A fast-charging lithium-ion battery and its preparation method and application
By adding specific additives and optimizing the electrolyte to the positive electrode of lithium iron phosphate batteries, the shortcomings of low temperature and fast charging performance of lithium iron phosphate batteries are solved, and efficient fast charging and stable cycle performance of the battery core are achieved.
Patent Information
- Application Number
- CN202410994165.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-07-24
AI Technical Summary
Lithium iron phosphate batteries have disadvantages in low temperature and fast charging performance, and traditional methods will sacrifice the cycle life and high temperature performance of the battery core when improving fast charging performance.
By adding cathode additives such as lithium ferrite and lithium oxalate to the positive electrode sheet of lithium-ion batteries, and using low-viscosity solvents and specific electrolyte additives, the conductive network of the electrode sheet and the ionic conductivity of the electrolyte are optimized to reduce the battery core's Ohmic impedance and negative interface impedance.
It significantly improves the fast charging performance and low-temperature performance of lithium iron phosphate batteries, while maintaining the cycle performance and high-temperature performance of the battery core, making it suitable for applications such as new energy vehicles.
Smart Images

Figure SMS_2
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a fast-charging lithium ion battery and a preparation method and application thereof. Background Art
[0002] Lithium-ion secondary batteries have the advantages of high energy density, long cycle life and high environmental friendliness. In recent years, with the increasing involution of the new energy vehicle market (such as the continuously increasing demand for driving range, fast charging, low cost, safety performance, etc.), the development of lithium-ion power batteries that take into account both energy density and fast charging performance requirements has become a powerful way to meet market demand and enhance corporate competitiveness and survival. Lithium iron phosphate batteries have gradually occupied a dominant position in the new energy vehicle battery market due to their good thermal stability and safety performance, moderate energy density and relatively low cost.
[0003] However, due to its poor kinetic properties, lithium iron phosphate materials have relatively poor low-temperature performance and fast-charging performance. In addition, lithium iron phosphate materials will damage the negative electrode SEI due to the problem of iron dissolution in the positive electrode. In order to ensure its cycle performance and high-temperature performance, the electrolyte used usually adds more negative electrode film-forming additives such as vinylene carbonate (the amount is usually more than twice that of ternary lithium batteries), which causes the negative electrode interface impedance of lithium iron phosphate batteries to be high, exacerbating the fast charging and low-temperature performance disadvantages of lithium iron phosphate batteries.
[0004] When improving fast charging performance, traditional methods need to increase the amount of low-impedance additives or reduce the total amount of negative electrode film-forming additives, but this also sacrifices the cycle life and high-temperature performance of the battery cell. To improve the fast charging performance of lithium iron phosphate while taking into account the cycle and high-temperature performance of the battery cell, we can start from optimizing the conductive electronic network of the electrode sheet, optimizing the pore tortuosity of the positive and negative electrode sheets, and improving the ionic conductivity of the electrolyte. At present, the ionic conductivity of the traditional carbonate solvent system has reached a bottleneck. Low-viscosity carboxylates (such as ethyl acetate, methyl propionate, methyl acetate, etc.) and nitrile solvents (such as acetonitrile, fluoroacetonitrile, propionitrile, etc.) can significantly improve the ionic conductivity of the electrolyte and reduce the ohmic impedance of the battery cell; however, these low-viscosity solvents are generally less compatible with the negative electrode than carbonates, and more negative electrode film-forming additives need to be added for protection, resulting in a further increase in the negative electrode interface impedance of the battery cell.
[0005] In view of this, the present invention is proposed to provide a solution that can effectively improve the cycle performance and fast charging performance of lithium iron phosphate batteries. Summary of the invention
[0006] The first purpose of the present invention is to provide a fast-charging lithium-ion battery, which is used to solve the technical defect that fast-charging performance and high and low temperature performance cannot be taken into account at the same time. By limiting the electrolyte, electrolyte additives, positive electrode lithium supplement additives and their dosage ratios, an organic combination of a specific positive electrode sheet and a high lithium ion conductivity electrolyte is achieved, which can simultaneously achieve a significant reduction in the battery's liquid phase ohmic impedance and the negative electrode interface impedance, significantly improve the fast-charging performance and low-temperature performance of the lithium iron phosphate battery cell, and will not cause a decrease in the battery cell's cycle performance and high-temperature performance.
[0007] The second object of the present invention is to provide a method for preparing the fast-charging lithium-ion battery, which is simple and easy to implement and can meet the needs of mass production.
[0008] The third object of the present invention is to provide an electrical device.
[0009] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:
[0010] A fast-chargeable lithium-ion battery, wherein the positive electrode of the lithium-ion battery comprises lithium iron phosphate and a positive electrode additive; the positive electrode additive comprises at least one of lithium ferrite, lithium oxalate and lithium squarate;
[0011] The electrolyte of the lithium-ion battery includes a solvent, a lithium salt and an electrolyte additive; the solvent includes a low-viscosity solvent, and the viscosity of the low-viscosity solvent is ≤0.5cps; the electrolyte additive includes a carbonate additive, a sulfur-containing additive and a lithium salt additive.
[0012] The method for preparing the fast-charging lithium-ion battery comprises the following steps:
[0013] The raw material components of the positive electrode of the lithium-ion battery are fully mixed to prepare a positive electrode slurry; the positive electrode slurry is coated on an aluminum foil current collector by a double-layer coating method, and the positive electrode sheet is obtained after drying;
[0014] Fully mixing raw material components of lithium-ion battery electrolyte to prepare electrolyte;
[0015] The positive electrode sheet, the negative electrode sheet, the separator and the electrolyte are assembled to prepare a fast-charging lithium-ion battery.
[0016] An electrical device comprises the lithium-ion battery.
[0017] Compared with the prior art, the present invention has the following beneficial effects:
[0018] (1) The present invention designs and adopts a positive electrode sheet with a specific composition; wherein a positive electrode additive that can release oxygen (such as lithium ferrite) or carbon dioxide (such as lithium oxalate or lithium squarate) during the battery cell formation process is added to the positive electrode sheet, so that the negative electrode of the battery cell is in a biased oxidizing atmosphere during the first formation process, which is conducive to the formation of a low-impedance SEI film with a biased inorganic component on the surface of the negative electrode, which can greatly reduce the interface impedance of the negative electrode; this makes it possible to add more negative electrode film-forming additives to the high ionic conductivity electrolyte (to ensure the cycle and high temperature performance) without significantly increasing the interface impedance of the negative electrode of the battery cell.
[0019] (2) The present invention uses a positive electrode slurry containing a positive electrode additive to leave pores and vacancies in the positive electrode sheet after formation, thereby improving the tortuosity of the positive electrode sheet, enhancing the dynamic performance of the positive electrode sheet, and improving the overall fast charging and low temperature performance of the battery cell.
[0020] (3) The present invention uses a high ionic conductivity electrolyte prepared with a low viscosity solvent, which can significantly reduce the ohmic impedance of the battery cell and eliminate the concentration polarization between the surface of the negative electrode sheet and the surface of the internal active material during high-rate charging, thereby increasing the negative electrode lithium plating current threshold. DETAILED DESCRIPTION
[0021] The technical scheme of the present invention will be clearly and completely described below in conjunction with specific embodiments, but those skilled in the art will appreciate that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work are within the scope of protection of the present invention. Those who do not specify specific conditions in the embodiments are carried out according to conventional conditions or conditions recommended by the manufacturer. Those who do not specify the manufacturer for reagents or instruments used are conventional products that can be purchased commercially. In addition, the terms "one", "two", "1", "2", etc. are only used for descriptive purposes and cannot be interpreted as indicating or implying relative importance.
[0022] The first aspect of the present invention is to provide a fast-charging lithium-ion battery, which belongs to a secondary battery.
[0023] The positive electrode of the lithium-ion battery includes lithium iron phosphate and a positive electrode additive; the positive electrode additive includes at least one of lithium ferrite, lithium oxalate and lithium squarate; the electrolyte of the lithium-ion battery includes a solvent, a lithium salt and an electrolyte additive; the solvent includes a low-viscosity solvent, and the viscosity of the low-viscosity solvent is ≤0.5cps; the electrolyte additive includes a carbonate additive, a sulfur-containing additive and a lithium salt additive.
[0024] As a preferred embodiment, the positive electrode additive is lithium ferrite.
[0025] As a preferred embodiment, the mass ratio of the positive electrode additive to the positive electrode slurry is W1, 0.3%≤W1≤1%, and in some optional embodiments, the value of W1 includes but is not limited to any one of 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, or any two of them. It should be noted here that the preparation of "positive electrode slurry" is a necessary step in the conventional electrode preparation process in this field, that is, the slurry obtained by mixing the positive electrode active material, positive electrode additive and other components (such as conductive agent, binder, etc.) with a solvent.
[0026] As a preferred embodiment, the mass ratio of the low-viscosity solvent to the electrolyte is W2, 20%≤W2≤60%. In some optional embodiments, the value of W2 includes but is not limited to 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, any one of them or a numerical range consisting of any two of them.
[0027] As a preferred embodiment, the mass ratio of the carbonate additive to the electrolyte is W3, 4%≤W3≤6%. In some optional embodiments, the value of W3 includes but is not limited to 4%, 4.2%, 4.5%, 4.8%, 5%, 5.2%, 5.5%, 5.8%, 6%, any one of them or a numerical range consisting of any two of them.
[0028] As a preferred embodiment, the mass ratio of the sulfur-containing additive to the electrolyte is W4, 0.3%≤W4≤2%. In some optional embodiments, the value of W4 includes but is not limited to 0.3%, 0.4%, 0.5%, 0.6%, 0.8%, 1%, 1.2%, 1.5%, 1.6%, 1.8%, 2%, any one of which or a numerical range consisting of any two of them.
[0029] As a preferred embodiment, the mass ratio of the lithium salt additive to the electrolyte is W5, 0.3%≤W5≤1%. In some optional embodiments, the value of W5 includes but is not limited to 0.3%, 0.4%, 0.5%, 0.6%, 0.8%, 1%, 1.2%, 1.5%, 1.6%, 1.8%, 2%, any one of which or a numerical range consisting of any two of them.
[0030] As a more preferred embodiment, the weight ratio of each component in the lithium-ion battery satisfies the following relationship: 0.12≤(W3+W4+W5) / W2≤0.23, that is, the total amount of the electrolyte additive and the amount ratio of the low-viscosity solvent are preferably limited; since the low-viscosity solvent introduced in the present invention has a probability of side reactions with the negative electrode interface, that is, there is a certain instability compared with conventional electrolyte solvents, it is necessary to ensure the amount of the electrolyte additive to enhance the interface stability of the battery cell; but correspondingly, the electrolyte additive also has a certain upper limit to prevent the battery impedance from increasing and offset the improvement of the fast charging capability of the low-viscosity solvent.
[0031] As a more preferred embodiment, the weight ratio of each component in the lithium-ion battery satisfies the following relationship: 2≤W3 / (W4+W5)≤6; that is, the usage ratio of the organic additive and the inorganic additive in the electrolyte additive is preferably limited. When the ratio of the two is within an appropriate range, the thermal stability and mechanical toughness of the battery cell SEI can be effectively balanced, further balancing the high temperature storage performance and cycle performance of the battery.
[0032] As a more preferred embodiment, the weight ratio of each component in the lithium-ion battery satisfies the following relationship: 0.08≤W1 / W3≤0.16, that is, the usage ratio of the positive electrode additive to the carbonate additive is preferably limited; wherein, the carbonate additive is a key additive in the lithium iron phosphate battery, and the internal resistance of the battery is positively correlated with its addition amount, and the positive electrode additive can reduce the battery impedance. Therefore, as the amount of the positive electrode additive increases, the amount of the carbonate additive can be increased synchronously, and at the same time, it will not lead to an increase in the impedance of the battery cell, and has good cycle performance and high temperature performance while ensuring low impedance of the battery cell.
[0033] As a preferred embodiment, the positive electrode of the lithium-ion battery includes lithium iron phosphate, a positive electrode additive, a conductive agent and a binder; wherein, lithium iron phosphate can be understood as a positive electrode active component. In some optional embodiments, the lithium-ion battery also includes other positive electrode active components, but the present invention is based on the improvement of the lithium iron phosphate battery, so the positive electrode active material is only lithium iron phosphate or lithium iron phosphate is the main active component; as a more preferred embodiment, the conductive agent includes at least one of carbon nanotubes, acetylene black, Ketjen black or carbon fiber, and the binder includes at least one of polyvinylidene fluoride, polytetrafluoroethylene, polyacrylonitrile or polyacrylic acid.
[0034] As a more preferred embodiment, in the positive electrode of the lithium ion battery, the mass ratio of the lithium iron phosphate, the positive electrode additive, the conductive agent and the binder is (95~97): (0.3~1.0): (0.5~2): (1.5~2.5).
[0035] As a preferred embodiment, the positive electrode of the lithium-ion battery includes a current collector and a positive electrode coating layer coated on both sides of the current collector. The double-layer coating can effectively improve the distribution of the pores of the positive electrode sheet; it can be understood that the lithium iron phosphate and the positive electrode additive (as well as the conductive agent and the binder) are components in the positive electrode coating layer; the positive electrode additive only exists in the positive electrode coating layer on one side; in some more preferred embodiments, the positive electrode additive only exists on one side of the positive electrode sheet close to the surface of the electrode sheet and away from the current collector.
[0036] As a preferred embodiment, the electrolyte has an ion conductivity of ≥13 mS / cm at room temperature, and has relatively high ion conductivity.
[0037] As a preferred embodiment, the low-viscosity solvent includes at least one of carboxylic acid esters, acetonitrile, fluoroacetonitrile, and propionitrile, wherein the carboxylic acid ester includes at least one of ethyl acetate, methyl acetate, and methyl propionate; the viscosity range of the overall solvent achieved by the above-mentioned low-viscosity solvent component belongs to a suitable interval range.
[0038] As a more preferred embodiment, the mass ratio of the sum of the masses of the acetonitrile, the fluoroacetonitrile or the propionitrile to the electrolyte is W6, W6<20%; it can be understood that there should be an upper limit on the amount of low-viscosity nitrile solvents to avoid negative effects on the high temperature performance of the battery when the amount of nitrile solvents is too high.
[0039] As a more preferred embodiment, the low viscosity solvent is ethyl acetate, or a two-component combination of ethyl acetate and acetonitrile.
[0040] As a preferred embodiment, the solvent also includes cyclic carbonate; wherein the cyclic carbonate includes ethylene carbonate, propylene carbonate, etc.; in some more preferred embodiments, the mass ratio of the cyclic carbonate to the electrolyte is 8%~12%, and appropriately reducing the amount of the cyclic carbonate is beneficial to improving the fast charging and low temperature performance of the battery cell.
[0041] As an optional embodiment, the solvent further includes a chain ester; wherein the chain ester includes dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, propyl propionate, methyl butyrate, ethyl butyrate, butyl butyrate and the like.
[0042] As a preferred embodiment, the lithium salt includes at least one of lithium hexafluorophosphate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethylsulfonyl)imide, lithium perchlorate or lithium tetrafluoroborate.
[0043] As a preferred embodiment, the mass ratio of the lithium salt to the electrolyte is 12% to 20%.
[0044] As a preferred embodiment, the carbonate additive includes at least one of vinylene carbonate, fluoroethylene carbonate or EBC; wherein the structural formula of the EBC is: .
[0045] As a preferred embodiment, the sulfur-containing additive includes at least one of vinyl sulfate, propylene sulfate, 1,3-propane sultone, 1,4-butane sultone, methylene methanedisulfonate, vinyl bissulfate, spiro vinyl sulfate or dimethyl sulfite.
[0046] As a preferred embodiment, the lithium salt additive includes at least one of lithium difluorophosphate, lithium bis(oxalatoborate), lithium bis(oxalatophosphate), lithium difluorooxalatoborate or lithium fluorosulfonate.
[0047] As a preferred embodiment, the present invention does not impose any restrictions on the negative electrode and separator of the fast-charging lithium-ion battery; those skilled in the art can use any commercially available product or homemade product; on the premise of realizing the secondary battery function, any negative electrode or separator can be used as an optional embodiment of the present invention.
[0048] As a preferred embodiment, when the positive electrode additive includes the lithium ferrite, the first full charge cut-off voltage of the fast-charging lithium-ion battery is ≥4.2V; when the positive electrode additive includes the lithium squarate, the first full charge cut-off voltage of the fast-charging lithium-ion battery must be ≥4.3V; when the positive electrode additive includes the lithium oxalate, the first full charge cut-off voltage of the fast-charging lithium-ion battery is ≥4.8V.
[0049] The second aspect of the present invention is to provide a method for preparing the fast-charging lithium-ion battery.
[0050] The preparation method comprises the following steps: fully mixing raw material components of the positive electrode of the lithium ion battery to prepare a positive electrode slurry; coating it on an aluminum foil current collector by a double-layer coating method, and drying it to obtain a positive electrode sheet; fully mixing raw material components of the lithium ion battery electrolyte to obtain an electrolyte; and assembling the positive electrode sheet, the negative electrode sheet, the separator and the electrolyte to obtain a fast-charging lithium ion battery.
[0051] The solvent composition and dosage of the positive electrode slurry, the specific coating operation, the drying temperature or time, the assembly of the battery functional components, etc. involved in the present invention can adopt the conventional characteristics or parameter ranges in the field, and the present invention does not impose additional limitations on the above characteristics.
[0052] As a preferred embodiment, the fast-charging lithium-ion battery is obtained by sequentially assembling, packaging, injecting electrolyte, forming and finally sealing the positive electrode sheet, the negative electrode sheet, the separator and the electrolyte; wherein the formation adopts high-temperature formation, and the formation temperature is 40°C~50°C.
[0053] A third aspect of the present invention is to provide an electrical device.
[0054] The electrical equipment should include the lithium-ion battery as described in the first aspect; those skilled in the art can understand that the electrical equipment includes but is not limited to electric vehicles, household appliances, mobile communication equipment, office appliances, industrial equipment, etc. As long as a device includes the fast-charging lithium-ion battery, it can be used as a feasible implementation method of the present invention.
[0055] Example 1
[0056] This embodiment provides a secondary lithium-ion battery, which is composed of a positive electrode sheet, a negative electrode sheet, a separator, an electrolyte and a shell, and the manufacturing process thereof is as follows.
[0057] (1) Positive electrode manufacturing: lithium iron phosphate, lithium ferrite, conductive carbon black, carbon nanotubes, and polyvinylidene fluoride are prepared and mixed in a certain mass ratio. During the mixing process, N-methylpyrrolidone is used to prepare the mixture into a positive electrode slurry with a solid content of 60%. A double-layer coating process is adopted, with the upper and lower layers each accounting for 50wt.%. Among them, lithium iron phosphate, lithium ferrite, conductive carbon black, carbon nanotubes, and polyvinylidene fluoride in the upper layer are mixed in a mass ratio of 96.5:0:1:0.5:2, and lithium iron phosphate, lithium ferrite, conductive carbon black, carbon nanotubes, and polyvinylidene fluoride in the lower layer are mixed in a mass ratio of 95.5:1:1:0.5:2; then the upper and lower layers of slurry are respectively coated on the aluminum foil current collector, and after drying at 60°C, they are rolled and die-cut to form the required positive electrode sheet.
[0058] (2) Negative electrode manufacturing: Graphite, conductive carbon black, sodium carboxymethyl cellulose, and styrene-butadiene rubber were prepared in a mass ratio of 96:1:1:2 and mixed with deionized water to form a slurry with a solid content of 51%. The slurry was then coated on a copper foil current collector and dried at 60°C before being rolled and die-cut to form the desired negative electrode sheet.
[0059] (3) Preparation of electrolyte: The electrolyte was prepared by mixing according to the following mass proportions: 12 wt % of lithium hexafluorophosphate, 3 wt % of lithium bis(fluorosulfonyl)imide, 25 wt % of ethylene carbonate, 10 wt % of ethyl methyl carbonate, 43 wt % of ethyl acetate, 4 wt % of vinylene carbonate, 2 wt % of fluorocarbonic acid, 0.5 wt % of vinyl sulfate, 0.3 wt % of lithium difluorophosphate, and 0.2 wt % of tris(trimethylsilyl) phosphate.
[0060] (4) Dry cell manufacturing: The positive and negative electrode sheets prepared above are stacked with a ceramic-coated PP separator of corresponding size and thickness of 12 microns using a stacking machine to obtain a wound core with a capacity of 4Ah; after welding the pole ears, they are packaged with aluminum-plastic film, baked at 85°C for 24 hours, and then filled with liquid for packaging. After standing, they are formed.
[0061] The formation is carried out in a 45°C incubator, and the steps are as follows: 1) Use a current of 0.2A to charge the battery for 2 hours, and the cut-off voltage is 3.65V; 2) Then use a current of 0.8A to charge the battery at a constant current and constant voltage to 4.2V, and the cut-off current is 0.2A; 3) The battery cell is aged in a 45°C incubator for 24 hours, and then taken out, vented, and repackaged; 4) Use a current of 1.33A to charge the battery cell at a constant current and constant voltage to 3.65V, and the cut-off current is 0.2A; 5) Use a current of 1.33A to discharge the battery cell at a constant current, and the cut-off voltage is 2.0V; 6) Continue to use a current of 1.33A to charge and discharge the battery cell in the range of 2.0V~3.65V for 2 weeks.
[0062] After the formation is completed, final sealing is performed to finally obtain the lithium-ion secondary battery of this embodiment.
[0063] Example 2
[0064] It is basically the same as Example 1, except that:
[0065] (3) Preparation of electrolyte: The electrolyte was prepared by mixing according to the following mass proportions: 12 wt % lithium hexafluorophosphate, 3 wt % lithium bis(fluorosulfonyl)imide, 20 wt % ethylene carbonate, 8 wt % ethyl methyl carbonate, 40 wt % ethyl acetate, 10 wt % acetonitrile, 4 wt % vinylene carbonate, 2 wt % fluoroethylene carbonate, 0.6 wt % vinyl sulfate, and 0.4 wt % lithium bis(oxalatoborate).
[0066] Example 3
[0067] It is basically the same as Example 1, except that:
[0068] (1) Positive electrode manufacturing: lithium iron phosphate, lithium ferrite, conductive carbon black, carbon nanotubes, and polyvinylidene fluoride are prepared and mixed in a mass ratio of 95.5:1:1:0.5:2. During the mixing process, the mixture is prepared into a positive electrode slurry with a solid content of 60% using N-methylpyrrolidone; the slurry is then coated on an aluminum foil current collector to produce a double-sided coated electrode sheet, which is then dried at 60°C and roll-cut to produce the required positive electrode sheet;
[0069] (3) Preparation of electrolyte: The electrolyte was prepared by mixing according to the following mass proportions: 12 wt % of lithium hexafluorophosphate, 3 wt % of lithium bis(fluorosulfonyl)imide, 20 wt % of ethylene carbonate, 8 wt % of ethyl methyl carbonate, 40 wt % of ethyl acetate, 10 wt % of acetonitrile, 4 wt % of vinylene carbonate, 2 wt % of fluoroethylene carbonate, 0.8 wt % of vinyl sulfate, 0.3 wt % of lithium difluorophosphate, and 0.2 wt % of tris(trimethylsilyl) phosphate.
[0070] Example 4
[0071] It is basically the same as Example 1, except that:
[0072] (1) Cathode manufacturing: Replace lithium ferrite with lithium squarate as a whole;
[0073] (4) The formation is carried out in a 45°C incubator, and the steps are as follows: 1) Use a current of 0.2A to charge the battery for 2 hours, with a cut-off voltage of 3.65V; 2) Then use a current of 0.8A to charge the battery at a constant current and constant voltage to 4.3V, with a cut-off current of 0.2A; 3) The battery cell is aged in a 45°C incubator for 24 hours, and then taken out, vented, and repackaged; 4) Use a current of 1.33A to charge the battery cell at a constant current and constant voltage to 3.65V, with a cut-off current of 0.2A; 5) Use a current of 1.33A to discharge the battery cell at a constant current, with a cut-off voltage of 2.0V; 6) Continue to use a current of 1.33A to charge and discharge the battery cell in the range of 2.0V~3.65V for 2 weeks.
[0074] Example 5
[0075] It is basically the same as Example 1, except that:
[0076] (3) Preparation of electrolyte: The electrolyte was prepared by mixing according to the following mass proportions: 12 wt % of lithium hexafluorophosphate, 3 wt % of lithium bis(fluorosulfonyl)imide, 25 wt % of ethylene carbonate, 10 wt % of ethyl methyl carbonate, 43 wt % of methyl propionate, 4 wt % of vinylene carbonate, 2 wt % of fluorocarbonic acid, 0.7 wt % of vinyl sulfate, 0.2 wt % of lithium difluorophosphate, and 0.1 wt % of tris(trimethylsilyl) phosphate.
[0077] Example 6
[0078] It is basically the same as Example 1, except that:
[0079] (3) Preparation of electrolyte: The electrolyte was prepared by mixing according to the following mass proportions: 12 wt % of lithium hexafluorophosphate, 3 wt % of lithium bis(fluorosulfonyl)imide, 25 wt % of ethylene carbonate, 10 wt % of ethyl methyl carbonate, 43 wt % of methyl acetate, 4 wt % of vinylene carbonate, 2 wt % of fluorocarbonic acid, 0.6 wt % of vinyl sulfate, and 0.4 wt % of lithium difluorooxalatoborate.
[0080] Example 7
[0081] It is basically the same as Example 1, except that:
[0082] (3) Preparation of electrolyte: The electrolyte was prepared by mixing according to the following mass proportions: 12 wt % lithium hexafluorophosphate, 3 wt % lithium bis(fluorosulfonyl)imide, 25 wt % ethylene carbonate, 32 wt % ethyl methyl carbonate, 20 wt % acetonitrile, 4 wt % vinylene carbonate, 2 wt % fluorocarbonic acid, 1 wt % vinyl sulfate, 0.5 wt % propane sultone, and 0.5 wt % lithium difluorophosphate bis(oxalate).
[0083] Comparative Example 1
[0084] It is basically the same as Example 1, except that:
[0085] (1) Positive electrode manufacturing: lithium iron phosphate, conductive carbon black, carbon nanotubes, and polyvinylidene fluoride are prepared and mixed in a mass ratio of 96.5:1:0.5:2. During the mixing process, the mixture is prepared into a positive electrode slurry with a solid content of 60% using N-methylpyrrolidone; the slurry is then coated on an aluminum foil current collector, dried at 60°C, and then roll-pressed and die-cut to form the required positive electrode sheet.
[0086] (3) Preparation of electrolyte: The electrolyte was prepared by mixing according to the following mass proportions: 10 wt % of lithium hexafluorophosphate, 3 wt % of lithium bis(fluorosulfonyl)imide, 25 wt % of ethylene carbonate, 25 wt % of ethyl methyl carbonate, 32 wt % of dimethyl carbonate, 3 wt % of vinylene carbonate, 1 wt % of fluorocarbonic acid, 0.7 wt % of vinyl sulfate, 0.2 wt % of lithium difluorophosphate, and 0.1 wt % of tris(trimethylsilyl) phosphate.
[0087] Comparative Example 2
[0088] It is basically the same as Example 1, except that:
[0089] (3) Preparation of electrolyte: The electrolyte was prepared by mixing according to the following mass proportions: 12 wt % lithium hexafluorophosphate, 3 wt % lithium bis(fluorosulfonyl)imide, 20 wt % ethylene carbonate, 8 wt % ethyl methyl carbonate, 40 wt % ethyl acetate, 10 wt % acetonitrile, 4 wt % vinylene carbonate, 2 wt % fluoroethylene carbonate, 0.7 wt % vinyl sulfate, 0.2 wt % lithium difluorophosphate, and 0.1 wt % tris(trimethylsilyl) phosphate.
[0090] Comparative Example 3
[0091] It is basically the same as Example 1, except that:
[0092] (3) Preparation of electrolyte: The electrolyte was prepared by mixing according to the following mass proportions: 12 wt % lithium hexafluorophosphate, 3 wt % lithium bis(fluorosulfonyl)imide, 25 wt % ethylene carbonate, 10 wt % ethyl methyl carbonate, 45 wt % ethyl acetate, 3 wt % vinylene carbonate, 1 wt % fluorocarbonic acid, 0.7 wt % vinyl sulfate, 0.2 wt % lithium difluorophosphate, and 0.1 wt % tris(trimethylsilyl) phosphate.
[0093] Table 1 below provides the characteristic relationship between the above-mentioned embodiments of the present invention and the comparative examples.
[0094] Table 1
[0095] Group positive electrode Electrolyte Total amount of film-forming additives Comparative Example 1 Ordinary positive electrode Conventional carbonate electrolyte 5% Comparative Example 2 Ordinary positive electrode EA high conductivity electrolyte 7% Comparative Example 3 Ordinary positive electrode EA high conductivity electrolyte 5% Example 1 +0.5% Lithium Ferrite EA high conductivity electrolyte 7% Example 2 +0.5% Lithium Ferrite EA+ACN high conductivity electrolyte 7% Example 3 +1% Lithium Ferrite EA+ACN high conductivity electrolyte 7% Example 4 +0.5% Lithium Squarate EA high conductivity electrolyte 7% Example 5 +0.5% Lithium Ferrite MP High Conductivity Electrolyte 7% Example 6 +0.5% Lithium Ferrite MA High Conductivity Electrolyte 7% Example 7 +0.5% Lithium Ferrite ACN high conductivity electrolyte 7%
[0096] Test example
[0097] In order to compare the performance differences between the embodiments and the comparative examples, the following four tests were performed. Table 2 below provides the test results of the embodiments and the comparative examples.
[0098] (I) Three-electrode charging capacity test: Use the negative electrode constant voltage charging process to monitor the current change during the charging process; use an electrochemical workstation to monitor the voltage change of the negative electrode relative to the reference electrode, and control the current size, always keeping the potential difference between the negative electrode and the reference electrode at 5mV until the charging process is completed. The battery's maximum charging time can be calculated based on the current size during the charging process.
[0099] (ii) 25℃ / -20℃ DC internal resistance test: Test the charging DC internal resistance and discharging DC internal resistance at 50% SOC state respectively.
[0100] (iii) 25°C / 45°C cycle test: The capacity retention rate is tested after 500 cycles at 25°C and 45°C respectively.
[0101] (IV) 60°C high temperature storage test: Test the battery capacity recovery rate and gas production after 30 days under high temperature conditions.
[0102] Table 2
[0103]
[0104] Although the present invention has been illustrated and described with specific embodiments, it should be appreciated that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Those skilled in the art should understand that the technical solutions described in the above embodiments may be modified, or some or all of the technical features thereof may be replaced by equivalents without departing from the spirit and scope of the present invention. However, these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention. Therefore, this means that all such replacements and modifications within the scope of the present invention are included in the appended claims.
Claims
1. A fast-charge lithium-ion battery, characterized in that: The positive electrode of the lithium-ion battery includes lithium iron phosphate and a positive electrode additive; the positive electrode additive includes at least one of lithium ferrite, lithium oxalate and lithium squarate; The electrolyte of the lithium-ion battery comprises a solvent, a lithium salt and an electrolyte additive; the solvent comprises a low-viscosity solvent, and the viscosity of the low-viscosity solvent is ≤0.5 cps; the electrolyte additive comprises a carbonate additive, a sulfur-containing additive and a lithium salt additive; The fast-chargeable lithium-ion battery meets the following characteristics (A) to (E) and characteristics (a) to (c): (A) The mass ratio of the positive electrode additive to the positive electrode slurry is W1, 0.3%≤W1≤1%; (B) The mass ratio of the low-viscosity solvent to the electrolyte is W2, 20%≤W2≤60%; (C) The mass ratio of the carbonate additive to the electrolyte is W3, 4%≤W3≤6%; (D) The mass ratio of the sulfur-containing additive to the electrolyte is W4, 0.3%≤W4≤2%; (E) The mass ratio of the lithium salt additive to the electrolyte is W5, 0.3%≤W5≤1%; (a) 0.12≤(W3+W4+W5) / W2≤0.23; (b) 2≤W3 / (W4+W5)≤6; (c) 0.08≤W1 / W3≤0.
16.
2. The fast-chargeable lithium-ion battery according to claim 1, characterized in that: The positive electrode of the lithium-ion battery comprises lithium iron phosphate, a positive electrode additive, a conductive agent and a binder; The mass ratio of the lithium iron phosphate, the positive electrode additive, the conductive agent and the binder is (95-97): (0.8-1.5): (0.1-1): (1.5-2.5).
3. The fast-chargeable lithium-ion battery according to claim 1, characterized in that: The low viscosity solvent includes at least one of carboxylic acid ester, acetonitrile, fluoroacetonitrile, and propionitrile, wherein the carboxylic acid ester includes at least one of ethyl acetate, methyl acetate, and methyl propionate; The solvent further comprises a cyclic carbonate; wherein the cyclic carbonate comprises ethylene carbonate or propylene carbonate, and the mass ratio of the cyclic carbonate to the electrolyte is 8% to 12%.
4. The fast-chargeable lithium-ion battery according to claim 1, characterized in that: The lithium salt includes at least one of lithium hexafluorophosphate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethylsulfonyl)imide, lithium perchlorate or lithium tetrafluoroborate; The mass ratio of the lithium salt to the electrolyte is 12% to 20%.
5. The fast-chargeable lithium-ion battery according to claim 1, characterized in that: The fast-chargeable lithium-ion battery includes at least one of the following features (1) to (3): (1) The carbonate additive includes at least one of vinylene carbonate, fluoroethylene carbonate or EBC; (2) The sulfur-containing additive includes at least one of vinyl sulfate, propylene sulfate, 1,3-propane sultone, 1,4-butane sultone, methylene disulfonate, vinyl bissulfate, spirosulfate or dimethyl sulfite; (3) The lithium salt additive includes at least one of lithium difluorophosphate, lithium bis(oxalatoborate), lithium bis(oxalatophosphate), lithium difluorooxalatoborate or lithium fluorosulfonate.
6. The fast-chargeable lithium-ion battery according to claim 1, characterized in that: The positive electrode of the lithium-ion battery includes a current collector and a positive electrode coating layer coated on both sides of the current collector; One side of the positive electrode coating layer includes the positive electrode additive, and the other side of the positive electrode coating layer does not include the positive electrode additive.
7. The method for preparing a fast-chargeable lithium-ion battery according to any one of claims 1 to 6, characterized in that: The preparation method comprises the following steps: The raw material components of the positive electrode of the lithium-ion battery are fully mixed to prepare a positive electrode slurry; the positive electrode slurry is coated on an aluminum foil current collector by a double-layer coating method, and the positive electrode sheet is obtained after drying; Fully mixing raw material components of lithium-ion battery electrolyte to prepare electrolyte; The positive electrode sheet, the negative electrode sheet, the separator and the electrolyte are assembled to prepare a fast-charging lithium-ion battery.
8. An electrical device, characterized in that: The electrical equipment comprises a fast-charging lithium-ion battery as described in any one of claims 1 to 6.