Long-life graphite composite negative electrode material for energy storage and preparation method and application thereof
By mixing coke raw materials with heteroatom compounds and performing low-temperature graphitization, combined with the coating treatment of amine compounds, etc., a fluorine-doped hard carbon material is formed, which solves the problem of poor cycle performance of graphite anode materials in the existing technology, and significantly Improved material stability and battery performance.
Patent Information
- Application Number
- CN202411035764.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-07-31
AI Technical Summary
In the existing technology, the preparation process of artificial graphite anode materials cannot effectively improve high rate and long cycle life, especially in terms of structural stability and cycle performance.
Fluorine-doped hard carbon materials are formed by mixing coke raw materials with heteroatom compounds, pressing, calcining, and low-temperature graphitization, combined with chemical reaction coatings of amines, organic fluorides, and amino resins, and using water vapor to create pores. Reduce expansion and specific surface area, improve electronic conductivity and cycle performance.
It significantly improves the structural stability and electronic conductivity of the material, extends the cycle life of the battery, improves the energy density and dynamic performance of the lithium-ion battery, and improves the storage performance and cycle performance.
Smart Images

Figure CN118561277B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of electrode materials, and in particular to a long-life graphite composite negative electrode material for energy storage, and a preparation method and application thereof. Background Art
[0002] As the market's requirements for the cycle life of energy storage batteries increase, negative electrode materials are required to have characteristics such as stable structure and few defects to improve the material's cycle performance. Therefore, it is necessary to increase the material's interlayer spacing or reduce side reactions during the material's charge and discharge process through low-temperature graphitization or material doping and coating to improve the cycle performance.
[0003] In the prior art, the preparation process of artificial graphite negative electrode materials is crushing, shaping and grading to control the particle size distribution in the isotropic coke, reduce the fine powder content and increase the life, but the improvement is not large, especially for large rates and long cycles. Summary of the invention
[0004] The main purpose of the present invention is to provide a long-life graphite composite negative electrode material for energy storage and a preparation method and application thereof, aiming to improve the cycle performance of the electrode material.
[0005] To achieve the above object, the present invention provides a method for preparing a long-life graphite composite negative electrode material for energy storage, comprising the following steps:
[0006] S10. mixing, grinding, pressing, calcining, and graphitizing the coke raw material and the heteroatom compound to obtain a graphite precursor material;
[0007] S20. The amine compound, the organic fluorine compound, the amino resin and the organic solvent are mixed and dried to obtain a coating material;
[0008] S30. The graphite precursor material, the coating material and the solvent are mixed, filtered, vacuum dried, introduced with water vapor to activate pore formation, and heated to obtain a long-life graphite composite negative electrode material for energy storage;
[0009] Among them, the mass ratio of coke raw material to heteroatom compound is 100:(1~5);
[0010] The mass ratio of the amine compound, the organic fluorine compound, the amino resin and the organic solvent is (5-15): (5-15): 100: 1000;
[0011] In step S10, the pressing pressure is 10-50 MPa;
[0012] In step S10, the calcination temperature is 600-800°C, and the calcination time is 1-6 hours;
[0013] In step S10, the graphitization temperature is 2600-2800°C, and the graphitization time is 6-24 hours;
[0014] In step S30, the mass ratio of the graphite precursor material, the coating material and the solvent is 100: (11-13): (260-1100);
[0015] In step S30, the activation pore-forming temperature is 800-1000°C, and the activation pore-forming time is 1-3 h;
[0016] In step S30, the temperature of heating carbonization is 2600-2800°C, and the duration of heating carbonization is 1-6 hours.
[0017] In one embodiment, the coke raw material includes at least one of oil-based needle coke, coal-based needle coke, petroleum coke and coal-based pitch coke; and / or,
[0018] The heteroatom compound includes at least one of pyrrole, furan, thiophene, pyridine, pyrimidine and quinoline.
[0019] In one embodiment, the amine compound includes at least one of naphthylamine, benzylamine, N-methylaniline, phenylhydrazine, methylaniline and benzylaniline; and / or,
[0020] The organic solvent comprises at least one of ethanol, ether and 1,3-butanediol; and / or,
[0021] The organic fluorine compound includes at least one of trifluoroethyl acrylate, hexafluorobutyl acrylate, pentafluorophenyl benzoate and difluoromethyl trifluoromethanesulfonate; and / or,
[0022] The amino resin includes at least one of urea-formaldehyde resin, melamine-formaldehyde resin, polyurethane resin, polyurethane resin and polyamide resin.
[0023] The present invention also provides a long-life graphite composite negative electrode material for energy storage, which is prepared according to the above-mentioned method for preparing the long-life graphite composite negative electrode material for energy storage.
[0024] The present invention also proposes an application of a long-life graphite composite negative electrode material for energy storage in a lithium-ion battery. The long-life graphite composite negative electrode material for energy storage includes the aforementioned long-life graphite composite negative electrode material for energy storage.
[0025] The technical scheme of the present invention improves the structural stability of the material and the electronic conductivity of the material by uniformly mixing the coke raw material and the heteroatom compound, and performs processes such as briquetting, shallow calcination, and low-temperature graphitization, and the material obtained by low-temperature graphitization has a large interlayer spacing and reduces expansion; by chemically reacting amine compounds, organic fluorine compounds, and amino resins and coating them on the surface of graphite, the impedance is reduced by utilizing the strong electronegativity of fluorine atoms, which can effectively increase the gram capacity of lithium-ion batteries and improve the energy density of lithium-ion batteries; at the same time, the F atoms at the edge of the fluorine-doped graphite negative electrode material can form more stable fluorides with lithium salts in the electrolyte to ensure the long cycle performance of the lithium-ion battery, and the amino resin is carbonized to obtain nitrogen-doped hard carbon, which improves the kinetic performance of the material; by forming pores through water vapor, the expansion of the material during charging and discharging is reduced, and amorphous carbon is coated on its surface to reduce the specific surface area and defects, thereby improving the storage performance and its cycle performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.
[0027] Figure 1 A schematic flow chart of a method for preparing a long-life graphite composite negative electrode material for energy storage provided by the present invention;
[0028] Figure 2 This is a scanning electron microscope image of the long-life graphite composite negative electrode material for energy storage in Example 1 of the present invention.
[0029] The purpose, features and advantages of the present invention will be further described with reference to the accompanying drawings in conjunction with the embodiments. DETAILED DESCRIPTION
[0030] It should be noted that, in the embodiments, those without specifying specific conditions are carried out according to normal conditions or conditions recommended by the manufacturer. Those without specifying the manufacturer of reagents or instruments used are conventional products that can be purchased commercially. In addition, the meaning of "and / or" appearing in the full text includes three parallel schemes, and "A and / or B" is taken as an example, including schemes A, B, or A and B that meet the same time. In addition, the technical schemes between the various embodiments can be combined with each other, but must be based on the ability of ordinary technicians in the field to achieve. When the combination of the technical schemes is contradictory or cannot be achieved, it should be considered that the combination of such technical schemes does not exist, and is not within the scope of protection required by the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work, all belong to the scope of protection of the present invention.
[0031] At present, in the existing technology, the preparation process of artificial graphite negative electrode materials is crushing, shaping and grading to control the particle size distribution in the isotropic coke, reduce the fine powder content and increase the life, but the improvement is not large, especially for large rates and long cycles.
[0032] For this reason, please see Figure 1 The present invention proposes a method for preparing a long-life graphite composite negative electrode material for energy storage, comprising the following steps: S10. mixing a coke raw material and a heteroatom compound, grinding, pressing, calcining, and graphitizing to obtain a graphite precursor material; S20. mixing an amine compound, an organic fluorine compound, an amino resin, and an organic solvent, and then drying to obtain a coating material; S30. mixing the graphite precursor material, the coating material, and the solvent, filtering, vacuum drying, introducing water vapor to activate pores, and heating to obtain a long-life graphite composite negative electrode material for energy storage.
[0033] The technical solution of the present invention improves the structural stability of the material and the electronic conductivity of the material by uniformly mixing the coke raw material and the heteroatom compound, and subjecting the material to processes such as briquetting, shallow calcination, and low-temperature graphitization, and the material obtained by low-temperature graphitization has a large interlayer spacing and reduces expansion; by subjecting amine compounds, organic fluorine compounds, and amino resins to a chemical reaction and coating them on the surface of graphite, the impedance is reduced by utilizing the strong electronegativity of fluorine atoms, thereby effectively improving the gram capacity of lithium-ion batteries and improving the energy density of lithium-ion batteries; at the same time, the fluorine atoms at the edge of the fluorine-doped graphite negative electrode material can form more stable fluorides with lithium salts in the electrolyte, thereby ensuring the long cycle performance of the lithium-ion battery, and the amino resin is carbonized to obtain nitrogen-doped hard carbon, thereby improving the kinetic performance of the material; by forming pores through water vapor, the expansion of the material during charging and discharging is reduced, and amorphous carbon is coated on its surface to reduce the specific surface area and defects, thereby improving the storage performance and its cycle performance.
[0034] It should be noted that the coke raw material can be oil-based needle coke, coal-based needle coke, petroleum coke or coal-based asphalt coke, without limitation herein; the heteroatom compound is a heterocyclic compound including heteroatoms, wherein the heteroatoms include oxygen atoms, nitrogen atoms or sulfur atoms.
[0035] In one embodiment, the coke feedstock includes at least one of oil-based needle coke, coal-based needle coke, petroleum coke and coal-based asphalt coke; and / or the heteroatom compound includes at least one of pyrrole, furan, thiophene, pyridine, pyrimidine and quinoline.
[0036] The technical solution of the present invention adopts at least one of oil-based needle coke, coal-based needle coke, petroleum coke or coal-based asphalt coke. These coke raw materials have good graphitization degree and high thermal stability, which can significantly improve the conductivity, heat resistance and mechanical strength of the final product; by introducing heteroatom compounds such as pyrrole, furan, thiophene, pyridine, pyrimidine or quinoline, these compounds can effectively change the electronic structure of the material as doping elements, thereby adjusting and optimizing the electrochemical properties, optical properties or catalytic properties of the material. For example, heteroatoms can increase the specific surface area of the material and increase the number of active sites when it is used as a catalyst or electrode material, thereby improving the catalytic efficiency or the energy density and cycle stability of the battery. The types of the above coke raw materials and heteroatom compounds can be defined separately or simultaneously; when defined simultaneously, the energy density and cycle stability of the obtained long-life graphite composite negative electrode material for energy storage can be further improved.
[0037] In one embodiment, the mass ratio of the coke raw material to the heteroatom compound is 100:(1-5).
[0038] The technical solution of the present invention adjusts the mass ratio of the coke raw material to the heteroatom compound to 100:(1-5). This ratio ensures the effective incorporation of the heteroatom compound, and will neither significantly affect the material properties due to too low a content, nor cause material structure damage or processing difficulties due to too high a content. In addition, within this mass ratio range, structural defects caused by excessive heteroatoms can be avoided, the overall performance of the electrode material can be kept stable, and the service life of the electrode material can be effectively extended.
[0039] In one embodiment, the amine compound includes at least one of naphthylamine, benzylamine, N-methylaniline, phenylhydrazine, methylaniline and benzylaniline; and / or, the organic solvent includes at least one of ethanol, ether and 1,3-butanediol; and / or, the organic fluorine compound includes at least one of trifluoroethyl acrylate, hexafluorobutyl acrylate, pentafluorophenyl benzoate and difluoromethyl trifluoromethanesulfonate; and / or, the amino resin includes at least one of urea-formaldehyde resin, melamine-formaldehyde resin, polyurethane resin, polyurethane resin and polyamide resin.
[0040] The technical solution of the present invention can effectively react with the target substance by adopting specific amine compounds to improve the selectivity and yield of the chemical reaction; by adopting organic solvents such as ethanol and ether, it can not only effectively dissolve various reactants and products and improve the uniformity of the reaction system, but also adjust the polarity of the reaction medium and promote the smooth progress of the reaction; by adopting specific organic fluorine compounds, it can form more stable fluorides with lithium salts in the electrolyte to ensure the long cycle performance of the lithium ion battery; by adopting specific amino resins, after chemical reactions and coating on the graphite surface, it can help adjust the pore structure of the electrode material and optimize the penetration and distribution of the electrolyte inside the electrode. At the same time, the amino resin forms nitrogen-doped hard carbon and its suitable pore structure after carbonization, which can effectively increase the gram capacity of the lithium ion battery and improve the energy density of the lithium ion battery.
[0041] In one embodiment, the mass ratio of the amine compound, the organic fluorine compound, the amino resin and the organic solvent is (5-15): (5-15): 100: 1000.
[0042] The technical solution of the present invention adjusts the mass ratio of the amine compound, the organic fluorine compound, the amino resin and the organic solvent, and the mass ratio between the amine compound and the organic fluorine compound is closely controlled within a similar range, which is conducive to accurately controlling the chemical reaction process. This balance ensures the effective encounter and reaction of the two active components in the reaction system, reduces the occurrence of side reactions, and improves the yield and purity of the target product.
[0043] In one embodiment, in step S10, the pressing pressure is 10-50 MPa; and / or, in step S10, the calcination temperature is 600-800°C, and the calcination time is 1-6 h; and / or, in step S10, the graphitization temperature is 2600-2800°C, and the graphitization time is 6-24 h.
[0044] The technical solution of the present invention ensures the close stacking of raw materials and forms a highly dense preform by adjusting the pressing pressure. This pressure range can not only effectively eliminate internal voids and improve the density and mechanical strength of the material, but also avoid deformation or cracks caused by excessive pressure, laying a good structural foundation for the subsequent calcination and graphitization process; by adjusting the calcination temperature and duration, it can ensure the full volatilization of impurities and avoid excessive sintering leading to reduced material stability; by adjusting the graphitization temperature and duration, the deep graphitization transformation of the raw materials is promoted, and the electrochemical performance and cycle performance of the material are improved.
[0045] In one embodiment, in step S30, the mass ratio of the graphite precursor material, the coating material and the solvent is 100: (11-13): (260-1100).
[0046] The technical solution of the present invention ensures the uniformity and integrity of the coating layer by adjusting the mass ratio of the ink precursor material to the coating material. An appropriate amount of coating material can effectively cover the surface of the graphite precursor to form a continuous and thin coating layer, avoiding poor contact of the internal active substances due to excessive thickness or insufficient protection due to excessive thinness, thereby improving the overall stability and cycle performance of the material.
[0047] In one embodiment, in step S30, the activation pore-forming temperature is 800-1000°C, and the activation pore-forming time is 1-3 hours; and / or, in step S30, the heating carbonization temperature is 2600-2800°C, and the heating carbonization time is 1-6 hours.
[0048] The technical solution of the present invention can effectively remove impurities and volatile substances in the raw materials by adjusting the temperature and duration of activation pore formation, and also create rich micropores and mesoporous structures, increase the specific surface area of the electrode material, enhance the liquid retention performance of the material, and further improve the cycle performance; by adjusting the temperature and duration of carbonization, the raw materials can be thoroughly carbonized, so that the prepared electrode material has excellent electrochemical properties.
[0049] The present invention also provides a long-life graphite composite negative electrode material for energy storage, which is prepared according to the above-mentioned method for preparing the long-life graphite composite negative electrode material for energy storage.
[0050] Since the long-life graphite composite negative electrode material for energy storage adopts all the technical solutions of all the above embodiments, it has at least all the beneficial effects brought by the technical solutions of the above embodiments, which will not be described one by one here.
[0051] The present invention also proposes an application of a long-life graphite composite negative electrode material for energy storage in a lithium-ion battery. The long-life graphite composite negative electrode material for energy storage includes the aforementioned long-life graphite composite negative electrode material for energy storage.
[0052] Since the present application adopts all the technical solutions of all the above embodiments, it has at least all the beneficial effects brought by the technical solutions of the above embodiments, which will not be described one by one here.
[0053] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only used to explain the present invention, and are not used to limit the present invention.
[0054] Example 1
[0055] This embodiment provides a long-life graphite composite negative electrode material for energy storage, and the preparation method thereof comprises the following steps:
[0056] Step S10:
[0057] 100 g of oil-based needle coke and 3 g of pyrrole were added to a ball mill and mixed evenly, and then briquetting was performed at a pressure of 30 MPa, and then the temperature was raised to 700°C for shallow calcination for 3 h in a nitrogen atmosphere, and then the temperature was raised to 2700°C for low-temperature graphitization for 12 h to obtain a graphite precursor material;
[0058] Step S20:
[0059] 10 g of naphthylamine, 10 g of trifluoroethyl acrylate and 100 g of urea-formaldehyde resin were added to 1000 g of ethanol and dispersed evenly, and spray-dried (inlet temperature 150°C, outlet temperature 80°C, flow rate 0.1 kg / h, time 1 h) to obtain a coating material;
[0060] Step S30:
[0061] 110 g of the coating material was added to 5500 g of N-methylpyrrolidone organic solvent and dispersed evenly to a concentration of 2wt%. Then, 1000 g of graphite precursor material was added and dispersed evenly. The residue was filtered and vacuum dried at 80°C for 24 h. The temperature was then raised to 900°C and water vapor (flow rate 500 mL / min) was introduced to activate pores for 2 h. The temperature was then raised to 1300°C and methane gas (flow rate 50 mL / min) was introduced to carbonize for 3 h to obtain a long-life graphite composite negative electrode material for energy storage.
[0062] Example 2
[0063] This embodiment provides a long-life graphite composite negative electrode material for energy storage, and the preparation method thereof comprises the following steps:
[0064] Step S10:
[0065] 100 g of petroleum coke and 1 g of furan were added to a ball mill and mixed evenly, and then briquetted at a pressure of 10 MPa, and then heated to 600 °C in a nitrogen atmosphere for shallow calcination for 6 h, and then heated to 2600 °C for low-temperature graphitization for 24 h to obtain a graphite precursor material;
[0066] Step S20:
[0067] 5 g of benzylamine, 5 g of hexafluorobutyl acrylate, and 100 g of melamine formaldehyde resin were added to 1000 g of ethanol and dispersed evenly, and spray-dried (inlet temperature 150°C, outlet temperature 80°C, flow rate 0.1 kg / h, time 1 h) to obtain a coating material;
[0068] Step S30:
[0069] 110 g of the coating material was added to 11000 g of N-methylpyrrolidone organic solvent and dispersed evenly and configured to a concentration of 1 wt%. Then, 1000 g of graphite precursor material was added and dispersed evenly. The residue was filtered and vacuum dried at 80°C for 24 h. The temperature was then raised to 800°C and water vapor (flow rate 300 mL / min) was introduced to activate pores for 3 h. The temperature was then raised to 1200°C and ethylene gas (flow rate 50 mL / min) was introduced to carbonize for 6 h to obtain a long-life graphite composite negative electrode material for energy storage.
[0070] Example 3
[0071] This embodiment provides a long-life graphite composite negative electrode material for energy storage, and the preparation method thereof comprises the following steps:
[0072] Step S10:
[0073] 100g of coal-based pitch coke and 5g of thiophene were added to a ball mill and mixed evenly, and then briquetting was performed at a pressure of 50Mpa, and then the temperature was raised to 800°C for shallow calcination for 1h in a nitrogen atmosphere, and then the temperature was raised to 2800°C for low-temperature graphitization for 6h to obtain a graphite precursor material;
[0074] Step S20:
[0075] 15 g of N-methylaniline, 15 g of pentafluorophenyl benzoate, and 100 g of polyurethane resin were added to 1000 g of ethanol and dispersed evenly, and spray-dried (inlet temperature 150°C, outlet temperature 80°C, flow rate 0.1 kg / h, time 1 h) to obtain a coating material;
[0076] Step S30:
[0077] 130 g of the coating material was added to 2600 g of N-methylpyrrolidone organic solvent and dispersed evenly and configured to a concentration of 5 wt%. Then, 1000 g of graphite precursor material was added and dispersed evenly, filtered, and the filter residue was vacuum dried at 80°C for 24 h, then heated to 1000°C and water vapor (flow rate 800 mL / min) was introduced to activate pores for 1 h, and then heated to 1500°C and acetylene gas (flow rate 200 mL / min) was introduced to carbonize for 1 h to obtain a long-life graphite composite negative electrode material for energy storage.
[0078] Comparative Example 1
[0079] This comparative example provides a long-life graphite composite negative electrode material for energy storage, and its preparation method is similar to the preparation method in Example 1, except that: naphthylamine and trifluoroethyl acrylate are not added in step S20.
[0080] Comparative Example 2
[0081] This comparative example provides a long-life graphite composite negative electrode material for energy storage, and its preparation method is similar to the preparation method in Example 1, except that: step S20 does not perform water vapor pore formation and does not perform carbon source gas coating;
[0082] The detailed preparation process is:
[0083] Step S20:
[0084] 10g of naphthylamine, 10g of trifluoroethyl acrylate and 100g of urea-formaldehyde resin were added to 1000g of ethanol and dispersed evenly, and spray-dried (inlet temperature 150°C, outlet temperature 80°C, flow rate 0.1kg / h, time 1h) to obtain a coating material; then the obtained coating material was added to 5500g of N-methylpyrrolidone organic solvent, dispersed evenly and configured to a concentration of 2wt%, and then 1000g of graphite precursor material was added and dispersed evenly, filtered, and the obtained filter residue was vacuum dried at 80°C for 24h, and then heated to 1100°C for carbonization for 3h to obtain a long-life graphite composite negative electrode material for energy storage.
[0085] Comparative Example 3
[0086] This comparative example provides a long-life graphite composite negative electrode material for energy storage, and its preparation method is similar to the preparation method in Example 1, except that: no polyurethane resin is added in step S20.
[0087] Performance Testing
[0088] (1) SEM test
[0089] The long-life graphite composite negative electrode material for energy storage prepared in Example 1 was subjected to SEM testing, and the results are as follows: Figure 2 As shown. Figure 2 It can be seen that the material presents a single particle structure with a particle size between 10 and 15 μm.
[0090] (2) Physical and chemical properties test
[0091] The specific surface areas of the graphite composite materials in Examples 1 to 3 and Comparative Examples 1 to 3 were tested according to the test method in the standard GB / T-24533-2019 "Graphite Anode Materials for Lithium Ion Batteries". The diffusion coefficient of the powder material was tested by GITT; the resistivity of the powder was tested by a four-probe tester; the OI value of the powder and its interlayer spacing were tested by XRD; the test results are shown in Table 1.
[0092] Table 1 Physical and chemical properties of long-life graphite composite negative electrode materials for energy storage in Examples 1 to 3 and Comparative Examples 1 to 3
[0093]
[0094] It can be seen from Table 1 that the diffusion coefficients of the graphite composite materials prepared in Examples 1 to 3 and their powder OI values are significantly better than those in Comparative Examples 1 to 3. The reason is that the pores in the material improve the isotropy of the material, and amorphous carbon is filled in the pores to reduce the impedance and its OI value. At the same time, the porous structure of the inner core improves the specific surface area of the material and improves the diffusion coefficient of the material.
[0095] (3) Button battery test
[0096] The graphite composite materials prepared in Examples 1 to 3 and the long-life graphite composite negative electrode materials for energy storage in Comparative Examples 1 to 3 were respectively assembled into button batteries according to the following method: The long-life graphite composite negative electrode materials for energy storage prepared in Examples 1 to 3 and Comparative Examples 1 to 3 were used as negative electrodes, and were assembled into button batteries with lithium sheets, electrolytes and diaphragms in a glove box with argon and water content less than 0.1 ppm. Among them, the diaphragm was celegard 2400; the electrolyte was a solution of LiPF6, in which the concentration of LiPF6 was 1 mol / L, and the solvent was a mixed solution obtained by mixing ethylene carbonate (EC) and diethyl carbonate (DMC) in a weight ratio of 1:1.
[0097] The button batteries were tested for their performance using a blue battery tester. The test conditions were: 0.1C rate charge and discharge, voltage range 0.005~2 V, and stop after 3 cycles. Then the discharge capacity under 1C was tested, and the 1C / 0.1C rate performance and cycle performance (25±3℃, 0.2C / 0.2C, 100 weeks) were calculated. The test results are shown in Table 2.
[0098] Table 2 Performance of button cells using the long-life graphite composite negative electrode materials for energy storage in Examples 1 to 3 and Comparative Examples 1 to 3
[0099]
[0100] It can be seen from Table 2 that the discharge capacity and first efficiency of the button cells using the graphite composite materials of Examples 1 to 3 are significantly higher than those of Comparative Examples 1 to 3. The experimental results show that the reason is that the graphite materials of the examples have a low degree of graphitization and a large interlayer spacing, which improves the cycle performance.
[0101] (4) Soft pack battery performance test
[0102] The long-life graphite composite negative electrode materials for energy storage of Examples 1 to 3 and Comparative Examples 1 to 3 were used as negative electrode active materials, and assembled into 5Ah soft-pack batteries with positive electrode active materials such as lithium iron phosphate, electrolyte and diaphragm. The diaphragm was celegard 2400, and the electrolyte was LiPF6 solution (the solvent was a mixed solution of EC and DEC with a volume ratio of 1:1, and the concentration of LiPF6 was 1.1 mol / L). The prepared soft-pack batteries were tested for cycle and rate performance, and the test results are detailed in Table 3.
[0103] It should be noted that the cycle performance refers to the 500-cycle performance of the battery tested at a charge and discharge rate of 1C / 1C, a voltage range of 2.5V-3.65V, and a temperature of 25±3℃;
[0104] Table 3 Cycling performance of batteries using the long-life graphite composite negative electrode materials for energy storage in Examples 1 to 3 and Comparative Examples 1 to 3
[0105]
[0106] Table 3 shows the cycle performance of the soft-pack battery prepared from the obtained graphite composite material. It can be seen from the table that the cycle performance of the battery in the embodiment is significantly better than that of the comparative example. The reason is that the graphite composite material obtained in the embodiment has a large interlayer spacing to reduce expansion and its doping with heteroatoms improves the electronic conductivity of the material and improves the structural stability of the material. At the same time, the material in the embodiment has a high diffusion coefficient and a low powder OI value, which reduces expansion and improves fast charging performance, and further improves the cycle performance.
[0107] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent structural changes made by using the contents of the present invention specification under the inventive concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.
Claims
1. A method for preparing a long-life graphite composite negative electrode material for energy storage, characterized in that: The following steps are involved: S10. adding the coke raw material and the heteroatom compound to a ball mill, mixing, pressing, calcining, and graphitizing to obtain a graphite precursor material; S20. The amine compound, the organic fluorine compound, the amino resin and the organic solvent are mixed and dried to obtain a coating material; S30. The graphite precursor material, the coating material and the solvent are mixed, filtered, vacuum dried, introduced with water vapor to activate pore formation, and heated to obtain a long-life graphite composite negative electrode material for energy storage; Among them, the mass ratio of coke raw material to heteroatom compound is 100:(1~5); The mass ratio of the amine compound, the organic fluorine compound, the amino resin and the organic solvent is (5-15): (5-15): 100: 1000; The amine compound includes at least one of naphthylamine, benzylamine, N-methylaniline, phenylhydrazine and benzylaniline; The organic fluorine compound includes at least one of trifluoroethyl acrylate, hexafluorobutyl acrylate, pentafluorophenyl benzoate and difluoromethyl trifluoromethanesulfonate; The amino resin includes at least one of urea-formaldehyde resin, melamine-formaldehyde resin, polyurethane resin and polyamide resin; The heteroatom compound includes at least one of pyrrole, furan, thiophene, pyridine, pyrimidine and quinoline; In step S10, the pressing pressure is 10-50 MPa; In step S10, the calcination temperature is 600-800°C, and the calcination time is 1-6 hours; In step S10, the graphitization temperature is 2600-2800°C, and the graphitization time is 6-24 hours; In step S30, the mass ratio of the graphite precursor material, the coating material and the solvent is 100: (11-13): (260-1100); In step S30, the activation pore-forming temperature is 800-1000°C, and the activation pore-forming time is 1-3 h; In step S30, the temperature of heating carbonization is 1200° C., 1300° C. or 1500° C., and the duration of heating carbonization is 1 to 6 hours.
2. The method for preparing a long-life graphite composite negative electrode material for energy storage according to claim 1, characterized in that: The coke raw material includes at least one of oil-based needle coke, coal-based needle coke, petroleum coke and coal-based pitch coke.
3. The method for preparing a long-life graphite composite negative electrode material for energy storage according to claim 1, characterized in that: The organic solvent includes at least one of ethanol, diethyl ether and 1,3-butanediol.
4. A long-life graphite composite negative electrode material for energy storage, characterized in that: The long-life graphite composite negative electrode material for energy storage is prepared according to the method for preparing the long-life graphite composite negative electrode material for energy storage according to any one of claims 1 to 3.
5. Application of a long-life graphite composite negative electrode material for energy storage in a lithium-ion battery, characterized in that: The long-life graphite composite negative electrode material for energy storage includes the long-life graphite composite negative electrode material for energy storage according to claim 4.