is cold drawn, and the total deformation amount is 99%.

[0091] In step (5), the copper rod in step (4) is annealed at a temperature of 850° C. for 40 min and a cooling method of furnace cooling to obtain a nano-precipitation-strengthened high-strength and high-corrosion-resistant copper alloy sample.

[0092] Figure 2 This is a statistical diagram of special grain boundaries and grain sizes of the nano-precipitation strengthened high-strength and high-corrosion resistant copper alloy sample prepared in Example 2. Figure 2 The upper left and upper right figures are the percentages of special grain boundaries. Figure 2 The lower left and right figures in the figure are grain size distribution diagrams of the copper alloy. The results show that the average grain size of the nano-precipitation strengthened high-strength and high-corrosion resistant copper alloy sample obtained in this embodiment is 57.2μm, and the percentage of special grain boundaries (low ΣCSL) is 49.3%.

[0093] The nano-precipitation-strengthened high-strength and high-corrosion-resistant copper alloy sample obtained in Example 2 was subjected to performance tests, including room temperature tensile properties, room temperature yield strength properties, elongation after fracture, uniform corrosion rate of static seawater immersion under room temperature conditions, and uniform corrosion rate under clean artificial seawater (chemical composition as shown in Table 1) flushing conditions with a flow rate of 3 m / s at room temperature. Its performance is shown in Table 3. In Table 3: room temperature tensile strength, room temperature yield strength and elongation after fracture were tested in accordance with GB / T228.1-2010 "Metallic Material Tensile Test Part 1: Room Temperature Test Method". The uniform corrosion rate of static seawater immersion under room temperature conditions was tested in accordance with GB / T 6384-2008 "Seawater Corrosion Test Method for Metal Materials for Ships and Marine Engineering in Natural Environments". Determination of uniform corrosion rate under clean artificial seawater (chemical composition as shown in Table 1) flushing conditions with a flow rate of 3 m / s at room temperature The copper alloy sample was flushed with clean artificial seawater with the chemical composition shown in Table 1 at a speed of 3 m / s. The traditional B10 alloy in Table 3 is a commercially available product.

[0094] Table 3 Performance test results of nano-precipitation strengthened high-strength and high-corrosion-resistant copper alloy samples prepared in Example 2

[0095]

[0096] Example 3

[0097] The present embodiment provides a method for preparing a novel corrosion-resistant white copper alloy that is resistant to high-velocity seawater erosion, comprising the following steps: (1) casting, (2) homogenization, (3) hot extrusion, (4) cold drawing, and (5) annealing.

[0098] In step (1), electrolytic copper, electrolytic nickel, pure manganese, pure aluminum, Cu-20Fe master alloy, Cu-20Cr master alloy, Cu-20Ce master alloy are used as raw materials, and the composition and mass percentage of each element (wt%) are: Ni 15%, Fe 1.6%, Mn 1.3%, Cr 0.4%, Al 2.5%, Ce 0.03%, and the balance of Cu and inevitable impurity elements. The raw materials are added to a melting furnace. In order to control the content of impurity elements, a three-high graphite crucible is selected, and the temperature is raised to 1300°C. After the above raw materials are completely melted, they are stirred evenly, covered with charcoal, and an inert gas is passed through the melting furnace for protection. Then, the obtained liquid alloy is placed in a mold for cooling by non-vacuum casting to cast the required ingot.

[0099] In step (2), the outer skin of the ingot in step (1) is turned off by 2 mm and then homogenized in a box-type resistance furnace. The homogenization temperature is 980° C. and the time is 2 h.

[0100] In step (3), the extrusion barrel and the die are first preheated to a temperature of 620° C., and then the sample homogenized in step (2) is taken out and quickly sent to an extruder for extrusion, with an extrusion deformation of 90%. The extruded copper rod blank is water-cooled in water.

[0101] In step (4), the copper rod blank prepared in step (3) is cold drawn, and the total deformation is 85%.

[0102] In step (5), the copper rod in step (4) is annealed at a temperature of 830° C. for a holding time of 60 min and a cooling method of furnace cooling to obtain a nano-precipitation-strengthened high-strength and high-corrosion-resistant copper alloy sample.

[0103] Figure 3 This is a statistical diagram of special grain boundaries and grain sizes of the nano-precipitation strengthened high-strength and high-corrosion-resistant copper alloy sample prepared in Example 3. Figure 3 The upper left and upper right figures are the percentages of special grain boundaries. Figure 3 The lower left and lower right figures in the figure are grain size distribution diagrams of the copper alloy. The results show that the average grain size of the nano-precipitation strengthened high-strength and high-corrosion resistant copper alloy sample prepared in Example 3 is 76.4 μm, and the percentage of special grain boundaries (low ΣCSL) is 43.9%.

[0104] The nano-precipitation-strengthened high-strength and high-corrosion-resistant copper alloy sample obtained in Example 3 was subjected to performance tests, including room temperature tensile properties, room temperature yield strength properties, elongation after fracture, uniform corrosion rate of static seawater immersion under room temperature conditions, and uniform corrosion rate under clean artificial seawater (chemical composition as shown in Table 1) flushing conditions with a flow rate of 3 m / s at room temperature. Its performance is shown in Table 4. In Table 4: room temperature tensile strength, room temperature yield strength and elongation after fracture were tested in accordance with GB / T228.1-2010 "Metallic Material Tensile Test Part 1: Room Temperature Test Method". The uniform corrosion rate of static seawater immersion under room temperature conditions was tested in accordance with GB / T 6384-2008 "Seawater Corrosion Test Method for Metal Materials for Ships and Marine Engineering in Natural Environments". Determination of uniform corrosion rate under clean artificial seawater (chemical composition as shown in Table 1) flushing conditions with a flow rate of 3 m / s at room temperature The copper alloy sample was flushed with clean artificial seawater with the chemical composition shown in Table 1 at a speed of 3 m / s. The traditional B10 alloy in Table 4 is a commercially available product. It includes room temperature tensile properties, corrosion rate after static immersion for 21 days at room temperature, and corrosion rate after flushing in artificial seawater at a flow rate of 3 m / s for 21 days at room temperature. Its properties are shown in Table 4.

[0105] Table 4 Performance test results of nano-precipitation strengthened high-strength and high-corrosion-resistant copper alloy samples prepared in Example 3

[0106]

[0107] Example 4

[0108] The present embodiment provides a method for preparing a novel corrosion-resistant white copper alloy that is resistant to high-velocity seawater erosion, comprising the following steps: (1) casting, (2) homogenization, (3) hot extrusion, (4) cold drawing, and (5) annealing.

[0109] In step (1), electrolytic copper, electrolytic nickel, pure manganese, pure aluminum, Cu-20Fe master alloy, Cu-20Cr master alloy, and Cu-20Ce master alloy are used as raw materials, and the composition and mass percentage of each element (wt%) are: Ni 15%, Fe 1%, Mn 1.3%, Cr 0.2%, Al 2.5%, Ce 0.03%, and the balance of Cu and inevitable impurity elements. The raw materials are added to a melting furnace. In order to control the content of impurity elements, a three-high graphite crucible is selected, and the temperature is raised to 1300°C. After the above raw materials are completely melted, they are stirred evenly, covered with charcoal, and an inert gas is passed through the melting furnace for protection. Then, the obtained liquid alloy is placed in a mold for cooling by non-vacuum casting to cast the required ingot.

[0110] In step (2), the outer skin of the ingot in step (1) is turned off by 2 mm and then homogenized in a box-type resistance furnace. The homogenization temperature is 900° C. and the time is 8 hours.

[0111] In step (3), the extrusion barrel and the die are first preheated to a temperature of 700° C., and then the sample homogenized in step (2) is taken out and quickly sent to an extruder for extrusion, with an extrusion deformation of 90%. The extruded copper rod blank is water-cooled in water.

[0112] In step (4), the copper rod blank prepared in step (3) is cold drawn, and the total deformation is 50%.

[0113] In step (5), the copper rod in step (4) is annealed at a temperature of 700° C. for a holding time of 120 min and a cooling method of furnace cooling to obtain a nano-precipitation-strengthened high-strength and high-corrosion-resistant copper alloy sample.

[0114] Figure 4 This is a statistical diagram of special grain boundaries and grain sizes of the nano-precipitation strengthened high-strength and high-corrosion resistant copper alloy sample prepared in Example 4. Figure 4 (a) and (b) are the percentage diagrams of special grain boundaries. Figure 4The grain size distribution diagrams of the copper alloys in (c) and (d) show that the average grain size of the nano-precipitation strengthened high-strength and high-corrosion resistant copper alloy sample prepared in Example 4 is 70.6 μm, and the percentage of special grain boundaries (low ΣCSL) is 31%.

[0115] The nano-precipitation-strengthened high-strength and high-corrosion-resistant copper alloy sample obtained in Example 4 was subjected to performance tests, including room temperature tensile properties, room temperature yield strength properties, elongation after fracture, uniform corrosion rate of static seawater immersion under room temperature conditions, and uniform corrosion rate under clean artificial seawater (chemical composition as shown in Table 1) flushing conditions with a flow rate of 3m / s at room temperature. Its performance is shown in Table 5. In Table 5: room temperature tensile strength, room temperature yield strength and elongation after fracture were tested in accordance with GB / T228.1-2010 "Metallic Material Tensile Test Part 1: Room Temperature Test Method". The uniform corrosion rate of static seawater immersion under room temperature conditions was tested in accordance with GB / T 6384-2008 "Seawater Corrosion Test Method for Metal Materials for Ships and Marine Engineering in Natural Environments". Determination of uniform corrosion rate under clean artificial seawater (chemical composition as shown in Table 1) flushing conditions with a flow rate of 3m / s at room temperature The copper alloy sample was flushed with clean artificial seawater with the chemical composition shown in Table 1 at a speed of 3m / s. The traditional B10 alloy in Table 5 is a commercially available product.

[0116] Table 5 Performance test results of nano-precipitation strengthened high-strength and high-corrosion-resistant copper alloy samples prepared in Example 4

[0117]

[0118] Comparative Example 1

[0119] This comparative example provides a method for preparing a novel corrosion-resistant white copper alloy that is resistant to high-velocity seawater erosion, comprising the following steps: (1) casting, (2) homogenization, (3) hot extrusion, (4) cold drawing, and (5) annealing.

[0120] In step (1), electrolytic copper, electrolytic nickel, pure manganese, pure aluminum, Cu-20Fe master alloy, Cu-20Cr master alloy, and Cu-20Ce master alloy are used as raw materials, and the composition and mass percentage (wt%) of each element are: Ni 7%, Fe 1%, Mn 1%, Cr 0.1%, Ce 0.03%, and the balance of Cu and unavoidable impurity elements. The raw materials are added to a melting furnace. In order to control the content of impurity elements, a three-high graphite crucible is selected, and the temperature is raised to 1300°C. After the above raw materials are completely melted, they are stirred evenly, covered with charcoal, and an inert gas is passed through the melting furnace for protection. After that, the obtained liquid alloy is placed in a mold for cooling by non-vacuum casting to cast the required ingot.

[0121] In step (2), the outer skin of the ingot in step (1) is turned off by 2 mm and then homogenized in a box-type resistance furnace. The homogenization temperature is 900° C. and the time is 4 hours.

[0122] In step (3), the extrusion barrel and the die are first preheated to a temperature of 650° C., and then the sample homogenized in step (2) is taken out and quickly sent to an extruder for extrusion, with an extrusion deformation of 90%. The extruded copper rod blank is water-cooled in water.

[0123] In step (4), the copper rod blank prepared in step (3) is cold drawn, and the total deformation is 50%.

[0124] In step (5), the copper rod in step (4) is subjected to a finished product annealing treatment, the annealing temperature is 700° C., the holding time is 60 min, and the cooling method is water cooling to obtain a copper alloy sample.

[0125] Figure 5 The special grain boundary and grain size statistics of the copper alloy sample prepared in Comparative Example 1. The results show that there is no second phase precipitation in the matrix of the copper alloy sample prepared in Comparative Example 1, the average grain size is 35μm, and the percentage of special grain boundaries (low ΣCSL) is 18.4%. Compared with the copper alloy samples prepared in Examples 1 to 4, there is no second phase precipitation, the grains are finer, the number of special grain boundaries is small, and the mechanical and corrosion resistance properties are significantly lower than those of the copper alloy samples prepared in Examples 1 to 4.

[0126] Comparative Example 2

[0127] This comparative example provides a method for preparing a novel corrosion-resistant white copper alloy that is resistant to high-velocity seawater erosion, comprising the following steps: (1) casting, (2) homogenization, (3) hot extrusion, (4) cold drawing, and (5) annealing.

[0128] In step (1), electrolytic copper, electrolytic nickel, pure manganese, pure aluminum, Cu-20Fe master alloy, Cu-20Cr master alloy, and Cu-20Ce master alloy are used as raw materials, and their composition and the mass percentage content (wt%) of each element are: Ni 11%, Fe 1.7%, Mn 1.5%, Cr 0.3%, Al 2%, Ce 0.02%, and the remaining amount of Cu and inevitable impurity elements. The raw materials are added to the melting furnace. In order to control the content of impurity elements, a three-high graphite crucible is selected, and the temperature is raised to 1200°C. After the above raw materials are completely melted, they are stirred evenly, covered with charcoal, and inert gas is passed through the melting furnace for protection. After that, the obtained liquid alloy is placed in a mold for cooling by non-vacuum casting to cast the required ingot.

[0129] In step (2), the outer skin of the ingot in step (1) is turned off by 3 mm and then homogenized in a box-type resistance furnace. The homogenization temperature is 950° C. and the time is 3 hours.

[0130] In step (3), the extrusion barrel and the die are first preheated to a temperature of 550° C., and then the sample homogenized in step (2) is taken out and quickly sent to an extruder for extrusion, with an extrusion deformation of 87%. The extruded copper rod blank is water-cooled in water.

[0131] In step (4), the copper rod blank prepared in step (3) is cold drawn, and the total deformation is 40%.

[0132] In step (5), the copper rod in step (4) is annealed at a temperature of 850° C., a holding time of 40 min, and an air cooling method.

[0133] The copper alloy samples obtained in Comparative Examples 1 and 2 were subjected to performance tests, including room temperature tensile properties, room temperature yield strength properties, elongation after fracture, uniform corrosion rate under static seawater immersion at room temperature, and uniform corrosion rate under clean artificial seawater (chemical composition as shown in Table 1) flushing conditions at room temperature with a flow rate of 3 m / s. The properties are shown in Table 6. In Table 6: room temperature tensile strength, room temperature yield strength and elongation after fracture were tested in accordance with GB / T228.1-2010 "Metallic Material Tensile Test Part 1: Room Temperature Test Method". The uniform corrosion rate under static seawater immersion at room temperature was tested in accordance with GB / T 6384-2008 "Seawater Corrosion Test Method for Metallic Materials for Ships and Marine Engineering in Natural Environments". Determination of uniform corrosion rate under clean artificial seawater (chemical composition as shown in Table 1) flushing conditions at a flow rate of 3 m / s at room temperature The copper alloy samples were flushed with clean artificial seawater with the chemical composition shown in Table 1 at a speed of 3 m / s. The traditional B10 alloy in Table 6 is a commercially available product.

[0134] Table 6 Performance test results of nano-precipitation strengthened high-strength and high-corrosion-resistant copper alloy samples prepared in Comparative Example 1

[0135]

[0136] It can be seen from the above embodiments that the nano-precipitation-strengthened high-strength and high-corrosion-resistant copper alloy provided by the present invention includes the following elements in percentage by mass: 8-16wt% Ni element, 1-2wt% of the sum of Fe element and Cr element, the ratio of the mass percentage of Fe element and Cr element ≥3:1, 1-2wt% Mn element, 1-3wt% Al element, 0.01-0.03wt% Ce element, and the balance of Cu element and inevitable impurity elements. The present invention adopts a method combining homogenization treatment → hot extrusion → cold deformation → annealing treatment, and the prepared copper alloy has good grain size uniformity, the average grain size can be controlled between 50-100μm, the number of special grain boundaries (low ΣCSL) is more than 30%, and a large number of high-density and dispersed nano-precipitation phases are precipitated inside the grains. Compared with traditional copper-nickel alloys, it has excellent mechanical and corrosion resistance matching. The results of the embodiment show that the nano-precipitation-strengthened high-strength and high-corrosion-resistant copper alloy provided by the present invention has a tensile strength of ≥400MPa, a yield strength of ≥200MPa, an elongation after fracture of ≥30%, a uniform corrosion rate of <0.015mm / a in static seawater immersion at room temperature, and a uniform corrosion rate of ≤0.035mm / a in clean artificial seawater (wherein the chemical composition of clean artificial seawater is shown in Table 1) at a flow rate of 3m / s at room temperature. The nano-precipitation-strengthened high-strength and high-corrosion-resistant copper alloy prepared by the present invention can be widely used in cooling water pipelines of main and auxiliary engines of ships, fire water pipelines of offshore oil production platforms, heat exchangers of coastal power plants, and brine heaters of multi-stage flash evaporation devices for seawater desalination, etc., providing a theoretical basis for the optimized design of high-strength and high-corrosion-resistant copper-nickel alloys for marine engineering and ships and their service reliability in marine environments.

[0137] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.

Claims

1. A nano-precipitation strengthened high-strength and high-corrosion resistant copper alloy, comprising the following elements in percentage by weight: 11-16wt% of Ni, 1-2wt% of the sum of Fe and Cr, a mass ratio of Fe to Cr of ≥3:1, 1-1.7% of Fe, 0.2-0.4wt% of Cr, 1.3-2wt% of Mn, 2-3wt% of Al, 0.02-0.03wt% of Ce, and the balance of Cu; The nano-precipitation strengthened high-strength and high-corrosion-resistant copper alloy comprises a matrix and a second phase dispersedly distributed inside the matrix; the second phase comprises Cr 2 Ni phase and / or Cr 2 Fe phase, the second phase is nanoscale; the average grain size of the nano-precipitation strengthened high-strength and high-corrosion resistant copper alloy is 50~100μm; the percentage of low ΣCSL grain boundaries in the nano-precipitation strengthened high-strength and high-corrosion resistant copper alloy is 31~53%; the average grain size of the second phase is 10~50nm.

2. The method for preparing the nano-precipitation strengthened high-strength and high-corrosion resistant copper alloy according to claim 1, It is characterized in that The following steps are involved: The raw materials for preparing the nano-precipitation-strengthened high-strength and high-corrosion-resistant copper alloy are melted, and the obtained melt is cast to obtain an ingot; The ingot is heated and homogenized to obtain a homogenized copper alloy billet; The homogenized copper alloy billet is subjected to hot extrusion treatment and then water-cooled to obtain a first deformed copper alloy billet; cold drawing the first deformed copper alloy billet to obtain a second deformed copper alloy billet; The second deformed copper alloy billet is annealed to obtain the nano-precipitation strengthened high-strength and high-corrosion resistant copper alloy.

3. The preparation method according to claim 2, It is characterized in that The raw materials for preparing the nano-precipitation strengthened high-strength and high-corrosion-resistant copper alloy include: copper element, nickel element, manganese element, aluminum element, copper-iron master alloy, copper-chromium master alloy and copper-cerium master alloy; the mass percentage of iron element in the copper-iron master alloy is 10-20wt%; the mass percentage of chromium element in the copper-chromium master alloy is 10-20wt%; the mass percentage of cerium element in the copper-cerium master alloy is 10-20wt%.

4. The preparation method according to claim 2 or 3, It is characterized in that The smelting temperature is 1150-1400°C.

5. The preparation method according to claim 2, It is characterized in that The temperature of the homogenization treatment is 900-1000° C., and the insulation time is 2-8 hours.

6. The preparation method according to claim 2, It is characterized in that The extrusion deformation amount of the hot extrusion treatment is 40-90%, the initial temperature of the homogenized copper alloy billet during the hot extrusion treatment is 900-1000°C, and the temperature of the extrusion barrel and the die used in the hot extrusion treatment is 400-700°C.

7. The preparation method according to claim 2, It is characterized in that The deformation amount of the cold drawing process is 50-99%.

8. The preparation method according to claim 2, It is characterized in that The annealing treatment temperature is 700-850° C., the heat preservation time is 0.5-2 hours, and the cooling method is furnace cooling.

9. Application of the nano-precipitation strengthened high-strength and high-corrosion-resistant copper alloy according to claim 1 or the nano-precipitation strengthened high-strength and high-corrosion-resistant copper alloy prepared by the preparation method according to any one of claims 2 to 8 in marine engineering and marine seawater cooling systems.

Citation Information

Patent Citations

  • New multi-element high-strength high-corrosion-resistance copper alloy and preparation method thereof

    CN110592424A

  • Copper alloy material and preparation method thereof

    CN114134364A

  • Corrosion-resistant cupronickel alloy containing high-proportion special grain boundary and preparation method of corrosion-resistant cupronickel alloy

    CN116676505A

  • Improvements in or relating to copper-base alloys

    GB761110A

  • HIGH YOUNG Cu-Ni-Al-BASED COPPER ALLOY SHEET, METHOD FOR PRODUCING THE SAME, AND CONDUCTIVE SPRING MEMBER

    JP2020079436A