Binder and pole piece, electrochemical device and electronic device containing the same
By using a binder composed of salt-coated polymer and polymer salt, the problem of poor ion transmission performance of traditional binders in power batteries is solved, achieving both high discharge capacity and cycle performance, and is suitable for use in high-pressure environments. Power battery.
Patent Information
- Application Number
- CN202411009446.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-07-26
AI Technical Summary
Traditional PVDF binders have poor ion transport performance in power batteries and cannot balance high discharge capacity and cycle performance.
A binder composed of salt-encapsulated polymer and polymer salt is used. The mass percentage of the salt is not less than 50%, including lithium salt and sodium salt. It is combined with polymers such as polyvinylidene fluoride and hexafluoropropylene copolymer to form a homogeneous phase. system to improve bonding performance and ion transport capabilities.
It achieves excellent bonding performance and ion transport performance under high pressure, significantly improves the cycle stability and discharge capacity of power batteries, especially in solid-state lithium-ion batteries, which balances high energy density and cycle performance.
Smart Images

Figure SMS_4 
Figure SMS_5
Abstract
Description
Technical Field
[0001] The invention relates to an adhesive and a pole piece, an electrochemical device and an electronic device containing the adhesive. Background Art
[0002] Power batteries have the advantages of high operating voltage, light weight, small size, no memory effect, low self-discharge rate, long cycle life, and high energy density. They are currently widely used in mobile phones, laptops, tablets, electric vehicles, energy storage grids and other fields. Among them, common power batteries include lithium-ion batteries, sodium-ion batteries and potassium-ion batteries. In recent years, with the rapid development of electric vehicles, people have higher demands for battery energy density, safety, cost and environmental protection. High-voltage positive electrodes, as an important means to improve battery energy density, have become the current development trend of power batteries.
[0003] PVDF is generally used as a binder in the preparation process of power battery pole pieces. However, traditional PVDF has poor ion transport performance and limited adhesion. The power battery produced cannot ensure high discharge capacity while taking into account excellent cycle performance. Summary of the invention
[0004] In order to solve the above technical problems, the present invention provides a binder and a pole piece, an electrochemical device and an electronic device containing the binder. The binder has excellent bonding performance and ion transmission performance and is resistant to high voltage. The electrochemical device (especially a power battery) using the binder has excellent cycle stability and high discharge capacity.
[0005] To achieve the above objectives, the present invention adopts the following technical solutions.
[0006] In a first aspect, the present invention provides a binder, which includes a salt-encapsulated polymer; the salt-encapsulated polymer includes salt and polymer; the mass percentage of salt in the salt-encapsulated polymer is not less than 50%; the salt in the salt-encapsulated polymer is one or both of lithium salt and sodium salt; the binder also includes polymer salt, and the polymer salt is one or both of polymer lithium salt and polymer sodium salt; the mass ratio of the polymer salt to the salt-encapsulated polymer is 1:(0.2-50).
[0007] In a second aspect, the present invention provides a pole piece, which includes an active material layer, and the active material layer includes the binder as described above.
[0008] In a third aspect, the present invention provides an electrochemical device comprising the electrode sheet as described above.
[0009] In a fourth aspect, the present invention provides an electronic device comprising the electrochemical device as described above.
[0010] The positive and progressive effects of the present invention are:
[0011] The invention provides a binder comprising a salt-encapsulated polymer and a polymer salt. The binder can ensure excellent bonding performance while taking into account excellent ion transmission performance and high pressure resistance.
[0012] The power battery using the binder has excellent cycle performance and high discharge capacity. Especially in solid-state lithium-ion batteries, even if a certain amount of electrolyte is not added to the active material layer of the positive electrode or the negative electrode, the use of the binder can still take into account both excellent capacity and cycle performance. Furthermore, when applied to solid-state lithium-ion batteries using high-voltage positive electrodes such as lithium nickel manganese oxide positive electrodes, it can operate at a higher operating voltage, giving full play to the advantages of lithium nickel manganese oxide's high discharge capacity while significantly improving its cycle performance. DETAILED DESCRIPTION
[0013] The present invention is further described below by way of examples, but the present invention is not limited to the scope of the examples. The experimental methods in the following examples without specifying specific conditions are carried out according to conventional methods and conditions, or selected according to the product specifications.
[0014] Binder
[0015] In the binder provided in the first aspect of the present invention, it includes a salt-encapsulated polymer; the salt-encapsulated polymer includes salt and polymer; the mass percentage of salt in the salt-encapsulated polymer is not less than 50%; the salt in the salt-encapsulated polymer is one or both of lithium salt and sodium salt; the binder also includes a polymer salt, and the polymer salt is one or both of polymer lithium salt and polymer sodium salt; the mass ratio of the polymer salt to the salt-encapsulated polymer is 1:(0.2-50).
[0016] In the present invention, the salt-in-polymer refers to a homogeneous system formed by the dissolution of polymer and salt, wherein the mass of the salt accounts for more than 50% of the total mass of the entire system. When the mass percentage of the salt is less than 50%, it is difficult to form a homogeneous system. The full English name of the salt-in-polymer is: polymer-in-salt, referred to as PIS. Among them, the salt in the salt-in-polymer can be a lithium salt or a sodium salt conventionally used in the art. Generally speaking, the lithium salt or sodium salt conventionally used in the art can be soluble in the polymer to form a homogeneous system, that is, to obtain a salt-in-polymer, thereby further improving the ion transmission capacity of the binder on the basis of ensuring the bonding performance of the binder. Therefore, as long as it is a lithium salt or sodium salt conventionally used in the art, it can be used as the salt in the salt-in-polymer, and the specific type is not further limited.
[0017] In some preferred embodiments, the mass percentage of salt in the salt-in-polymer is 50%-90%, for example, 75%.
[0018] In an optional embodiment, the salt in the salt-in-polymer is a lithium salt, and the lithium salt includes one or more of lithium chloride, lithium bis(trifluoromethylsulfonyl)imide and lithium bis(fluorosulfonyl)imide.
[0019] In an alternative embodiment, the salt in the salt-in-polymer is a sodium salt, and the sodium salt includes sodium chloride.
[0020] In some optional embodiments, the polymer in the salt-in-polymer includes one or more of polyvinylidene fluoride (PVDF), polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-HFP), polyethylene oxide (PEO) and polyvinylene carbonate (PVCA).
[0021] In some specific embodiments, in the salt-in-polymer, the salt is lithium bis(trifluoromethylsulfonyl)imide, and the polymer is polyvinylidene fluoride-hexafluoropropylene copolymer.
[0022] In some specific embodiments, in the salt-in-polymer, the salt is lithium bis(trifluoromethylsulfonyl)imide and the polymer is polyvinylidene fluoride.
[0023] In some specific embodiments, in the salt-in-polymer, the salt is lithium bis(fluorosulfonyl)imide and the polymer is polyethylene oxide.
[0024] In some specific embodiments, in the polymer-in-salt, the salt is sodium chloride and the polymer is polyvinylidene fluoride-hexafluoropropylene copolymer.
[0025] Wherein, the polymer lithium salt optionally includes one or more of lithium polyacrylate, lithium carboxymethyl cellulose and lithium alginate.
[0026] Wherein, the polymer sodium salt optionally includes one or more of sodium polyacrylate, sodium carboxymethyl cellulose and sodium alginate.
[0027] In the present invention, the polymer salt refers to a polymer anion generated by the reaction of a polymer and a salt under certain conditions and connected to a metal cation through electrostatic interaction. For example, the polymer lithium salt refers to a polymer anion generated by the reaction of a polymer and a lithium-containing compound under certain conditions and connected to Li + The polymer connected by electrostatic interaction is also a lithium salt. For example, the polymer sodium salt refers to the polymer anion generated by the reaction of the polymer and the sodium-containing compound under certain conditions and Na + The polymers are linked by electrostatic interactions and are also a sodium salt.
[0028] In some preferred embodiments, the binder comprises a polymer-in-salt and a polymer salt, and the mass ratio of the polymer salt to the polymer-in-salt is, for example, 1:4 or 1:49.
[0029] In some specific embodiments, the binder includes lithium polyacrylate and salt-encapsulated polymer; in the salt-encapsulated polymer, the salt is lithium bis(trifluoromethylsulfonyl imide), the polymer is polyvinylidene fluoride-hexafluoropropylene copolymer, and the mass percentage of lithium bis(trifluoromethylsulfonyl imide) in the salt-encapsulated polymer is, for example, 75%; the mass ratio of the lithium polyacrylate to the salt-encapsulated polymer is, for example, 1:0.25, 1:0.5, 1:2, 1:4, 1:10, 1:20, 1:30, 1:40 or 1:49.
[0030] In a specific embodiment, the binder includes lithium polyacrylate and salt-encapsulated polymer; in the salt-encapsulated polymer, the salt is lithium bis(trifluoromethylsulfonyl imide), the polymer is polyvinylidene fluoride-hexafluoropropylene copolymer, and the mass percentage of lithium bis(trifluoromethylsulfonyl imide) in the salt-encapsulated polymer is 50%; the mass ratio of lithium polyacrylate to salt-encapsulated polymer is, for example, 1:4.
[0031] In a specific embodiment, the binder includes lithium polyacrylate and salt-encapsulated polymer; in the salt-encapsulated polymer, the salt is lithium bis(trifluoromethylsulfonyl imide), the polymer is polyvinylidene fluoride-hexafluoropropylene copolymer, and the mass percentage of lithium bis(trifluoromethylsulfonyl imide) in the salt-encapsulated polymer is 90%; the mass ratio of lithium polyacrylate to salt-encapsulated polymer is, for example, 1:4.
[0032] In some specific embodiments, the binder includes lithium polyacrylate and salt-encapsulated polymer; in the salt-encapsulated polymer, the salt is lithium bis(fluorosulfonyl)imide, the polymer is polyethylene oxide, and the mass percentage of lithium bis(fluorosulfonyl)imide in the salt-encapsulated polymer is, for example, 75%; the mass ratio of lithium polyacrylate to the salt-encapsulated polymer is, for example, 1:4.
[0033] In some specific embodiments, the binder includes lithium carboxymethyl cellulose and a salt-encapsulated polymer; in the salt-encapsulated polymer, the salt is lithium bis(trifluoromethylsulfonyl imide), the polymer is polyvinylidene fluoride-hexafluoropropylene copolymer, and the mass percentage of lithium bis(trifluoromethylsulfonyl imide in the salt-encapsulated polymer is, for example, 75%; the mass ratio of the lithium carboxymethyl cellulose to the salt-encapsulated polymer is, for example, 1:4.
[0034] In some specific embodiments, the binder includes lithium alginate and a salt-encapsulated polymer; in the salt-encapsulated polymer, the salt is lithium bis(trifluoromethylsulfonyl imide), the polymer is polyvinylidene fluoride-hexafluoropropylene copolymer, and the mass percentage of lithium bis(trifluoromethylsulfonyl imide) in the salt-encapsulated polymer is, for example, 75%; the mass ratio of the lithium alginate to the salt-encapsulated polymer is, for example, 1:4.
[0035] In some specific embodiments, the binder includes sodium polyacrylate and salt-encapsulated polymer; in the salt-encapsulated polymer, the salt is sodium chloride, the polymer is polyvinylidene fluoride-hexafluoropropylene copolymer, and the mass percentage of sodium chloride in the salt-encapsulated polymer is, for example, 75%; the mass ratio of the sodium polyacrylate to the salt-encapsulated polymer is, for example, 1:4.
[0036] In some specific embodiments, the binder includes lithium polyacrylate and salt-encapsulated polymer; in the salt-encapsulated polymer, the salt is lithium bis(trifluoromethylsulfonylimide), the polymer is polyvinylidene fluoride, and the mass percentage of lithium bis(trifluoromethylsulfonylimide) in the salt-encapsulated polymer is, for example, 75%; the mass ratio of the lithium polyacrylate to the salt-encapsulated polymer is, for example, 1:4.
[0037] Pole piece
[0038] In the pole piece provided in the second aspect of the present invention, it comprises an active material layer, and the active material layer comprises the binder as described above.
[0039] Positive electrode
[0040] In some embodiments, the electrode sheet is a positive electrode sheet, and the positive electrode sheet includes a positive electrode active material layer.
[0041] In an optional embodiment, the mass percentage of the positive electrode active material in the positive electrode active material layer is 60%-98%, for example, 84%.
[0042] In an optional embodiment, the mass percentage of the binder in the positive electrode active material layer is 10%-20%, for example, 15%.
[0043] In an optional embodiment, the positive electrode active material layer further includes a conductive agent, and the mass percentage of the conductive agent is optionally 1%-5%.
[0044] The type of the conductive agent is not particularly limited, and is a reagent used to ensure that the electrode has good charge and discharge performance. It can be selected from graphite materials such as natural graphite and artificial graphite, carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black and other carbon black materials, carbon fibers, metal fibers and other conductive fibers, metal powders such as carbon fluoride powder, aluminum powder, nickel powder and other metal powders, zinc oxide, potassium titanate and other conductive whiskers, and titanium dioxide and other conductive metal oxides or polyphenylene derivatives.
[0045] In a specific embodiment, the conductive agent is carbon black SP (Super P) and vapor grown carbon fiber (VGCF).
[0046] In the present invention, the positive electrode current collector in the positive electrode sheet may be a conventional positive electrode current collector in the art. The positive electrode current collector is a substrate supporting the positive electrode active material layer, usually a metal foil with a thickness of 3-500 microns. There is no particular restriction on the material, as long as it has high conductivity and does not produce chemical reactions in the power battery system. For example, it can be a foil formed after surface treatment of nickel, titanium, aluminum, nickel, silver, stainless steel, carbon, etc. The positive electrode current collector usually has a smooth surface, but fine lines may also be formed on its surface to increase the adhesion between the positive electrode active material and the current collector. In addition to the foil, the positive electrode current collector may also be used in any one or more combinations of various forms such as film, mesh, porous, foam or non-woven fabric. Generally, the positive electrode current collector is aluminum foil.
[0047] In the present invention, the preparation method of the positive electrode sheet generally comprises: fully stirring and mixing the components of the positive electrode active material layer in a solvent to obtain a positive electrode slurry, coating it on at least one surface of the positive electrode collector, drying it, and rolling and compacting it.
[0048] In some embodiments, the positive electrode sheet is a positive electrode sheet in a lithium-ion battery, and the positive electrode active material in the positive electrode active material layer can be a conventional positive electrode active material of a lithium-ion battery in the art, and can be a lithium-containing composite oxide. Specifically, LiMnO2, LiFeO2, LiMn2O4, Li2FeSiO4, LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2, LiNi5CO2Mn3O2, Li z Ni (1-x-y) Co x M y O2 (wherein 0.01≤x≤0.20, 0≤y≤0.20, 0.97≤z≤1.20, M represents at least one element selected from Mn, V, Mg, Mo, Nb and Al), LiFePO4 and Li z CO (1-x) M x O2 (wherein 0≤x≤0.1, 0.97≤z≤1.20, and M represents at least one element selected from the group consisting of Mn, Ni, V, Mg, Mo, Nb and Al).
[0049] In some optional embodiments, the positive electrode active material in the positive electrode active material layer is one or more of lithium nickel cobalt manganese oxide, lithium nickel manganese oxide, lithium iron phosphate, lithium manganese iron phosphate and lithium cobalt oxide.
[0050] In a preferred embodiment, the positive electrode active material in the positive electrode active material layer is lithium nickel manganese oxide, such as LiNi 0.5 Mn 1.5 O4.
[0051] Lithium nickel manganese oxide (LNMO) is a high-voltage positive electrode active material with a voltage platform of about 4.7 V and a specific energy of more than 600 Wh / kg. Since the lithium nickel manganese oxide material is mainly composed of nickel and manganese elements and does not contain cobalt, it is more environmentally friendly and has a relatively low cost. When lithium nickel manganese oxide is used as the positive electrode active material, the battery generally has a higher energy density, but its cycle stability is poor. By matching the binder of the present invention, especially in a solid-state electrode, while ensuring a higher energy density, excellent cycle stability can also be taken into account.
[0052] In a preferred embodiment, the positive electrode active material in the positive electrode active material layer is lithium nickel cobalt manganese oxide, such as LiNi 0.8 Co 0.1 Mn 0.1 O2.
[0053] In other embodiments, the positive electrode sheet is a positive electrode sheet in a sodium ion battery, the positive electrode active material in the positive electrode active material layer may be a conventional positive electrode active material of a sodium ion battery in the art, and the positive electrode active material may be a sodium ion-containing active material, such as a layered oxide, a polyanionic compound or a Prussian blue compound.
[0054] Optionally, the general formula of the layered oxide is Na x [MFeMn]O2, M is selected from at least one of Cu, Ni, Li, Mg, Al, Zn, Ti, Zr and Sn, and x≤1.
[0055] Optionally, the general formula of the polyanionic compound is Na x M y (X a O b ) z Z w , wherein M is selected from one or more of Ti, V, Cr, Mn, Fe, Co, Ni, Ca, Mg, Al and Nb; X is selected from one or more of Si, S, P, As, B, Mo, W and Ge, and Z is selected from F and / or OH.
[0056] Optionally, the general formula of the Prussian blue compound is Na x M[M'(CN)6], wherein M is selected from one or more of Mn, Ni, Co, Zn, Cu and Fe, and M' is selected from one or more of Mn, Ni, Co, Zn, Cu and Fe; optionally, 0<x≤2.
[0057] In a specific embodiment, the positive electrode active material is Prussian blue Na2Fe[Fe(CN)6].
[0058] Negative plate
[0059] In some embodiments, the negative electrode sheet includes a negative electrode active material layer including a binder as described above.
[0060] In the present invention, the preparation method of the negative electrode sheet generally comprises the following steps: the components of the negative electrode active material layer are fully stirred and mixed in a solvent to obtain a negative electrode slurry which is applied on at least one surface of the negative electrode current collector, dried, cold pressed, and cut to obtain the negative electrode sheet.
[0061] In some embodiments, the negative electrode sheet is a negative electrode sheet in a lithium ion battery, and the negative electrode active material in the negative electrode active material layer may be a conventional negative electrode active material of a lithium ion battery in the art. The negative electrode active material of the lithium ion battery may use a compound that can reversibly embed and deintercalate lithium. Specific examples include but are not limited to: carbon materials such as crystalline carbon (natural graphite and artificial graphite, etc.), amorphous carbon, carbon-coated graphite and resin-coated graphite, or oxide materials such as indium oxide, silicon oxide, tin oxide, lithium titanate, zinc oxide, and lithium oxide. These negative electrode active materials may be used alone or in combination of two or more. From the perspective of high energy density, carbon materials such as graphite may also be used in combination with Si, Si alloys, Si oxides and other Si-based materials.
[0062] In some embodiments, the negative electrode active material includes any one of soft carbon, hard carbon, artificial graphite, natural graphite, silicon, silicon oxides, silicon carbon compounds, or lithium titanate, or a combination of at least two thereof.
[0063] In the present invention, the negative electrode current collector in the negative electrode sheet may be a conventional negative electrode current collector in the art. The negative electrode current collector is a substrate supporting the negative electrode active material, usually a metal foil with a thickness of 3-500 microns. There is no particular restriction on the material, as long as it has high conductivity and does not produce chemical reactions in the power battery system. For example, it can be a foil formed after surface treatment of nickel, titanium, aluminum, nickel, silver, stainless steel, carbon, etc. The negative electrode current collector usually has a smooth surface, but fine lines may also be formed on its surface to increase the adhesion between the positive electrode active material and the current collector. In addition to the foil, the negative electrode current collector may also be used in any one or more combinations of various forms such as film, mesh, porous, foam or non-woven fabric. Generally, the negative electrode current collector is copper foil.
[0064] In other embodiments, the negative electrode sheet is a metal electrode, which may be lithium metal or a lithium-containing alloy; wherein the metal material in the lithium-containing alloy that can form an alloy with lithium is, for example, one or more of Cu, Sn, Si, Co, Mn, Fe, Sb and Ag.
[0065] Electrochemical Devices
[0066] The electrochemical device provided in the third aspect of the present invention comprises the pole piece as described above.
[0067] In an optional embodiment, the electrochemical device is a power battery.
[0068] In an optional embodiment, the power battery is a liquid battery, a solid battery or a semi-solid battery. The semi-solid battery has a solid electrolyte and a liquid electrolyte, and can also be a gel electrolyte.
[0069] In an optional embodiment, the power battery includes a lithium ion battery, a sodium ion battery or a potassium ion battery.
[0070] In a preferred embodiment, the lithium ion battery is a solid-state lithium ion battery.
[0071] In the present invention, the solid electrolyte in the solid-state lithium-ion battery may be a conventional solid electrolyte in the art.
[0072] In an optional embodiment, the solid electrolyte includes one or more of sulfide, halide and oxide inorganic electrolytes, such as Li6PS5Cl.
[0073] In a specific embodiment, the solid-state lithium-ion battery comprises a positive electrode sheet, a solid electrolyte layer and a negative electrode sheet stacked in sequence; the solid electrolyte layer comprises a solid electrolyte.
[0074] Electronic devices
[0075] The electronic device provided in the fourth aspect of the present invention comprises the electrochemical device as described above.
[0076] Exemplarily, the electronic device described in the present invention may be, but is not limited to, mobile devices (such as mobile phones, tablet computers, laptop computers, video recorders, portable printers / copiers, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems and backup power supplies, etc.
[0077] On the basis of being in accordance with the common sense in the art, the above-mentioned preferred conditions can be arbitrarily combined to obtain the preferred embodiments of the present invention. The present invention is further illustrated by way of examples below, but the present invention is not limited to the scope of the embodiments described. The experimental methods in the following examples that do not specify specific conditions are selected according to conventional methods and conditions, or according to the product specifications. Unless otherwise specified, the reagents and raw materials used in the present invention are commercially available.
[0078] The main reagents used in the following examples and comparative examples are as follows:
[0079] Polyacrylate lithium (PAALi) was purchased from Shenzhen Yanyi New Materials Co., Ltd., with the product model AONE;
[0080] Carboxymethyl cellulose lithium (CMCLi) was purchased from Green Energy Fiber (Chongqing) Technology Co., Ltd., product model RXCL230;
[0081] Lithium alginate was purchased from Taian Jiaye Biotechnology Co., Ltd.;
[0082] Lithium bis(trifluoromethylsulfonyl)imide (LiTFSI) was purchased from Aladdin Biochemical Technology Co., Ltd. under the trade name ;
[0083] Lithium bis(fluorosulfonyl)imide (LiFSI) was purchased from Aladdin Biochemical Technology Co., Ltd. under the trade name ;
[0084] Polyvinylidene fluoride (PVDF) was purchased from Arkema, with the product model Kynar® PVDF;
[0085] Polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-HFP) was purchased from Arkema, with the product model Kynar Flex® PVDF;
[0086] Polyethylene oxide (PEO) was purchased from Aladdin Biochemical Technology Co., Ltd., product model P101341;
[0087] Sodium polyacrylate (PAANa) was purchased from Dongfang Chemical Co., Ltd., with the product model PAAS;
[0088] Polyacrylic acid (PAA) was purchased from Aladdin, product model: .
[0089] Example 1
[0090] (1) Preparation of binder:
[0091] The PAALi and PIS (lithium salt is LiTFSI, polymer is PVDF-HFP, and the mass percentage of lithium salt is 75%) are evenly mixed to obtain a binder, wherein the mass ratio of PAALi to PIS is 1:4.
[0092] (2) Preparation of positive electrode:
[0093] The positive electrode active material is lithium nickel manganese oxide (LNMO, the specific molecular formula is LiNi 0.5 Mn 1.5O4), conductive agent (carbon black Super P and VGCF, mass ratio of 1:1) and the above-obtained binder are dispersed in N-methylpyrrolidone (NMP) in a mass ratio of 84:1:15 (a total of 100 parts by mass, and the mass percentage of the binder is 15%) to obtain a positive electrode slurry. The viscosity of the slurry is adjusted by adjusting the amount of NMP added so that the solid content of the positive electrode slurry is between 50% and 70%.
[0094] The slurry was coated on a 13 μm thick aluminum foil (which also included a 1 μm thick conductive carbon layer) by a doctor blade method. The coated positive electrode sheet was air-dried at 120°C for 2 h and then vacuum-dried for 24 h. It was then roller-compacted at a pressure of 80 MPa to obtain a positive electrode sheet (the thickness of the positive electrode active material layer was 100 μm).
[0095] Example 2
[0096] The only difference between this embodiment and embodiment 1 is that the mass percentage of the binder in the positive electrode active material layer is 10%, that is, the mass ratio of the positive electrode active material lithium nickel manganese oxide, the conductive agent and the binder obtained above is 89:1:10 (a total of 100 parts by mass), and the other conditions remain the same as in embodiment 1.
[0097] Example 3
[0098] The only difference between this embodiment and embodiment 1 is that the mass percentage of the binder in the positive electrode active material layer is 20%, that is, the mass ratio of the positive electrode active material lithium nickel manganese oxide, the conductive agent and the binder obtained above is 79:1:20 (a total of 100 parts by mass), and the other conditions remain the same as in embodiment 1.
[0099] Example 4
[0100] The difference between this embodiment and embodiment 1 is that the mass percentage of lithium salt in PIS is 50%, and the other conditions are the same as those in embodiment 1.
[0101] Example 5
[0102] The difference between this embodiment and embodiment 1 is that the mass percentage of lithium salt in PIS is 90%, and the other conditions are the same as those in embodiment 1.
[0103] Example 6
[0104] The difference between this embodiment and embodiment 1 is that the mass ratio of PAALi to PIS is 1:0.25, the total amount of binder remains unchanged, and the other conditions remain the same as in embodiment 1.
[0105] Example 7
[0106] The difference between this embodiment and embodiment 1 is that the mass ratio of PAALi to PIS is 1:0.5, the total amount of binder remains unchanged, and the other conditions remain the same as those in embodiment 1.
[0107] Example 8
[0108] The difference between this embodiment and embodiment 1 is that the mass ratio of PAALi to PIS is 1:2, the total amount of binder remains unchanged, and the other conditions remain the same as those in embodiment 1.
[0109] Example 9
[0110] The difference between this embodiment and embodiment 1 is that the mass ratio of PAALi to PIS is 1:10, the total amount of binder remains unchanged, and the other conditions remain the same as those in embodiment 1.
[0111] Example 10
[0112] The difference between this embodiment and embodiment 1 is that the mass ratio of PAALi to PIS is 1:20, the total amount of binder remains unchanged, and the other conditions remain the same as those in embodiment 1.
[0113] Embodiment 11
[0114] The difference between this embodiment and embodiment 1 is that the mass ratio of PAALi to PIS is 1:30, the total amount of binder remains unchanged, and the other conditions remain the same as those in embodiment 1.
[0115] Example 12
[0116] The difference between this embodiment and embodiment 1 is that the mass ratio of PAALi to PIS is 1:40, the total amount of binder remains unchanged, and the other conditions remain the same as those in embodiment 1.
[0117] Embodiment 13
[0118] The difference between this embodiment and embodiment 1 is that the mass ratio of PAALi to PIS is 1:49, the total amount of binder remains unchanged, and the other conditions remain the same as those in embodiment 1.
[0119] Embodiment 14
[0120] The only difference between this embodiment and embodiment 1 is that the lithium salt in PIS is LiTFSI, the polymer is PVDF, the mass percentage of the lithium salt is 75%, and the other conditions are the same as those in embodiment 1.
[0121] Embodiment 15
[0122] The only difference between this embodiment and embodiment 1 is that the lithium salt in PIS is LiFSI, the polymer is PEO, the mass percentage of the lithium salt is 75%, and the other conditions are the same as those in embodiment 1.
[0123] Example 16
[0124] The difference between this embodiment and embodiment 1 is that PAALi in the binder is replaced by CMCLi, and the other conditions are the same as those in embodiment 1.
[0125] Embodiment 17
[0126] The difference between this embodiment and embodiment 1 is that PAALi in the binder is replaced by lithium alginate, and the other conditions are the same as those in embodiment 1.
[0127] Embodiment 18
[0128] The difference between this embodiment and embodiment 1 is that the positive electrode active material is lithium nickel cobalt manganese oxide (NCM) (specific molecular formula is LiNi 0.8 Co 0.1 Mn 0.1 O2), and the other conditions remain the same as in Example 1.
[0129] Embodiment 19
[0130] (1) Preparation of binder:
[0131] The binder is obtained by uniformly mixing PAANa and PIS (the sodium salt is NaCl, the polymer is PVDF-HFP, and the mass percentage of the sodium salt is 75%), wherein the mass ratio of PAANa to PIS is 1:4.
[0132] (2) Preparation of positive electrode:
[0133] The positive electrode active material Prussian blue Na2Fe[Fe(CN)6], the conductive agent (carbon black Super P and VGCF, mass ratio of 1:1) and the binder obtained above were dispersed in N-methylpyrrolidone (NMP) at a mass ratio of 84:1:15 (a total of 100 parts by mass, the mass percentage of the binder is 15%) to obtain a positive electrode slurry. The slurry viscosity was adjusted by adjusting the amount of NMP added so that the solid content of the positive electrode slurry was between 50% and 70%.
[0134] The slurry was coated on a 13 μm thick aluminum foil (which also included a 1 μm thick conductive carbon layer) by a doctor blade method. The coated positive electrode sheet was air-dried at 120°C for 2 h and then vacuum-dried for 24 h. It was then roller-compacted at a pressure of 80 MPa to obtain a positive electrode sheet (the thickness of the positive electrode active material layer was 100 μm).
[0135] Comparative Example 1
[0136] The difference between this comparative example and Example 1 is that the binder is PVDF, the total amount of the binder remains unchanged, and the other conditions remain the same as those in Example 1.
[0137] Comparative Example 2
[0138] The difference between this comparative example and Example 1 is that the binder contains only PAALi, the total amount of the binder remains unchanged, and the other conditions remain the same as those in Example 1.
[0139] Comparative Example 3
[0140] The difference between this comparative example and Example 1 is that PVDF is used to replace PIS, and the other conditions are the same as those in Example 1.
[0141] Comparative Example 4
[0142] The difference between this comparative example and Example 1 is that the mass percentage of lithium salt in PIS is 40%, and the other conditions are the same as those in Example 1.
[0143] Comparative Example 5
[0144] The difference between this comparative example and Example 1 is that the binder is PVDF, the total amount of the binder remains unchanged, and when preparing the positive electrode sheet, the positive electrode slurry also includes an electrolyte Li6PS5Cl, wherein the mass ratio of the positive electrode active material lithium nickel manganese oxide, the conductive agent, the binder PVDF and the electrolyte is 64:1:15:20 (a total of 100 parts by mass, the mass percentage of the binder is 15%, and the mass percentage of the electrolyte is 20%).
[0145] Comparative Example 6
[0146] The difference between this comparative example and Example 1 is that PAALi in the binder is replaced by polyacrylic acid (PAA), and the other conditions are the same as those in Example 1.
[0147] Comparative Example 7
[0148] The difference between this comparative example and Example 1 is that PVDF is used to replace PAALi, and the other conditions are the same as those in Example 1.
[0149] Comparative Example 8
[0150] The difference between this comparative example and Example 1 is that the binder contains only PIS, the total amount of the binder remains unchanged, and the other conditions remain the same as those in Example 1.
[0151] Comparative Example 9
[0152] The only difference between this comparative example and Example 19 is that the binder contains only PAANa, the total amount of the binder remains unchanged, and the other conditions remain the same as Example 19.
[0153] Comparative Example 10
[0154] The only difference between this comparative example and Example 19 is that the binder contains only PIS, the total amount of the binder remains unchanged, and the other conditions remain the same as Example 19.
[0155] Effect test 1: Peeling force of positive electrode
[0156] Take the positive electrode sheets in Examples 1-19 and Comparative Examples 1-10, cut the positive electrode sheets with a die cutter to obtain positive electrode sheets with a length × width of 400mm × 20mm. Take a flat thin steel plate with a length of 200-300mm and a width of 40mm. First, stick a double-sided tape (length of 150mm, width of 20mm) on the center of the steel plate, smooth it with force, and ensure that the double-sided tape is tightly attached to the center of the steel plate. Peel off the double-sided tape to get the adhesive strip, and attach the above-mentioned positive electrode sheet to the adhesive strip to ensure that the positive electrode sheet and the adhesive strip are completely attached. Fix the steel plate on the lower fixture of the universal material testing machine and fix it vertically; insert the other positive electrode sheet that is not attached to the adhesive strip into the upper fixture and fix it so that the positive electrode sheet attached to the adhesive strip on the lower fixture is 180° with the positive electrode sheet fixed by the upper fixture. After fixing the test sample, set the test width to 20 mm, the peeling speed to 50-100 mm / min, and then start the test (universal material testing machine, Instron 5940) to obtain the peeling force.
[0157] Effect Test 2
[0158] A lithium ion battery is prepared using the positive electrode sheets prepared in Examples 1-18 and Comparative Examples 1-8. The preparation method of the lithium ion battery comprises the following steps:
[0159] A solid electrolyte layer (composed of Li6PS5Cl) is stacked on one side of the prepared positive electrode sheet, and the sheet is pressed at a pressure of 300MPa to press the positive electrode sheet and the solid electrolyte layer together. Subsequently, an indium sheet is stacked on the other side of the solid electrolyte layer as a negative electrode sheet, and an all-solid-state battery is obtained after sealing in a vacuum or inert atmosphere.
[0160] The lithium-ion battery prepared above was tested as follows:
[0161] (1) 0.3C discharge capacity at 80°C
[0162] At 25°C, the battery was first activated by charging and discharging at 0.1C for one cycle. Then the lithium-ion battery prepared as above was connected to a Blue Electric charge and discharge tester. It was charged and discharged for a long cycle at 80°C to measure its discharge capacity. The operating voltage range of the battery test was 3.4V (discharge cut-off voltage) ~ 4.5V (charge cut-off voltage), and the test rate was 0.3C.
[0163] (2) Number of cycles at 25°C (cycle capacity retention rate is 80%)
[0164] At 25°C, first charge and discharge the battery for one cycle at 0.1C to activate it. Connect the lithium-ion battery prepared above to a blue electric charge and discharge tester, and then cycle it for a long time at a rate of 0.3C until the ratio of the capacity of the nth cycle to the capacity of the first cycle at 0.3C is less than 80%. The capacity retention rate of the n-1th cycle is defined as 80%, the number of cycles is recorded as n-1, and the test is stopped.
[0165] Effect test 3
[0166] The positive electrode sheets prepared in Example 19 and Comparative Examples 9-10 were used to prepare sodium ion batteries. The preparation method of the sodium ion battery is as follows:
[0167] A solid electrolyte layer (the solid electrolyte layer is composed of Na6PS5Cl) is stacked on the surface of one side of the positive electrode sheet as described above, and the sheet is pressed at a pressure of 300MPa to press the positive electrode sheet and the solid electrolyte layer together. Subsequently, an indium sheet is stacked on the other side of the solid electrolyte layer as a negative electrode sheet, and an all-solid-state battery is obtained after sealing in a vacuum or inert atmosphere.
[0168] The sodium ion battery prepared above was tested as follows:
[0169] (1) 0.3C discharge capacity at 80°C
[0170] At 25°C, the battery was first activated by charging and discharging at 0.1C for one cycle. Then the sodium-ion battery prepared as above was connected to a Blue Electric charge and discharge tester. It was charged and discharged for a long cycle at 80°C to measure its discharge capacity. The operating voltage range of the battery test was 2V (discharge cut-off voltage) ~ 4V (charge cut-off voltage), and the test rate was 0.3C.
[0171] (2) Number of cycles at 25°C (cycle capacity retention rate is 80%)
[0172] At 25°C, first charge and discharge the battery at 0.1C for one cycle to activate it. Connect the sodium ion battery prepared above to the Blue Electric charge and discharge tester, and then cycle it for a long time at a rate of 0.3C until the ratio of the capacity of the nth cycle to the capacity of the first cycle at 0.3C is less than 80%. The capacity retention rate of the n-1th cycle is defined as 80%, the number of cycles is recorded as n-1, and the test is stopped.
[0173] Application Example 1
[0174] A mobile phone comprises a control device, an output device and a power source, wherein the control device is a chip, the output device is a screen, and the power source is a lithium ion battery prepared using the binder in Examples 1-18 or a sodium ion battery prepared using the binder in Example 19.
[0175] Application Example 2
[0176] A pure electric vehicle comprises an engine and a power source, wherein the power source is a lithium ion battery prepared using the binder in Examples 1-18 or a sodium ion battery prepared using the binder in Example 19.
[0177] Application Example 3
[0178] An electric train comprises an engine and a power source, wherein the power source is a lithium ion battery prepared using the binder in Examples 1-18 or a sodium ion battery prepared using the binder in Example 19.
[0179] The results of effect tests 1-3 are shown in Table 1.
[0180]
[0181]
[0182] Note: “ / ” in Table 1 means that the condition parameter is not involved in the specific experiment.
[0183] The binder of the present invention includes PIS and polymer salt, which has excellent bonding performance and ion transmission performance, and can withstand high pressure. Based on this, the binder can be used in lithium ion batteries or sodium ion batteries, and can take into account excellent cycle stability and high discharge capacity. Traditional binders have poor ion transmission performance and are not resistant to high pressure, and cannot match the requirements of electrodes, especially high-voltage positive electrodes using lithium nickel manganese oxide positive electrode materials, for high energy density and cycle stability.
[0184] Taking lithium-ion batteries as an example, the peeling force of the positive electrode sheet using the binder in Examples 1-18 can reach more than 100 N / m. On this basis, the lithium-ion battery including the electrode sheet and the solid electrolyte can have both excellent cycle stability and high discharge capacity. Specifically, the number of cycles at 25°C (cycle capacity retention rate of 80%) can reach more than 180 cycles, and the 0.3C discharge capacity at 80°C can reach more than 100 mAh / g.
[0185] When using traditional binders, a certain amount (generally not less than 20%) of solid electrolyte needs to be added to the active material layer of the positive electrode sheet and / or the negative electrode sheet to function normally. However, the solid-state lithium-ion batteries in the above embodiments of the present invention can still achieve good stability and excellent ion transmission performance in the positive electrode sheet without adding solid electrolyte, thereby ensuring that the battery has good cycle performance and fast charging performance. In the present invention, the mass percentage of the binder in the positive electrode active material layer is preferably 10%-20% (Examples 1-3), but the higher the binder content, the better the battery performance. In Example 3, the binder content is higher than that in Example 1, and the number of cycles is slightly increased, but the discharge capacity is slightly decreased.
[0186] When only conventional PVDF is used as a binder (Comparative Example 1), although the binder has good bonding properties, when used to prepare the tested lithium-ion battery, under the test conditions of the present invention, the battery can hardly work, and the discharge capacity and cycle number of the battery are both 0. This may be because the binder of the present invention can form a sufficiently effective ion conduction path and has good ion transport performance, while simply using PVDF as a binder in a solid-state lithium-ion battery cannot form a sufficiently effective ion conduction path.
[0187] In Comparative Example 2, the binder only uses polymer lithium salt (PAALi) without PIS. Although the binder has excellent bonding performance, the electrode sheet containing it has good peeling force, and the obtained battery has excellent cycle stability, its discharge capacity is greatly reduced. Similarly, when PAALi and PVDF (Comparative Example 3) are used as binders, it is impossible to ensure excellent cycle stability of lithium-ion batteries while taking into account excellent capacity.
[0188] The PIS of the present invention refers to a salt content of not less than 50%. In fact, PIS cannot be formed when the salt content is less than 50%. In Comparative Example 4, LiTFSI / PVDF-HFP is used, in which the salt content is 40%. Even if it is compounded with PAALi, it cannot achieve both cycle stability and discharge capacity. When the salt content in PIS is as high as 90% (Example 5), the discharge capacity is very high, and the cycle performance is reduced compared with Examples 1 and 4. This may be because the higher the salt content of PIS, the less contribution of PIS to the bonding performance.
[0189] The mass ratio of polymer lithium salt and PIS in the binder also has a certain influence on the performance of lithium-ion batteries, as shown in Examples 1 and 6-13, wherein the higher the PIS content, the lower the amount of PAALi used, the more effective ion conduction paths there are, but the adhesion is reduced, and the resulting lithium-ion battery has a higher capacity and a reduced cycle stability.
[0190] The types of polymer lithium salts and PIS in the binder have a certain influence on the peeling force of the obtained pole piece, the cycle stability and capacity of the lithium-ion battery. When the polymer lithium salt in the binder is the same, the lithium salt in the PIS is the same, and only the polymer in the PIS is different, such as the PIS in Example 14 uses LiTFSI / PVDF, compared with Example 1, the number of cycles and the discharge capacity are slightly reduced. When the polymer lithium salt in the binder is the same, the lithium salt and the polymer in the PIS are different, such as the PIS in Example 15 uses LiFSI / PEO, compared with Example 1, the number of cycles is significantly reduced, but the discharge capacity is increased. When the PIS in the binder is the same, but the polymer lithium salt is different, the performance of the battery is also different. Specifically, compared with the polymer lithium salt CMCLi (Example 16) and lithium alginate (Example 17), PAALi (Example 1) has a slightly higher adhesion to the current collector, the positive electrode sheet containing it has a larger peeling force, and the cycle performance of the obtained lithium-ion battery is more excellent.
[0191] Compared with Example 1, Comparative Examples 6-7 use PIS as a binder, and the first component uses non-salt polymer PAA or PVDF instead of polymer lithium salt. Its cycle stability and discharge capacity are significantly reduced, and it is impossible to take into account both excellent cycle stability and discharge capacity. In Comparative Example 8, PIS is used alone as a binder. Although its discharge capacity is improved, its cycle stability is greatly reduced, and it is impossible to take into account both excellent cycle stability and discharge capacity. From the above comparison, it can be seen that Example 1, based on Comparative Examples 6-8, uses a polymer lithium salt and PIS compound, which can greatly improve the discharge capacity without reducing the cycle stability (the number of cycles is more than 500).
[0192] The binder of the present invention is suitable for various positive electrode active materials of lithium ion batteries. In Example 21, the positive electrode active material is NCM, the number of cycles is as high as more than 1200 cycles, and the discharge capacity is as high as more than 200 mAh / g.
[0193] Similarly, when the binder of the present invention is used in sodium ion batteries, the above advantages can still be exerted. Compared with Example 19, in Comparative Example 10, the salt-encapsulated polymer NaCl / PVDF-HFP is used alone. Although the discharge capacity is improved, its cycle stability is reduced; in Comparative Example 9, PAANa is used alone as a binder. Although the cycle stability is improved, its discharge capacity is greatly reduced. From the above comparison, it can be seen that Example 19 uses a binder compounded with PAANa and NaCl / PVDF-HFP at the same time, which can greatly improve the discharge capacity while achieving almost no loss in cycle stability.
[0194] Although the specific embodiments of the present invention are described above, it should be understood by those skilled in the art that this is only for illustration and the protection scope of the present invention is defined by the appended claims. Those skilled in the art may make various changes or modifications to these embodiments without departing from the principles and essence of the present invention, but these changes and modifications all fall within the protection scope of the present invention.
Claims
1. A binder, It is characterized in that It includes a salt-encapsulated polymer, wherein the salt-encapsulated polymer refers to a homogeneous system formed by the dissolution of a polymer and a salt; the salt-encapsulated polymer includes a salt and a polymer; the mass percentage of the salt in the salt-encapsulated polymer is not less than 50%; the salt in the salt-encapsulated polymer is one or both of a lithium salt and a sodium salt; the polymer in the salt-encapsulated polymer includes one or more of polyvinylidene fluoride, a polyvinylidene fluoride-hexafluoropropylene copolymer, polyethylene oxide and polyvinylene carbonate; The binder further comprises a polymer salt, and the polymer salt is one or both of a polymer lithium salt and a polymer sodium salt; the mass ratio of the polymer salt to the salt-encapsulated polymer is 1:(0.2-50).
2. The adhesive according to claim 1, It is characterized in that The mass percentage of salt in the salt-in-polymer is 50%-90%.
3. The adhesive according to claim 1, It is characterized in that The binder satisfies one or more of the following conditions ad: a. The salt in the salt-in-polymer is a lithium salt, and the lithium salt includes one or more of lithium chloride, lithium bis(trifluoromethylsulfonyl)imide and lithium bis(fluorosulfonyl)imide; b. The salt in the salt-in-polymer is a sodium salt, and the sodium salt includes one or more of sodium chloride, sodium bis(trifluoromethylsulfonyl)imide and sodium bis(fluorosulfonyl)imide; c. The polymer salt is a polymer lithium salt, and the polymer lithium salt includes one or more of lithium polyacrylate, lithium carboxymethyl cellulose and lithium alginate; d. The polymer salt is a polymer sodium salt, and the polymer sodium salt includes one or more of sodium polyacrylate, sodium carboxymethyl cellulose and sodium alginate.
4. A pole piece comprising an active material layer, It is characterized in that The active material layer includes the binder according to any one of claims 1 to 3.
5. The pole piece according to claim 4, It is characterized in that The electrode sheet is a positive electrode sheet; the positive electrode sheet includes a positive electrode active material layer.
6. The pole piece according to claim 5, It is characterized in that The positive electrode active material in the positive electrode active material layer is one or more of lithium nickel cobalt manganese oxide, lithium nickel manganese oxide, lithium iron phosphate, lithium manganese iron phosphate and lithium cobalt oxide; Alternatively, the positive electrode active material in the positive electrode active material layer is a sodium ion-containing active material.
7. The pole piece according to claim 5, It is characterized in that The positive electrode active material layer satisfies one or more of the following conditions ac: a. The mass percentage of the positive electrode active material in the positive electrode active material layer is 60%-98%; b. The mass percentage of the binder in the positive electrode active material layer is 10%-20%; c. The positive electrode active material layer further includes a conductive agent, and the mass percentage of the conductive agent is 1%-5%.
8. An electrochemical device, It is characterized in that It comprises a pole piece as claimed in any one of claims 4 to 7.
9. The electrochemical device according to claim 8, It is characterized in that The electrochemical device is a power battery; The power battery includes a lithium ion battery, a sodium ion battery or a potassium ion battery; And / or, the power battery is a liquid battery, a solid-state battery or a semi-solid-state battery.
10. An electronic device, It is characterized in that It comprises the electrochemical device as claimed in claim 8 or 9.
Citation Information
Patent Citations
Solid polymer lithium ion battery positive electrode and preparation method and application thereof
CN111554895A
Binder composition, sodium ion battery positive electrode slurry and sodium ion battery