A method for recycling and reusing waste materials of dry sulfide electrolyte membrane

Through high-speed crushing and precision rolling processes, the edge waste of the sulfide electrolyte membrane is recycled into efficient and low-cost regenerated membranes, which solves the problems of sulfide electrolyte membrane waste and reduced film-forming performance, and achieves improvement in economic benefits and production cost reduction.

CN118539033BActive Publication Date: 2024-10-18SHANGHAI FIRM LITHIUM NEW ENERGY TECH CO LTD

Patent Information

Application Number
CN202410993605.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-10-18
Estimated Expiration
2044-07-24

AI Technical Summary

Technical Problem

During the production process of dry sulfide electrolyte membranes, the problem of edge trimming waste caused by edge cracking or uneven thickness results in a waste of sulfide electrolyte, and existing recycling methods are difficult to effectively improve film-forming performance.

Method used

Use a high-speed pulverizer to crush the waste into fine particles, and screen it through a screen to obtain regenerated powder. It is pre-pressed and precision rolled to prepare a regenerated sulfide electrolyte membrane to ensure the fibrillation and drawing plastic effect of the binder.

Benefits of technology

It effectively reduces the waste of sulfide electrolyte, improves the recycling rate, reduces the production cost of solid-state batteries, and ensures the improvement of film-forming performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention discloses a method for recycling and reusing waste materials of dry-process sulfide electrolyte membranes, comprising the following steps: S1, trimming the edges of sulfide electrolyte membranes to obtain waste materials; S2, high-speed crushing the waste materials obtained in S1 to obtain powder materials; S3, drying and screening the powder materials obtained in S2 to obtain regenerated powder materials; S4, pre-pressing and rolling the powder materials obtained in S3 to obtain regenerated sulfide electrolyte blank membranes; S5, heating and rolling the sulfide electrolyte blank membranes obtained in S4 by a precision roller press to obtain sulfide electrolyte membranes. The present invention also discloses a sulfide electrolyte membrane prepared by the above method. This method for recycling waste materials at the edges of sulfide membranes can bring huge economic benefits and reduce the production cost of solid-state batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of polymer materials, and in particular to a method for recycling and reusing dry-process sulfide electrolyte membrane waste. Background Art

[0002] In recent years, the emergence of dry electrode technology has opened up space for cost reduction and efficiency improvement in the battery industry, and has broad prospects for technical application. Compared with the traditional wet coating method, dry electrodes have unique advantages such as environmental friendliness, low cost, enhanced compatibility, high production efficiency, and improved electrode performance due to the use of solvent-free processes. Dry electrode technology has transformed from the traditional "powder-slurry-film" route to a simple "powder-film" route. It can not only significantly simplify the manufacturing process to reduce production costs, but also reconstruct the microstructure of the electrode and improve battery performance. It is also an iterative process route for future production technology in the battery industry.

[0003] Sulfide solid electrolytes are sensitive to polar solvents and easily react with organic liquids. Some highly polar solvents such as (NMP, DMF, ethanol, etc.) will even completely dissolve sulfide electrolytes. Some weaker organic solvents such as (tetrahydrofuran, acetonitrile, etc.) will form complexes with sulfide electrolytes. Subsequent heating treatments will make it difficult to completely remove these organic solvents, causing the ionic conductivity of sulfide electrolytes to decrease by one to two orders of magnitude. Because the "powder-film" process route of dry electrode technology is well suited for the preparation of sulfide electrolyte films.

[0004] In the production process of conventional dry-process sulfide electrolyte membranes, the dry calendering technology of "powder dry mixing-pre-pressing blanks-step-by-step precision rolling" is used to prepare fibrillated materials by mixing powders with binders, and then rolling them layer by layer through a multi-roll precision calender to obtain a sulfide electrolyte membrane with an ideal thickness. However, during the production process of this technology, due to the ductility of the material during the calendering process, problems such as cracking at the edges of the sulfide electrolyte membrane or thin thickness will occur, resulting in waste and waste of sulfide electrolytes. For this reason, there is an urgent need for a process route that can recycle these edge wastes and re-form them into powder and membrane for recycling. When recycling waste materials, because the materials have been fibrillated and formed, the film-forming effect will generally be reduced when they are recycled, or the performance will decrease after film formation. Wet recycling will cause the ionic conductivity of the sulfide electrolyte to decrease. Summary of the invention

[0005] The technical problem to be solved by the present invention is that the thickness and density of the edge of the dry-process sulfide electrolyte membrane are uneven, resulting in the problem of trimming waste, which solves the existing problem of recycling and reusing trimming waste and reduces the waste of sulfide electrolyte in the production process. The present invention provides a method for recycling and reusing waste of dry-process sulfide electrolyte membrane, wherein the edge thickness and density of the sulfide electrolyte membrane prepared by dry rolling are trimmed to obtain waste, and the waste is crushed by a high-speed crusher to obtain powder. The powder is screened by a sieve to remove large particle agglomerates to obtain recycled powder. The powder is pre-pressed and rolled to obtain a regenerated sulfide electrolyte blank membrane, and the sulfide electrolyte blank membrane is then passed through a precision roller press to obtain a sulfide electrolyte membrane. This method of recycling waste from the edge of the sulfide membrane can bring huge economic benefits and reduce the production cost of solid-state batteries. This process breaks the waste film into small particles by high-speed crushing at high speed and in a short time without damaging the fibrillated binder such as PTFE, FEP, etc. It can also ensure that the binder continues to have the fibrillated wire drawing plasticity effect in the subsequent re-calendering film process.

[0006] The objective of the present invention is achieved through the following technical solutions:

[0007] In a first aspect, the present invention provides a method for recycling and reusing dry sulfide electrolyte membrane waste, comprising the following steps:

[0008] S1. Trimming the cracked parts or uneven thickness parts on both sides of the sulfide electrolyte membrane to recover the waste;

[0009] S2, the waste material obtained in S1 is crushed by a high-speed crusher to obtain powder, the speed of the high-speed crusher is 10000-20000 rpm, and the time is 10s-60s;

[0010] S3, drying and screening the powder obtained in S2 to obtain recycled powder;

[0011] S4, pre-pressing and rolling the powder obtained in S3 to obtain a regenerated sulfide electrolyte film;

[0012] S5. The sulfide electrolyte blank film obtained in S4 is heated and rolled by a precision roller press to obtain a sulfide electrolyte membrane.

[0013] As an embodiment of the present invention, the sulfide electrolyte membrane waste in S1 is composed of a sulfide electrolyte and a binder, and the binder is one or more of PTFE (polytetrafluoroethylene), ETEF (ethylene-tetrafluoroethylene copolymer) or FEP (fluorinated ethylene propylene copolymer).

[0014] Specifically, the sulfide electrolyte is Li6PS5Cl.

[0015] As an embodiment of the present invention, in S2, the rotation speed of high-speed crushing is 10000-20000 rpm, the time is 10s-60s, and the number of repetitions is 3-7 times. At low speed, the powder cannot be well broken up, and subsequent film formation is prone to uneven film surface. When crushed at high speed for a long time, the material temperature will be relatively high, affecting the material properties. Therefore, by high-speed crushing, at high speed and short-time processing, without damaging the fibrillated binder such as PTFE, FEP, etc., the waste film is broken into fine particles again, so that in the subsequent re-calendering film forming process, the binder continues to have the effect of fibrillated wire drawing plasticity, thereby improving the film forming effect and film forming performance of recycling.

[0016] As an embodiment of the present invention, in S3, the drying conditions are: temperature 60-120° C., time 4-8 h.

[0017] As an embodiment of the present invention, in S3, ultrasonic vibration screen is used for screening, and the screening particle size is ≤50 μm.

[0018] As an embodiment of the present invention, in the S4, the pre-pressing pressure is 0.5-2T, and the thickness of the regenerated sulfide electrolyte blank film obtained by rolling is 500 μm-1 mm.

[0019] As an embodiment of the present invention, in S5, a precision roller press is used to perform multi-stage rolling, and the decreasing difference of the rolling thickness is between 5 and 30 μm.

[0020] As an embodiment of the present invention, in S5, the temperature of the heating roller pressing is 50-120°C.

[0021] As an embodiment of the present invention, in the step S5, the thickness of the prepared sulfide electrolyte membrane is 10-100 μm.

[0022] In a second aspect, the present invention provides a sulfide electrolyte membrane prepared by any of the above-mentioned methods for recycling and reusing dry sulfide electrolyte membrane waste.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] (1) The present invention prepares a regenerated sulfide electrolyte membrane by trimming the edge waste of the sulfide membrane, high-speed crushing, screening, pre-pressing the blank and then precision rolling, thereby reducing the waste of sulfide electrolyte and improving the recycling rate, which can bring huge economic benefits and reduce the production cost of solid-state batteries.

[0025] (2) The preparation process of the present invention is simple and can be combined with the existing production line with low transformation cost, and has good application prospects in the production of sulfide electrolyte membranes.

[0026] (3) Through high-speed crushing, at high speed and in a short time, the waste film is broken down into fine particles without damaging the fibrillating binder such as PTFE, FEP, etc., and it can also ensure that the binder continues to have the fibrillating wire drawing plasticity effect in the subsequent re-calendering film process.

[0027] (4) There is no need to separate the sulfide electrolyte and the binder, which can well ensure that the fibrillated material can still form a good film after being crushed and recycled. DETAILED DESCRIPTION

[0028] The present invention is described in detail below in conjunction with specific embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those of ordinary skill in the art, several variations and improvements may be made without departing from the concept of the present invention. These all belong to the protection scope of the present invention.

[0029] Example 1

[0030] A method for recycling and reusing dry sulfide electrolyte membrane waste comprises the following steps:

[0031] (1) Initial treatment of sulfide electrolyte membrane waste recycling: first, the cracked parts or uneven thickness parts on both sides of the sulfide electrolyte membrane are trimmed to obtain waste; the sulfide electrolyte membrane waste is composed of a sulfide electrolyte and a binder, the sulfide electrolyte is Li6PS5Cl, and the binder is PTFE (polytetrafluoroethylene).

[0032] (2) The waste material obtained in step (1) is crushed and dispersed by a high-speed crusher at a speed of 10,000 rpm for 30 seconds, and the operation is repeated 6 times to obtain a powder;

[0033] (3) The powder obtained in step (2) is placed in a vacuum oven at 60°C, dried for 6 hours, and then transferred to an ultrasonic vibration sieve with a mesh size of 300 mesh (aperture size of about 48 μm) for sieving to obtain a regenerated powder;

[0034] (4) pre-pressing and rolling the regenerated powder obtained in step (3) at a pre-pressing pressure of 1 T to obtain a regenerated sulfide electrolyte film with a thickness of 800 μm;

[0035] (5) The sulfide electrolyte membrane obtained in step (4) is passed through a precision roller press, with the heating roller temperature being 60° C. and multi-stage rolling, with the thickness decreasing by 30 μm at each stage, to finally obtain a sulfide electrolyte membrane with a thickness of 50 μm.

[0036] Example 2

[0037] A method for recycling and reusing dry sulfide electrolyte membrane waste comprises the following steps:

[0038] (1) Initial treatment of sulfide electrolyte membrane waste recycling: first, the cracked parts or uneven thickness parts on both sides of the sulfide electrolyte membrane are trimmed to obtain waste; the sulfide electrolyte membrane waste is composed of a sulfide electrolyte and a binder, the sulfide electrolyte is Li6PS5Cl, and the binder is ETEF (ethylene-tetrafluoroethylene copolymer).

[0039] (2) The waste material obtained in step (1) is crushed and dispersed by a high-speed crusher at a speed of 13,000 rpm for 45 seconds, and the operation is repeated three times to obtain a powder;

[0040] (3) placing the powder obtained in step (2) in a vacuum oven at 80°C, drying for 6 hours, and then transferring to an ultrasonic vibration sieve with a mesh size of 300 meshes (aperture size of about 48 μm), and sieving to obtain a regenerated powder;

[0041] (4) pre-pressing and rolling the regenerated powder obtained in step (3) at a pre-pressing pressure of 2T to obtain a regenerated sulfide electrolyte film with a thickness of 600 μm;

[0042] (5) The sulfide electrolyte membrane obtained in step (4) is passed through a precision roller press, with the heating roller temperature being 80° C. and multi-stage rolling, with the thickness decreasing by 25 μm at each stage, to finally obtain a sulfide electrolyte membrane with a thickness of 30 μm.

[0043] Example 3

[0044] A method for recycling and reusing dry sulfide electrolyte membrane waste comprises the following steps:

[0045] (1) Initial treatment of sulfide electrolyte membrane waste recycling: first, the cracked parts or uneven thickness parts on both sides of the sulfide electrolyte membrane are trimmed to obtain waste; the sulfide electrolyte membrane waste is composed of sulfide electrolyte and a binder, the sulfide electrolyte is Li6PS5Cl, and the binder is FEP (fluorinated ethylene propylene copolymer).

[0046] (2) The waste material obtained in step (1) is crushed and dispersed by a high-speed crusher at a speed of 15,000 rpm for 30 seconds, and the operation is repeated three times to obtain a powder;

[0047] (3) placing the powder obtained in step (2) in a vacuum oven at 100°C, drying for 6 hours, and then transferring to an ultrasonic vibration sieve with a mesh size of 300 (aperture size of about 48 μm) for sieving to obtain a regenerated powder;

[0048] (4) pre-pressing and rolling the regenerated powder obtained in step (3) at a pre-pressing pressure of 0.5 T to obtain a regenerated sulfide electrolyte film with a thickness of 1000 μm;

[0049] (5) The sulfide electrolyte membrane obtained in step (4) is passed through a precision roller press, with the heating roller temperature being 100° C. and multi-stage rolling, with the thickness decreasing by 20 μm at each stage, to finally obtain a sulfide electrolyte membrane with a thickness of 30 μm.

[0050] Example 4

[0051] A method for recycling and reusing dry sulfide electrolyte membrane waste comprises the following steps:

[0052] (1) Initial treatment of sulfide electrolyte membrane waste recycling: first, the cracked parts or uneven thickness parts on both sides of the sulfide electrolyte membrane are trimmed to obtain waste; the sulfide electrolyte membrane waste is composed of sulfide electrolyte and a binder, the sulfide electrolyte is Li6PS5Cl, and the binder is PTFE and FEP.

[0053] (2) The waste material obtained in step (1) is crushed and dispersed by a high-speed crusher at a speed of 18,000 rpm for 30 seconds, and the operation is repeated 6 times to obtain a powder;

[0054] (3) The powder obtained in step (2) is placed in a vacuum oven at 60°C, dried for 6 hours, and then transferred to an ultrasonic vibration sieve with a mesh size of 300 meshes (aperture size of about 48 μm) for sieving to obtain a regenerated powder;

[0055] (4) pre-pressing and rolling the regenerated powder obtained in step (3) at a pre-pressing pressure of 2T to obtain a regenerated sulfide electrolyte film with a thickness of 600 μm;

[0056] (5) The sulfide electrolyte membrane obtained in step (4) is passed through a precision roller press, with the heating roller temperature being 120° C. and multi-stage rolling, with the thickness decreasing by 10 μm at each stage, to finally obtain a sulfide electrolyte membrane with a thickness of 30 μm.

[0057] Comparative Example 1

[0058] This comparative example is the original sulfide electrolyte membrane after the edge waste is cut off.

[0059] Comparative Example 2

[0060] The speed of the pulverizer in step 2 is 5000 rpm, the time is 30 s, and the operation is repeated six times. The remaining steps are consistent with Experimental Example 1.

[0061] Comparative Example 3

[0062] In step 2, the pulverization method was changed to ball milling, the rotation speed was 400 rpm, and the ball milling time was 4 h. The remaining steps were consistent with those in Experimental Example 1.

[0063] Comparative Example 4

[0064] The speed of the pulverizer in step 2 is 12000 rpm, the time is 120 s, and the operation is repeated six times. The remaining steps are consistent with Experimental Example 1.

[0065] In order to evaluate the ionic conductivity of the regenerated sulfide electrolyte membrane, the electrolyte membrane was made into a sheet, placed in an all-solid-state battery mold, and matched with blocking electrodes at both ends for analysis using the AC impedance method.

[0066] The calculation formula is as follows:

[0067] σLi+=L / (RS)

[0068] Where σLi+——ionic conductivity of solid electrolyte (ms / cm)

[0069] L——Thickness of solid electrolyte (cm)

[0070] R——Intrinsic resistance of solid electrolyte (Ω)

[0071] S——Cross-sectional area of ​​solid electrolyte (cm 2 )

[0072] The results of testing the sulfide electrolyte membranes in Examples 1 to 4 and Comparative Examples 1 to 4 according to the above method are shown in Table 1.

[0073] Table 1 Test results of electrolyte membranes of various embodiments and comparative examples

[0074]

[0075] The above describes the specific embodiments of the present invention. It should be understood that the present invention is not limited to the above specific embodiments, and those skilled in the art may make various modifications or variations within the scope of the claims, which do not affect the essence of the present invention.

Claims

1. A method for recycling and reusing dry sulfide electrolyte membrane waste, characterized in that: The steps include: S1. Trimming the cracked parts or uneven thickness parts on both sides of the sulfide electrolyte membrane to recover the waste; S2, the waste material obtained in S1 is crushed by a high-speed crusher to obtain powder, the speed of the high-speed crusher is 10000-20000 rpm, the time is 10s-60s, and the number of repetitions is 3-7 times; S3, drying and screening the powder obtained in S2 to obtain recycled powder; S4, pre-pressing and rolling the powder obtained in S3 to obtain a regenerated sulfide electrolyte film; S5, heating and rolling the sulfide electrolyte blank film obtained in S4 by a precision roller press to obtain a sulfide electrolyte membrane; The drying conditions in S3 are: temperature 60-120° C., time 4-8 h; The sieving in S3 uses an ultrasonic vibrating screen, and the sieving particle size is ≤50 μm; The pre-pressing pressure in S4 is 0.5-2T, and the thickness of the regenerated sulfide electrolyte blank film obtained by rolling is 500 μm-1 mm; In the S5, a precision roller press is used for multi-stage rolling, and the decreasing difference of the rolling thickness is between 5 and 30 μm; The temperature of the heating roller in S5 is 50-120°C; The thickness of the sulfide electrolyte membrane prepared in S5 is 10-100 μm.

2. A sulfide electrolyte membrane, characterized in that: The dry sulfide electrolyte membrane waste material is prepared by the method for recycling and reusing the dry sulfide electrolyte membrane waste material as described in claim 1.

Citation Information

Patent Citations

  • Method for recycling leftover materials generated in preparation process of electrode membrane of solid-state battery

    CN118082047A

Cited By

  • Method for recycling sulfide electrolyte

    CN121460768A