A high-temperature oxidation-resistant high-entropy alloy material and preparation method thereof

By using aluminum liquid wrapping method and vacuum arc melting technology in AlCrFeCoNi high-entropy alloy, optimizing the element ratio and melting conditions, the problem of insufficient anti-oxidation performance at high temperatures is solved, and the anti-oxidation performance and stability of the alloy are significantly improved.

CN118516580BActive Publication Date: 2024-10-01XIANGTAN UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411002412.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-10-01
Estimated Expiration
2044-07-25

AI Technical Summary

Technical Problem

The AlCrFeCoNi high-entropy alloy has insufficient resistance to oxidation and hot corrosion at high temperatures, especially when the aluminum content reaches 20at.%, it still does not reach the ideal state.

Method used

Using the aluminum liquid wrapping method as a pretreatment method, the Al raw materials and Si raw materials are uniformly stirred at 670~700°C to form an Al-Si alloy, and then pre-smelting and formal smelting are performed in a vacuum arc melting furnace to control the element ratio and smelting conditions. To form high temperature oxidation resistant high entropy alloy.

Benefits of technology

The addition of Si significantly improves the high-temperature oxidation resistance of the alloy, forms a dense oxide film, improves the overall performance of the alloy, and achieves excellent stability and durability at high temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118516580B_ABST
    Figure CN118516580B_ABST
Patent Text Reader

Abstract

The present invention discloses a high-temperature oxidation-resistant high-entropy alloy material and a preparation method thereof, belonging to the technical field of high-entropy alloy preparation. The present invention reduces the oxidation rate of the alloy to 6.2×10 ‑9 mg 2 / cm 4 / s, allowing the material to reach a complete oxidation resistance level and exhibit excellent oxidation resistance. The preparation method of the high entropy alloy material proposes a new smelting pretreatment method-aluminum liquid encapsulation method, which allows Si elements to better combine with Al and Fe elements to form a new phase, thereby improving the high-temperature oxidation resistance of the high entropy alloy. And it makes the raw materials less likely to explode during the smelting process, and the smelting is more uniform. The method is simple to operate, easy to control, cost-effective, and suitable for industrial-scale mass production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of high entropy alloy preparation, and specifically relates to a high-temperature oxidation-resistant high entropy alloy material and a preparation method thereof. Background Art

[0002] AlCrFeCoNi high entropy alloy is an alloy system with wide application potential. At room temperature, the alloy exhibits high strength and good ductility. In addition, in the medium and high temperature range of 700 ℃ to 850 ℃, AlCrFeCoNi high entropy alloys show excellent resistance to high temperature oxidation and hot corrosion. Compared with traditional nickel-based high temperature alloys, this high entropy alloy contains a higher content of antioxidant and corrosion-resistant elements such as aluminum (Al) and chromium (Cr). Therefore, AlCrFeCoNi high entropy alloys are considered to be a strong competitor for the new generation of high temperature metal structural materials, suitable for high temperature environments such as aerospace and nuclear industries.

[0003] At high temperatures, high entropy alloys react mainly through selective oxidation of elements. For example, aluminum in AlCrFeCoNi high entropy alloys is preferentially oxidized under high temperature conditions to form a highly resistant Al2O3 film, thereby protecting the metal matrix. Studies have shown that the oxidation behavior of alloys depends largely on their chemical composition, especially the aluminum content. For example, Butler et al.'s research pointed out that Al x During the oxidation process, CoCrFeNi high entropy alloys first undergo a transient oxidation stage, and then exhibit parabolic growth laws to varying degrees. With the increase of aluminum content, the oxidation resistance of the alloy is significantly improved. However, even when the aluminum content reaches 20at.%, the oxidation resistance of AlCoCrFeNi high entropy alloys has not reached the ideal state. Further studies have shown that silicon (Si) elements can change the growth mechanism of the oxide film and significantly improve its oxidation resistance and hot corrosion resistance. Therefore, Si plays an important role in improving the high-temperature oxidation performance of AlCoCrFeNi high entropy alloys. Adding Si can not only improve the density and stability of the oxide film, but also significantly enhance the overall performance of the alloy in high-temperature environments. In summary, AlCrFeCoNi-based high entropy alloys containing trace silicon can significantly improve their oxidation resistance under high-temperature conditions by optimizing the chemical composition, especially the Al and Si contents, providing a more reliable material choice for high-temperature applications. Summary of the invention

[0004] In view of the above-mentioned prior art, the present invention provides a high-temperature oxidation-resistant high-entropy alloy material and a preparation method thereof, which solves the problem of insufficient oxidation resistance and heat corrosion resistance.

[0005] In order to achieve the above object, the technical solution adopted by the present invention is: to provide a method for preparing a high-temperature oxidation-resistant high-entropy alloy material, comprising the following steps:

[0006] S1: pre-treating the raw material to remove the oxide layer;

[0007] S2: melting Al raw material into aluminum melt at 670-700 °C, keeping the temperature for 15-20 min, adding Si raw material and stirring evenly during the heat preservation process, cooling the aluminum melt mixed with Si raw material to room temperature after the heat preservation, and obtaining Al-Si alloy block;

[0008] S3: In the order of melting points of the alloy raw materials from low to high, Al-Si alloy block, Cr raw material, Fe raw material, Co raw material and Ni raw material are placed into a water-cooled copper mold of a vacuum arc melting furnace, and an indicator element is placed in the center of the mold, and the mold is evacuated and then filled with high-purity argon gas to a slightly positive pressure state;

[0009] S4: Pre-melt in a vacuum arc melting furnace, and when the indicator element has no obvious color change, formally melt the raw material; melt the raw material to a molten state, repeatedly melt it 5 times until it is uniform, stop the furnace and cool for 10-15 minutes, and then obtain a high-temperature oxidation-resistant high-entropy alloy material;

[0010] The added amounts of the above-mentioned Al raw materials, Cr raw materials, Fe raw materials, Co raw materials, Ni raw materials and Si raw materials are based on the atomic ratio of each element in the obtained high-temperature oxidation-resistant high-entropy alloy material, which is Al 19.5%~20%, Cr 19.5%~20%, Fe 19.5%~20%, Co 19.5%~20%, Ni 19.5%~20%, and Si 0.8%~2.4%.

[0011] The beneficial effects of the present invention are as follows: the present invention uses a novel smelting pretreatment method, namely, an aluminum liquid encapsulation method, that is, before the re-smelting operation, Si particles are encapsulated with molten Al liquid to form an Al-Si alloy before a conventional smelting operation is performed, thereby avoiding the occurrence of raw material explosion during the smelting process, reducing the loss of raw materials during the smelting operation, making the composition of the smelted high-entropy alloy material more uniform and more in line with the designed composition ratio, so that the Si element is better combined with the Al and Fe elements to form a new phase, thereby improving the high-temperature oxidation resistance of the high-entropy alloy.

[0012] Based on the above technical solution, the present invention can also be improved as follows.

[0013] Furthermore, the Al raw material, the Cr raw material, the Fe raw material, the Co raw material, the Ni raw material and the Si raw material are particles with a purity greater than 99.9% and a particle size of 1 to 3 mm.

[0014] The beneficial effect of adopting the further technical solution is that the smelting effect is closely related to the size of the raw material particles. Particles that are too large or too small will affect the uniformity of the smelted sample. Particles that are too large may lead to insufficient material contact and reduce the uniformity of the alloy; while particles that are too small may increase the loss of raw materials and cause the composition of the sample after smelting to deviate from the designed ratio.

[0015] Furthermore, the pretreatment for removing the oxide layer is to grind the surface of the raw material with sandpaper or a grinder, then put the raw material into anhydrous ethanol in turn and clean it with ultrasonic wave for 300 s, and finally dry it at 80 °C.

[0016] Furthermore, the molar ratio of each element in the high temperature oxidation resistant high entropy alloy material is: Al:Cr:Fe:Co:Ni=1:1:1:1:1.

[0017] Further, S3 was evacuated to 5×10 -3 Pa.

[0018] Furthermore, the indicator element is Ti, and the vacuum arc pre-melting process is to control the arc distance to 1-3 mm from the Ti surface, control the current to 60 A, and maintain it for 60 s.

[0019] Furthermore, the vacuum arc melting process is as follows: the current gradually increases from 60 A to 120 A, the speed is 5-8 A / s, each melting time is 5 min, and the raw materials are turned over after the alloy is cooled.

[0020] Furthermore, S4 cooling is performed by circulating water cooling with a flow rate of 20 cm / s.

[0021] The beneficial effect of adopting the further technical solution is that the smelting quality and production efficiency of the alloy can be effectively improved, while ensuring that the physical and chemical properties of the final product meet high-standard application requirements.

[0022] The invention also discloses a high-temperature oxidation-resistant high-entropy alloy material prepared by adopting the preparation method of the high-temperature oxidation-resistant high-entropy alloy material.

[0023] The beneficial effects of the present invention are as follows: the alloy material of the present invention is not only low in cost and high in performance, but also can be used at high temperatures, significantly improving its anti-oxidation ability. The addition of Si causes lattice distortion, which helps to relax the lattice distortion energy, thereby promoting the formation of the BCC phase. The XRD spectrum of this type of high entropy alloy is analyzed, and it is found that the XRD of the alloy without Si addition only shows the BCC diffraction peak, indicating that the single-phase BCC crystal structure is mainly formed in the alloy, while in the alloy containing Si, a superlattice (100) related to the ordered BCC appears B2 Diffraction peaks indicate the existence of phase separation in the alloy. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1XRD diagrams of high temperature oxidation resistant high entropy alloy materials prepared in Examples 1 to 3 and Comparative Example 1;

[0025] Figure 2 The scanning electron microscope images of the high temperature oxidation resistant high entropy alloy materials prepared in Examples 1 to 3 and Comparative Example 1;

[0026] Figure 3 The oxidation kinetic curves of the high temperature oxidation resistant high entropy alloy materials prepared in Examples 1 to 3 and Comparative Example 1;

[0027] Figure 4 XRD diagrams of high temperature oxidation resistant high entropy alloy materials obtained in Examples 1 to 3 and Comparative Example 1 after oxidation at 900°C for 96 h;

[0028] Figure 5 The oxidation surface diagram of the high temperature oxidation resistant high entropy alloy material obtained in Examples 1 to 3 and Comparative Example 1 after oxidation at 900°C for 96 h;

[0029] Figure 6 This is an EDS image of the oxide layer cross section of the high temperature oxidation resistant high entropy alloy material obtained in Comparative Example 1 after oxidation at 900°C for 96 h;

[0030] Figure 7 This is an EDS image of the oxide layer cross section of the high temperature oxidation resistant high entropy alloy material obtained in Example 1 after oxidation at 900°C for 96 h;

[0031] Figure 8 This is an EDS image of the oxide layer cross section of the high temperature oxidation resistant high entropy alloy material obtained in Example 2 after oxidation at 900°C for 96 h;

[0032] Fig. 9 This is an EDS image of the oxide layer cross section of the high-temperature oxidation-resistant high-entropy alloy material prepared in Example 3 after being oxidized at 900°C for 96 h. DETAILED DESCRIPTION

[0033] The specific implementation modes of the present invention are described in detail below with reference to the embodiments.

[0034] Example 1

[0035] A high-temperature, oxidation-resistant high-entropy alloy material, wherein the atomic ratio of each element is 19.84%: 19.84%: 19.84%: 19.84%: 19.84%: 0.8%. Converted into a mass ratio, Al: Cr: Fe: Co: Ni: Si (by mass ratio) is 10.6%: 20.5%: 22.1%: 23.3%: 23.1%: 0.4%.

[0036] In this embodiment, the high temperature oxidation resistant high entropy alloy material is prepared by the following steps:

[0037] S1: Grind the surface of the raw material with sandpaper to remove the oxide film on the surface of the raw material; weigh the polished raw material particles Al 1.0642g, Cr 2.0495g, Fe 2.2072g, Co 2.3253g, Ni 2.3096g, Si0.0441g, based on the total smelting amount of 10 g, and then put the weighed different particles into anhydrous ethanol in turn and clean them with ultrasonic waves for 300 s, and then put them into a vacuum drying oven and set the drying temperature to 80 °C to dry them;

[0038] S2: Al particles are melted into aluminum melt at 680°C, and the mixture is kept warm for 15 min. Si particles are added during the heat preservation process and stirred evenly. After the heat preservation, the aluminum melt mixed with Si particles is cooled to room temperature to obtain an Al-Si alloy block.

[0039] S3: In the order of the melting points of the alloy raw materials from low to high, put the Al-Si alloy block, Cr particles, Fe particles, Co particles, and Ni particles into the water-cooled copper mold of the vacuum arc melting furnace, and put the Ti particles in the center of the mold. After turning on the circulating water cooling system of the vacuum arc furnace, first start the mechanical pump to draw a low vacuum, then start the molecular pump to draw a high vacuum, then introduce high-purity argon gas to make the air pressure display number above 0, repeat the above-mentioned gas washing operation once, remove other impurity gases in the vacuum arc furnace, and ensure the effect of sample melting, and then introduce high-purity argon gas to make the air pressure 0.03 pa;

[0040] S4: Initiate an arc through the tungsten electrode, and adjust the arc so that it is 2 mm above the surface of the Ti particles. During the first smelting, the current is controlled to be 60 A and maintained for 60 s. When the Ti particles do not change color significantly, continue smelting; move the tungsten electrode to 2 mm above the metal raw material to be smelted, increase the current from 0 A to 100 A at a current increase rate of 6 A / s for smelting, and smelt for 3 minutes each time. After the alloy is cooled (circulating water flow rate 20 cm / s water cooling), turn it over, repeat the above smelting operation, count the front smelting and reverse smelting as one smelting operation, repeat the smelting 5 times, stop the furnace for cooling (circulating water flow rate 20 cm / s water cooling) for 10 minutes, open the vent valve, and open the smelting furnace when the air pressure in the arc melting furnace is consistent with the normal pressure, and then the high-temperature oxidation-resistant high-entropy alloy material AlCrFeCoNiSi is obtained. 0.04 .

[0041] Example 2

[0042] A high-temperature, oxidation-resistant high-entropy alloy material, wherein the atomic ratio of each element is 19.68%: 19.68%: 19.68%: 19.68%: 19.68%: 19.68%: 1.6%. Converted into a mass ratio, Al: Cr: Fe: Co: Ni: Si (by mass ratio) is 10.6%: 20.4%: 22.0%: 23.2%: 23.0%: 0.8%.

[0043] In this embodiment, the high temperature oxidation resistant high entropy alloy material is prepared by the following steps:

[0044] S1: Grind the surface of the raw material with sandpaper to remove the oxide film on the surface of the raw material; weigh the polished raw material particles Al 1.0595g, Cr 2.0405g, Fe 2.1975g, Co 2.3152g, Ni 2.2995g, Si0.0878g, based on the total smelting amount of 10 g, and then put the weighed different particles into anhydrous ethanol in turn and clean them with ultrasonic waves for 300 s, and then put them into a vacuum drying oven and set the drying temperature to 80 °C to dry them;

[0045] S2: Al particles are melted into aluminum melt at 670°C, and the mixture is kept warm for 20 min. Si particles are added during the heat preservation process and stirred evenly. After the heat preservation, the aluminum melt mixed with Si particles is cooled to room temperature to obtain an Al-Si alloy block.

[0046] S3: In the order of the melting points of the alloy raw materials from low to high, put the Al-Si alloy block, Cr particles, Fe particles, Co particles, and Ni particles into the water-cooled copper mold of the vacuum arc melting furnace, and put the Ti particles in the center of the mold. After turning on the circulating water cooling system of the vacuum arc furnace, first start the mechanical pump to draw a low vacuum, then start the molecular pump to draw a high vacuum, then introduce high-purity argon gas to make the air pressure display number above 0, repeat the above-mentioned gas washing operation once, remove other impurity gases in the vacuum arc furnace, and ensure the effect of sample melting, and then introduce high-purity argon gas to make the air pressure 0.01 pa;

[0047] S4: Initiate an arc through the tungsten electrode, and adjust the arc so that it is 1 mm above the surface of the Ti particles. During the first smelting, the current is controlled to be 60 A and maintained for 60 s. When the Ti particles do not change color significantly, continue smelting; move the tungsten electrode to 2 mm above the metal raw material to be smelted, increase the current from 0 A to 90 A at a current increase rate of 5 A / s for smelting, and smelt for 4 minutes each time. After the alloy is cooled (circulating water flow rate 20 cm / s water cooling), turn it over, repeat the above smelting operation, count the front smelting and reverse smelting as one smelting operation, repeat the smelting 5 times, stop the furnace for cooling (circulating water flow rate 20 cm / s water cooling) for 15 minutes, open the vent valve, and open the smelting furnace when the air pressure in the arc melting furnace is consistent with the normal pressure, and then the high-temperature oxidation-resistant high-entropy alloy material AlCrFeCoNiSi is obtained. 0.08 .

[0048] Example 3

[0049] A high-temperature, oxidation-resistant high-entropy alloy material, wherein the atomic ratio of each element is 19.52%: 19.52%: 19.52%: 19.52%: 19.52%: 2.4%. Converted into a mass ratio, Al: Cr: Fe: Co: Ni: Si (by mass ratio) is 10.5%: 20.3%: 21.9%: 23.1%: 23.0%: 1.2%.

[0050] In this embodiment, the high temperature oxidation resistant high entropy alloy material is prepared by the following steps:

[0051] S1: Grind the surface of the raw material with sandpaper to remove the oxide film on the surface of the raw material; weigh the polished raw material particles Al 1.0549g, Cr 2.0316g, Fe 2.1875g, Co 2.3050g, Ni 2.2894g, Si0.1313g, based on the total smelting amount of 10g, and then put the weighed different particles into anhydrous ethanol in turn and clean them with ultrasonic waves for 300 seconds, and then put them into a vacuum drying oven and set the drying temperature to 80℃ to dry them;

[0052] S2: melting Al particles into aluminum melt at 700°C, keeping the temperature for 18 min, adding Si particles and stirring evenly during the heat preservation process, cooling the aluminum melt mixed with Si particles to room temperature after the heat preservation to obtain an Al-Si alloy block;

[0053] S3: In the order of melting point of alloy raw materials from low to high, put Al-Si alloy block, Cr particles, Fe particles, Co particles, Ni particles into the water-cooled copper mold of vacuum arc melting furnace, and put Ti particles in the center of the mold. After opening the circulating water cooling system of vacuum arc furnace, first start the mechanical pump to draw low vacuum, then start the molecular pump to draw high vacuum, then introduce high-purity argon gas to make the air pressure display number above 0, repeat the above-mentioned gas washing operation once, remove other impurity gases in vacuum arc furnace, ensure the effect of sample melting, and then introduce high-purity argon gas to make the air pressure 0.05 pa;

[0054] S4: Initiate an arc through the tungsten electrode, and adjust the arc so that it is 3 mm above the surface of the Ti particles. During the first smelting, the current is controlled to be 60 A and maintained for 60 s. When the Ti particles do not change color significantly, continue smelting; move the tungsten electrode to 3 mm above the metal raw material to be smelted, increase the current from 0 A to 120 A at a current increase rate of 5 A / s for smelting, and smelt for 5 minutes each time. After the alloy is cooled (circulating water flow rate 20 cm / s water cooling), turn it over, repeat the above smelting operation, count the front smelting and reverse smelting as one smelting operation, repeat the smelting 5 times, stop the furnace for cooling (circulating water flow rate 20 cm / s water cooling) for 12 minutes, open the vent valve, and open the smelting furnace when the air pressure in the arc melting furnace is consistent with the normal pressure, and then the high-temperature oxidation-resistant high-entropy alloy material AlCrFeCoNiSi is obtained. 0.12 .

[0055] Comparative Example 1

[0056] A high-temperature oxidation-resistant high-entropy alloy material, wherein the elements Al:Cr:Fe:Co:Ni (by atomic ratio) are 20%:20%:20%:20%:20%:20%, and converted into a mass ratio, Al:Cr:Fe:Co:Ni (by mass ratio) is 10.7%:20.6%:22.2%:23.3%:23.2%, without adding Si.

[0057] The high temperature oxidation resistant high entropy alloy material in this comparative example is prepared by the following steps:

[0058] S1: Grind the surface of the raw material with sandpaper to remove the oxide film on the surface of the raw material; weigh the polished raw material particles Al 1.0689g, Cr 2.0589g, Fe 2.2169g, Co 2.3357g, Ni 2.3198g, based on the total smelting amount of 10g, and then put the weighed different particles into anhydrous ethanol in turn and clean them with ultrasonic waves for 300 seconds, and then put them into a vacuum drying oven and set the drying temperature to 80℃ to dry them;

[0059] S2: Place Al particles, Cr particles, Fe particles, Co particles, and Ni particles into the water-cooled copper mold of the vacuum arc melting furnace in the order of the melting point of the alloy raw materials from low to high, and place Ti particles in the center of the mold. After turning on the circulating water cooling system of the vacuum arc furnace, first start the mechanical pump to draw a low vacuum, then start the molecular pump to draw a high vacuum, then introduce high-purity argon gas to make the air pressure display number above 0, repeat the above-mentioned gas washing operation once, remove other impurity gases in the vacuum arc furnace, and ensure the effect of sample melting, and then introduce high-purity argon gas to make the air pressure display number above 0 in a slightly positive pressure state;

[0060] S3: The arc is triggered by the tungsten electrode, and the arc is adjusted to be 2 mm above the surface of the Ti particles. During the first smelting, the current is controlled to be 60 A and maintained for 60 s. When the Ti particles do not change color significantly, the smelting is continued; the tungsten electrode is moved to 2 mm above the metal raw material to be smelted, and the current is increased from 0 A to 100 A at a current increase rate of 6A / s for smelting. Each smelting is 3 minutes. After the alloy is cooled (circulating water flow rate 20 cm / s water cooling), it is turned over and the above smelting operation is repeated. The front smelting and the reverse smelting are counted as one smelting operation. The smelting is repeated 5 times, and the furnace is stopped for cooling (circulating water flow rate 20 cm / s water cooling) for 10 minutes. The vent valve is opened. When the air pressure in the arc melting furnace is consistent with the normal pressure, the melting furnace can be opened to obtain the high-temperature oxidation-resistant high-entropy alloy material AlCrFeCoNi.

[0061] Comparative Example 2

[0062] The difference from the preparation conditions in Example 1 is that the aluminum liquid encapsulation pretreatment method is not used, part of the alloy material explodes during the smelting process, the smelted high entropy alloy sample does not conform to the designed composition, and the sample is not melted uniformly.

[0063] Comparative Example 3

[0064] The difference from the preparation conditions in Example 1 is that the circulating water flow rate of the circulating water cooling system of the vacuum arc furnace is adjusted to 40 cm / s. The results show that cracks appeared in the alloy sample obtained during the rapid cooling process, which indicates that too fast cooling rate may cause the internal stress of the material to increase, thereby causing cracks. In addition, the unevenness of the alloy composition also suggests that rapid cooling may affect the flow and uniform solidification of the alloy melt in the mold, further proving the importance of a suitable cooling rate for maintaining the alloy structure and properties.

[0065] Comparative Example 4

[0066] The difference from the preparation conditions in Example 1 is that the current growth rate during smelting was set at 15 A / s and increased to 150 A. This operation caused the alloy raw material to partially splash out from the water-cooled copper mold during the smelting process, resulting in material loss. This loss not only reduces the output of the final product, but also causes the actual atomic ratio to differ greatly from the designed composition, affecting the expected performance and quality of the alloy.

[0067] Experimental Example 1

[0068] High temperature oxidation resistance test: The high temperature oxidation resistant high entropy alloy materials obtained in Examples 1 to 3 and the comparative example were cut into 3 mm × 6 mm × 10 mm rectangular block samples using a wire cutting machine, and then the six surfaces were polished using 400 mesh, 800 mesh, 1200 mesh, and 2000 mesh SiC sandpapers, respectively, and then polished using a diamond polishing paste with a particle size of 1.5 mm. This step requires that the six surfaces of the sample be polished until there are no obvious scratches under a metallographic microscope at 50 times, and then the polished sample is placed in anhydrous ethanol for ultrasonic cleaning, and then dried with a hair dryer. The sample can be used for high temperature oxidation resistance testing.

[0069] Use a high-temperature box furnace to carry out high-temperature oxidation tests. Put the clean samples into a clean corundum crucible. Set the high-temperature box furnace to 900 °C, put the crucible containing the alloy samples into the box furnace, take out the samples at 0 h, 2 h, 4 h, 6 h, 12 h, 24 h, 36 h, 48 h, 60 h, 72 h, 84 h, and 96 h, respectively, weigh the samples after they cool to room temperature, and record the changes in the mass of the samples.

[0070] The XRD patterns of the high temperature oxidation resistant high entropy alloy materials prepared in Examples 1 to 3 and Comparative Example 1 are as follows: Figure 1 As shown, the high temperature oxidation resistant high entropy alloy materials obtained in Examples 1 to 3 and Comparative Example 1 both have disordered BCC (A2) phase and ordered BCC (B2) phase structure, but the high temperature oxidation resistant high entropy alloy materials obtained in Examples 1 to 3 have lattice distortion due to the addition of Si, which helps to relax the lattice distortion energy, thereby promoting the formation of the BCC phase. The high temperature oxidation resistant high entropy alloy material obtained in Comparative Example 1 only shows BCC diffraction peaks, indicating that a single-phase BCC crystal structure is mainly formed in the alloy. In the high temperature oxidation resistant high entropy alloy materials obtained in Examples 1 to 3, the superlattice (100) related to the ordered BCC appears. B2 Diffraction peaks indicate the existence of phase separation in the alloy.

[0071] The high temperature oxidation resistant high entropy alloy materials prepared in Examples 1 to 3 and Comparative Example 1 were scanned using a scanning electron microscope. The results are as follows: Figure 2As shown in the figure, scanning electron microscopy showed that there was no obvious dendrite segregation in the four samples, indicating that the smelting was very uniform.

[0072] The mass gain per unit area of ​​the high temperature oxidation resistant high entropy alloy materials prepared in Examples 1 to 3 and Comparative Example 1 after oxidation at 900 °C for 96 h was statistically analyzed. Figure 3 As shown, in Example 1, a high temperature oxidation resistant high entropy alloy material AlCrFeCoNiSi 0.04 The oxidation gain after 96 h was only 0.008873 mg cm -2 Through data fitting, the oxidation rate of the high entropy alloy is only 7.76×10 -4 mg cm -2 ·h -1 (i.e. 8.51×10 -9 (mg 2 / cm 4 / s)). According to the oxidation resistance rating standard for steel and alloys provided in GB / T13303-1991 as shown in Table 1, the high entropy alloy belongs to the complete oxidation resistance level and has excellent oxidation resistance. Example 2 Preparation of high temperature oxidation resistant high entropy alloy material AlCrFeCoNiSi 0.08 The weight gain after oxidation for 96 h was 0.01420 mg cm -2 , and its oxidation rate is 1.33×10 -3 mg cm -2 ·h -1 (i.e. 1.51×10 -8 (mg 2 / cm 4 / s), the high temperature oxidation resistance is better than that of Example 1. According to the oxidation resistance rating standard of steel and alloys provided by GB / T13303-1991 shown in Table 1, AlCrFeCoNiSi 0.08 The high entropy alloy material also belongs to the level of complete oxidation resistance and has excellent oxidation resistance. Example 3 Preparation of high temperature oxidation resistant high entropy alloy material AlCrFeCoNiSi 0.12 The weight gain after 96 h oxidation was 0.007199 mg cm -2 , and its oxidation rate is 6.05×10 -4 mg cm -2 ·h -1 (6.20×10 -9 (mg 2 / cm 4 / s), the high temperature oxidation resistance is better than that of Example 1. According to the oxidation resistance rating standard of steel and alloys provided by GB / T13303-1991 shown in Table 1, AlCrFeCoNiSi 0.12The high entropy alloy material also belongs to the level of complete oxidation resistance and has excellent oxidation resistance. Comparative Example 1 prepared a high temperature oxidation resistant high entropy alloy material AlCrFeCoNi with an oxidation weight gain of 0.01136 mg cm -2 , and its oxidation rate is 1.96×10 -3 mg cm -2 ·h -1 (6.86×10 -8 (mg 2 / cm 4 / s), the high temperature oxidation resistance is worse than that of other embodiments in which Si is added. According to the oxidation resistance rating standard for steel and alloys provided in GB / T13303-1991 as shown in Table 1, the AlCrFeCoNi high entropy alloy material belongs to the oxidation resistance level and has excellent oxidation resistance. However, by adding a trace amount of Si, the oxidation resistance of the AlCrFeCoNi high entropy alloy material is improved by an order of magnitude, which shows that the addition of Si effectively improves the high temperature oxidation resistance of the alloy, achieves the effect of reducing the oxidation rate and extending the service life.

[0073] Table 1 Oxidation resistance rating standards for steel and alloys (from GB / T13303-1991)

[0074]

[0075] The oxidation kinetic curves of the high-temperature oxidation-resistant high-entropy alloy materials obtained in Examples 1 to 3 and Comparative Example 1 oxidized at 900°C for 96 hours satisfy the power law equation The oxidation mass gain data were fitted, and the obtained 96h oxidation kinetic curve approximately satisfied the parabolic law of oxidation. The fitted n value and K value are shown in Table 2.

[0076] Table 2 The overall n value and K value of the high temperature oxidation resistant high entropy alloy materials obtained in Examples 1 to 3 and Comparative Example 1 at 900 °C

[0077]

[0078] The high temperature oxidation resistant high entropy alloy materials prepared in Examples 1 to 3 and Comparative Example 1 were tested by X-ray diffractometer after being oxidized at 900 °C for 96 h. The results are as follows: Figure 4As shown, the oxide layer of the high-temperature oxidation-resistant high-entropy alloy material obtained in Examples 1 to 3 after oxidation at 900°C consists of five types of oxides: Al2O3, SiO2, Fe2O3, CoCr2O4, and NiFe2O4. These oxides form a dense oxide film on the surface of the substrate, which makes the high-temperature oxidation-resistant high-entropy alloy material have excellent oxidation resistance. The oxide layer of the high-temperature oxidation-resistant high-entropy alloy material obtained in Comparative Example 1 after oxidation at 900°C consists of only four types of oxides: Al2O3, Fe2O3, CoCr2O4, and NiFe2O4.

[0079] The surfaces of the high temperature oxidation resistant high entropy alloy materials obtained in Examples 1 to 3 and Comparative Example 1 after oxidation at 900 °C for 96 h were observed using an electron microscope. The results are as follows: Figure 5 As shown, the high temperature oxidation resistant high entropy alloy materials prepared in Examples 1 to 3 have a relatively smooth oxidized surface after oxidation, while the high temperature oxidation resistant high entropy alloy material prepared in Comparative Example 1 has a relatively loose oxidized surface after oxidation.

[0080] The high temperature oxidation resistant high entropy alloy materials prepared in Examples 1 to 3 and Comparative Example 1 were subjected to elemental analysis using an energy spectrum diffractometer after being oxidized at 900 °C for 96 h. The results are as follows: Figures 6 to 9 As shown, according to the EDS analysis of the oxide layer cross section, the high temperature oxidation resistant high entropy alloy material AlCrFeCoNiSi prepared in Example 1 0.04 The oxide layer formed after oxidation is thick and dense, which effectively isolates the direct contact between oxygen and the substrate and has excellent anti-oxidation performance; The high-temperature anti-oxidation high-entropy alloy material AlCrFeCoNiSi prepared in Example 2 0.08 The oxide layer formed after oxidation is thicker than that in Example 1 and is also continuous and dense, effectively isolating the direct contact between oxygen and the substrate, and also has excellent anti-oxidation performance; the high-temperature anti-oxidation high-entropy alloy material AlCrFeCoNiSi prepared in Example 2 0.12 The oxide layer formed after oxidation is thicker and continuous and denser than that in Example 2, which effectively isolates the direct contact between oxygen and the substrate. Compared with Examples 1 and 2, the high-temperature oxidation-resistant high-entropy alloy material AlCrFeCoNiSi 0.12 It has the most excellent anti-oxidation performance; and from the EDS image of the oxide layer cross section of the high-temperature oxidation-resistant high-entropy alloy material AlCrFeCoNi oxidized for 96 h obtained in Comparative Example 1, it can be seen that the oxide layer formed by the alloy material is dispersed and discontinuous.

[0081] In summary, the present invention optimizes the alloy composition by adding a trace amount of silicon to the AlCrFeCoNi-based alloy. This addition significantly improves the material's antioxidant properties and reaches a complete antioxidant level. This performance improvement enables the alloy to exhibit excellent stability and durability under extreme high temperature conditions, further confirming the key role of silicon in improving high-temperature antioxidant properties. Through this innovative alloy design and preparation method, the present invention not only achieves excellent adaptability to high-temperature environments, but also provides an efficient and economical material solution for high-temperature application fields such as aviation and energy.

[0082] Although the specific implementation of the present invention is described in detail in conjunction with the embodiments, it should not be understood as limiting the scope of protection of this patent. Within the scope described in the claims, various modifications and variations that can be made by those skilled in the art without creative work still fall within the scope of protection of this patent.

Claims

1. A method for preparing a high temperature oxidation resistant high entropy alloy material, characterized in that: The following steps are involved: S1: pre-treating the raw material to remove the oxide layer; S2: melting Al raw material into aluminum melt at 670-700 °C, keeping the temperature for 15-20 min, adding Si raw material and stirring evenly during the heat preservation process, cooling the aluminum melt mixed with Si raw material to room temperature after the heat preservation, and obtaining Al-Si alloy block; S3: Place Al-Si alloy block, Cr raw material, Fe raw material, Co raw material and Ni raw material into a water-cooled copper mold of a vacuum arc melting furnace in the order of the melting points of the alloy raw materials from low to high, place an indicator element in the center of the mold, evacuate the mold and then fill it with high-purity argon gas to a state of 0.01-0.05 Pa; S4: Pre-melt in a vacuum arc melting furnace, and when the indicator element has no obvious color change, formally melt the raw material; melt the raw material to a molten state, repeatedly melt it 5 times until it is uniform, stop the furnace and cool for 10-15 minutes, and then obtain a high-temperature oxidation-resistant high-entropy alloy material; The indicator element is Ti, and the vacuum arc pre-melting process is to control the arc distance to 1-3 mm from the Ti surface, control the current to 60 A, and maintain it for 60 s; The vacuum arc formal melting process is that the current gradually increases from 0 A to 90-120 A, the speed is 5-8 A / s, each melting time is 3-5 min, and the raw materials are turned over after the alloy is cooled; the cooling is water cooling using circulating water with a flow rate of 20 cm / s; The above-mentioned Al raw material, Cr raw material, Fe raw material, Co raw material, Ni raw material and Si raw material are particles with a purity greater than 99.9% and a particle size of 1~3mm. The amount of raw material added is based on the atomic ratio of each element of the obtained high-temperature oxidation-resistant high-entropy alloy material, which is Al 19.5%~20%, Cr 19.5%~20%, Fe 19.5%~20%, Co 19.5%~20%, Ni 19.5%~20%, and Si 0.8%~2.4%.

2. The method for preparing a high temperature oxidation resistant high entropy alloy material according to claim 1, characterized in that: The pretreatment for removing the oxide layer is to grind the raw material surface with sandpaper or a grinder, then put the raw materials into anhydrous ethanol and clean them with ultrasonic wave for 300 s, and finally dry them at 80 °C.

3. The method for preparing a high temperature oxidation resistant high entropy alloy material according to claim 1, characterized in that: The molar ratio of the elements in the high-temperature oxidation-resistant high-entropy alloy material is: Al:Cr:Fe:Co:Ni=1:1:1:1:

1.

4. The method for preparing a high temperature oxidation resistant high entropy alloy material according to claim 1, characterized in that: S3 was evacuated to 5 × 10 -3 Pa.

5. A high temperature oxidation resistant high entropy alloy material, characterized in that: The high temperature oxidation resistant high entropy alloy material is prepared by the preparation method of any one of claims 1 to 4.

Citation Information

Patent Citations

  • Multi-element high-entropy alloy film and preparation method thereof

    CN103898463A

  • Ultra-fine grained eutectic high-entropy alloy and preparation method thereof

    CN109750209A

  • High- strength and heat-resisting high entropy alloy matrix composites and method of manufacturing the same

    KR1020170124441A

  • High entropy alloy-based compositions and bond coats formed therefrom

    US20230323516A1

  • KR20230037076A