A circuit board electrolytic etching solution and its preparation method and application
Through electrolytic etching solution and pulse current technology, the problems of circuit board miniaturization and copper recycling are solved, efficient line etching and copper recycling are achieved, the service life of the etching solution is extended, production costs are reduced and safety is improved.
Patent Information
- Application Number
- CN202411062830.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-08-05
AI Technical Summary
Existing chemical etching solutions are difficult to meet the needs of miniaturization and functional diversification in circuit board production, and the etching solutions have a short service life, high recycling costs, and the risk of environmental pollution.
Electrolytic etching solution is used to etch circuit boards by electrolysis, combined with compound shore protection agent and pulse current, to achieve fine line etching and copper recovery, extend the service life of the etching solution, and reduce production costs.
It achieves etching of fine lines on circuit boards, with a copper recovery rate of over 80%, extending the service life of the electrolytic etching solution, reducing production costs, and improving the handling safety of the etching solution.
Smart Images

Figure CN118563400B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of printed circuit boards, and in particular to a circuit board electrolytic etching solution and a preparation method and application thereof. Background Art
[0002] Circuit boards are important components of electronic products. They are mainly used as carriers of electronic components to achieve electrical interconnection between electronic components. They are widely used in computers, mobile phones, automobiles, aerospace and military.
[0003] Circuit etching is a key step in the production process of circuit boards. Chemical etching is usually the main method. The principle is to use chemical reagents to etch away the exposed copper on the substrate without the anti-corrosion film through redox reaction, and retain the copper covered by the anti-corrosion film, thereby forming the required circuit. At present, the etching solutions used in circuit board production are mainly copper chloride / hydrochloric acid type and copper chloride / ammonium chloride type.
[0004] With the miniaturization, thinness, diversification of functions and high-speed operation of electronic products, in order to meet these special needs of electronic products, the development and innovation of circuit boards have shown extremely rich changes. The types of circuit board materials have increased, and the line width has become smaller and smaller. When the circuit is made, the physical and chemical properties of the copper layer that is etched away are gradually differentiated. These changes have a greater impact on chemical etching based on redox chemical reactions.
[0005] In addition, since part of the elemental copper in the chemical etching solution is oxidized to monovalent copper during the reaction process, as monovalent copper accumulates, the etching solution will lose its etching ability after a period of use. From the perspective of environmental protection, the chemical etching solution that has lost its etching ability should be recycled. At present, the recycling of etching solution mainly includes: recycling copper, recycling cuprous oxide, recycling cupric oxide, recycling copper sulfate, recycling cuprous chloride, and recycling cupric chloride. The various recycled copper products have great economic value and can be used not only in the electroplating process and etching process in the circuit board manufacturing process, but also in other production fields. However, the cost of waste liquid treatment is high, the technology is not very mature, and there is a risk of chlorine gas overflow during the treatment process.
[0006] In summary, if a circuit manufacturing technology that integrates fine circuit etching and copper recycling can be developed, it will be of great significance to the promotion of circuit etching technology. Summary of the invention
[0007] The circuit board etching method using an electrolytic etching solution of the present invention uses an electrolytic method to etch the circuit to replace the traditional chemical etching, which can meet the quality requirements of fine circuits of the circuit board, and can also recover the metal copper in the etching solution while etching the fine circuits of the circuit board. During production, the cathode copper recovery rate can exceed 80%, which is beneficial to prolonging the service life of the electrolytic etching solution and reducing the production cost.
[0008] Specifically, a circuit board electrolytic etching solution includes the following components:
[0009] Methanesulfonic acid 50-200g / L;
[0010] Copper methanesulfonate 30-90g / L;
[0011] Ferric chloride 2-6g / L;
[0012] Dispersant 0.01-0.1g / L;
[0013] Wetting agent 0.1-1g / L;
[0014] Shore protection agent 10-50g / L;
[0015] Water balance;
[0016] The bank protection agent comprises 1,2,4-triazole, diaminobenzothiazole and cyclohexanehexol hexaphosphate.
[0017] Preferably, in the bank protection agent, the mass ratio of 1,2,4-triazole, diaminobenzothiazole, and cyclohexane hexaphosphate is 1:(1.5-2.5):(1.5-2.5). Further, in the bank protection agent, the mass ratio of 1,2,4-triazole, diaminobenzothiazole, and cyclohexane hexaphosphate is 1:2:2.
[0018] More preferably, the bank protection agent is a compound of 1,2,4-triazole, diaminobenzothiazole and cyclohexanehexol hexaphosphate with ethanol and water.
[0019] More preferably, in the bank protection agent, the mass of ethanol is 15-25 times the total mass of 1,2,4-triazole, diaminobenzothiazole and cyclohexanehexol hexaphosphate, and the mass of water is 90-120 times the total mass of the three. Preferably, the dispersant is selected from at least one of propoxylated propynyl alcohol and glycerol.
[0020] Preferably, the wetting agent is polyethylene glycol with a molecular weight of 1000-20000, such as one or more polyethylene glycols with a molecular weight of 1000, 2000, 4000, 6000, 8000, 10000, and 20000.
[0021] The method for preparing the above-mentioned circuit board electrolytic etching solution comprises the following steps:
[0022] a. Add methanesulfonic acid to an appropriate amount of water and mix to dissolve;
[0023] b. adding copper methanesulfonate to the solution obtained in step a and mixing and dissolving;
[0024] c. Add ferric chloride to the solution obtained in step b and mix and dissolve;
[0025] d. The wetting agent is added to the solution obtained in step c and mixed and dissolved;
[0026] e. Add the revetment agent to the solution obtained in step d and mix and dissolve;
[0027] f. Add the dispersant to the solution obtained in step e to mix and dissolve, and add water to the standard volume to obtain the circuit board electrolytic etching solution.
[0028] Furthermore, the present invention also provides a circuit board electrolytic etching method. In a vertical continuous electrolysis device, the above-mentioned circuit board electrolytic etching solution is used as the electrolytic etching solution, the circuit board to be electrolytically etched after the circuit development is completed is used as the anode, and the stainless steel plate or titanium plate is used as the cathode, and etching is performed using positive and reverse pulse currents.
[0029] Preferably, the area ratio of the anode to the cathode is 1: (1-5); the current density is calculated based on the anode area, and the anode forward current density ranges from 0.5A to 2A / dm 2 , the ratio of forward current density to reverse current density is 1:(0.8-1.2), and the ratio of forward current to reverse current time (milliseconds) is (15-30) ms:1ms. More preferably, the ratio of forward current density to reverse current density is 1:1, and the ratio of forward current to reverse current time is 20ms:1ms.
[0030] Preferably, the electrolytic etching solution circulates and is sprayed on the etching surface of the circuit board perpendicular to the anode.
[0031] Preferably, the etching temperature of the electrolytic etching solution is 15-35°C.
[0032] The beneficial effect of the present invention is that the circuit board electrolytic etching solution of the present invention can use an electrolytic method to make fine circuits of the circuit board by adding a special compound shore protection agent, coordinating other components, and combining a characteristic pulse current, and can overcome the shortcomings of the chemical etching method when dealing with changes in circuit board materials.
[0033] During the electrolytic etching process using the circuit board electrolytic etching solution, the copper layer on the circuit board that is not covered by the anti-corrosion dry film loses electrons under the action of the electric field and continuously dissolves until the exposed copper layer is completely etched; the bank protection agent has a protective effect on the side wall of the copper wire, inhibits side corrosion under electrochemical resistance, and ensures the shape of the circuit; methanesulfonic acid and ferric chloride can effectively improve the influence of the difference in anode electric field distribution on the etching uniformity of the copper layer; the wetting agent and dispersant can improve the overall uniformity. In addition, during electrolytic etching, the present invention can recover copper in the electrolytic etching solution at the cathode, which is beneficial to prolonging the service life of the electrolytic etching solution and reducing production costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for describing the embodiments.
[0035] Figure 1 This is a metallographic slice diagram of a test circuit board of Example 1 of the present invention;
[0036] Figure 2 This is a metallographic slice diagram of a test circuit board of Comparative Example 1 of the present invention;
[0037] Figure 3 This is a metallographic section diagram of a test circuit board of comparative example 11 of the present invention;
[0038] Figure 4 This is a metallographic slice diagram of a test circuit board of Comparative Example 19 of the present invention;
[0039] Figure 5 This is a metallographic section diagram of the test circuit board of comparative example 21 of the present invention. DETAILED DESCRIPTION
[0040] In order to make the technical scheme of the present invention more clearly understood by those skilled in the art, the following embodiments are listed for illustration. It should be pointed out that the following embodiments do not limit the protection scope of the present invention.
[0041] Unless otherwise specified, the raw materials, reagents or devices used in the following examples can be obtained from conventional commercial sources or by existing known methods.
[0042] The circuit board electrolytic etching solutions of Examples 1-9 were prepared according to the following steps and the contents in Table 1 below:
[0043] a. Add methanesulfonic acid to an appropriate amount of water and stir to mix evenly;
[0044] b. Add copper methanesulfonate to the solution obtained in step a, stir to dissolve, and mix well;
[0045] c. Add ferric chloride to the solution obtained in step b, stir to dissolve, and mix well;
[0046] d. Add the wetting agent to the solution obtained in step c and stir to mix evenly;
[0047] e. Add the revetment agent to the solution obtained in step d and stir to mix evenly;
[0048] f. Add the dispersant to the solution obtained in step e, stir to dissolve, and add water to the standard volume to obtain the circuit board electrolytic etching solution.
[0049] In Example 1, 1,2,4-triazole, diaminobenzothiazole, and cyclohexanehexol hexaphosphate are sequentially dissolved in ethanol 15 times the total mass of the three at a mass ratio of 1:1.5:2.5, and diluted with water to 90 times the total mass of the three. The resulting solution is the shore protection agent of Example 1.
[0050] In Example 2, 1,2,4-triazole, diaminobenzothiazole, and cyclohexanehexol hexaphosphate are dissolved in ethanol 25 times their total mass in a mass ratio of 1:2.5:1.5, and diluted with water to 120 times their total mass. The resulting solution is the shore protection agent of Example 2.
[0051] In Example 3-9, 1,2,4-triazole, diaminobenzothiazole, and cyclohexanehexol hexaphosphate are dissolved in ethanol 20 times their total mass in a mass ratio of 1:2:2, and diluted with water to 100 times their total mass. The resulting solution is the shore protection agent of Example 3-9.
[0052] In Examples 1-5, the wetting agent is polyethylene glycol with a molecular weight of 4000, and the dispersant is propoxylated propynyl alcohol; in Examples 6-9, the wetting agent is polyethylene glycol with a molecular weight of 1000 and 10000, each accounting for 50 wt%, and the dispersant is glycerol;
[0053] Table 1 Component contents of the circuit board electrolytic etching solution of Examples 1-9
[0054]
[0055] The circuit board electrolytic etching solutions of the above Examples 1-9 were used for testing circuit board processing respectively, and the processing flow was: substrate→film lamination→exposure→development→electrolytic etching→film removal; wherein the specific method of electrolytic etching is as follows:
[0056] In a vertical continuous electrolysis device, the above-mentioned circuit board electrolytic etching solution is used as the electrolytic etching solution, the circuit board to be electrolytically etched after circuit development is used as the anode, the stainless steel plate is used as the cathode, and the etching is performed using positive and negative pulse currents;
[0057] The electrolytic etching solution exchange adopts the solution circulation + vertical anode spraying method (that is, the electrolytic etching solution circulates and sprays on the circuit board etching surface vertically to the anode);
[0058] The area ratio of anode to cathode is 1:2; the current density is calculated based on the anode area, and the anode forward current density range is 1.0A / dm 2 , the ratio of forward current density to reverse current density is 1:1, the ratio of forward current to reverse current time is 20ms:1ms; the solution temperature is 25°C when the circuit board electrolytic etching solution is electrolyzed.
[0059] The test circuit board samples prepared in Examples 1-9 were tested according to the following performance test method.
[0060] Test method:
[0061] 1. Appearance: Observe the processed circuit surface under a 10x magnifying glass. The circuit surface is qualified if it has uniform color, no obvious over-etching, and no obvious etching impurities.
[0062] 2. Residual copper in the circuit: Take a piece of electrolytically etched circuit board, check it on the AOI machine, and record the number of residual copper points in the circuit;
[0063] 3. Circuit dog teeth: Take a piece of electrolytically etched circuit board, check it on the AOI machine, and record the number of circuit dog teeth points;
[0064] 4. Etching factor: Take the circuit board treated with electrolytic etching, make circuit cross-section slices, and then measure and observe under a metallographic microscope to measure the top length, bottom length and circuit height of the circuit;
[0065] Etching factor = 2 times line height / (line bottom length - line top length) (etching factor is required to be greater than 3);
[0066] 5. Circuit bonding strength: Take the electrolytically etched circuit board and use 3M tape to pull the circuit vertically. If the circuit is not pulled up, it is qualified;
[0067] 6. Copper recovery: The copper recovery rate is calculated by dividing the total mass of copper added to the cathode after electrolytic etching by the total mass of copper reduced at the anode;
[0068] The performance test results of the sample circuit boards of Examples 1-9 are shown in Table 2 below:
[0069] Table 2 Performance test results of sample circuit boards of Examples 1-9
[0070]
[0071] Example 1 Test the metallographic section of the circuit board sample Figure 1 shown.
[0072] During the research and development process of the present invention, based on Example 3, circuit board electrolytic etching solutions of Comparative Examples 1-12 for testing were also prepared. The circuit board electrolytic etching solutions of Comparative Examples 1-12 differ from those of Example 3 only in the component contents shown in Table 3;
[0073] Table 3 Content of the circuit board electrolytic etching solution of Comparative Examples 1-12
[0074]
[0075] The circuit board electrolytic etching solutions of comparative examples 1-12 were used for test circuit board processing using the same process as in Example 3 to prepare test circuit boards of comparative examples 1-12, and performance tests were performed on the test circuit boards of comparative examples 1-12. The test results are shown in Table 4 below.
[0076] Table 4 Performance test results of circuit boards of comparative examples 1-12
[0077]
[0078] Comparative Example 1: Metallographic section of the test circuit board Figure 2 As shown; the metallographic section of the test circuit board of comparative example 11 is as follows Figure 3 shown.
[0079] During the research and development process of the present invention, based on Example 3, circuit board electrolytic etching solutions of Comparative Examples 13-22 containing different components for testing were also prepared. The details are as follows:
[0080] Comparative Example 13: The difference from Example 3 is that in the shore protection agent, the mass ratio of 1,2,4-triazole, diaminobenzothiazole, and cyclohexanehexol hexaphosphate is 1:2:7;
[0081] Comparative Example 14: The difference from Example 3 is that in the shore protection agent, the mass ratio of 1,2,4-triazole, diaminobenzothiazole, and cyclohexanehexol hexaphosphate is 1:7:2;
[0082] Comparative Example 15: The difference from Example 3 is that in the shore protection agent, the mass ratio of 1,2,4-triazole, diaminobenzothiazole, and cyclohexanehexol hexaphosphate is 0.1:2:2;
[0083] Comparative Example 16: The difference from Example 3 is that in the shore protection agent, the mass ratio of 1,2,4-triazole, diaminobenzothiazole, and cyclohexanehexol hexaphosphate is 7:2:2;
[0084] Comparative Example 17: The difference from Example 3 is that the bank protection agent does not include cyclohexanehexol hexaphosphate, and the mass ratio of 1,2,4-triazole to diaminobenzothiazole is 1:2;
[0085] Comparative Example 18: The difference from Example 3 is that the bank protection agent does not include diaminobenzothiazole, and the mass ratio of 1,2,4-triazole to cyclohexanehexol hexaphosphate is 1:2;
[0086] Comparative Example 19: The difference from Example 3 is that the shore protection agent does not include 1,2,4-triazole, and the mass ratio of diaminobenzothiazole to cyclohexanehexol hexaphosphate is 2:2;
[0087] Comparative Example 20: The difference from Example 3 is that in the shore protection agent, 1,2,4-triazole is replaced by benzimidazole, and the mass ratio of benzimidazole, diaminobenzothiazole, and cyclohexanehexol hexaphosphate is 1:2:2;
[0088] Comparative Example 21: The difference from Example 3 is that methanesulfonic acid is replaced by hydrochloric acid, and copper methanesulfonate is replaced by copper chloride;
[0089] Comparative Example 22: The difference from Example 3 is that methanesulfonic acid is replaced by formic acid, and copper methanesulfonate is replaced by copper chloride.
[0090] The circuit board electrolytic etching solutions of comparative examples 13-22 were used for test circuit board processing using the same process as in Example 3 to prepare test circuit boards of comparative examples 13-22. The test circuit boards of comparative examples 13-22 were subjected to performance tests, and the test results are shown in Table 5 below:
[0091] Table 5 Performance test results of circuit boards of comparative examples 13-22
[0092]
[0093] Comparative Example 19: Metallographic section of the test circuit board Figure 4 As shown; the metallographic section of the test circuit board of comparative example 21 is as follows Figure 5 shown.
[0094] During the research and development of the present invention, based on Example 3, the effects of different electrolytic etching conditions on the performance of the circuit board were also studied. Specifically, the circuit board electrolytic etching solution prepared in Example 3 was used for the following test circuit board processing of Comparative Examples 23-29 with different electrolytic etching conditions;
[0095] Comparative Example 23: The difference from Example 3 is that in the electrolytic etching, the ratio of the anode area to the cathode area is 1:10;
[0096] Comparative Example 24: The difference from Example 3 is that in the electrolytic etching, the anode to cathode area ratio is 1:0.5;
[0097] Comparative Example 25: The difference from Example 3 is that in the electrolytic etching, the anode forward current density range is 3.0 A / dm 2 ;
[0098] Comparative Example 26: The difference from Example 3 is that in the electrolytic etching, the ratio of the forward current density to the reverse current density is 1:2;
[0099] Comparative Example 27: The difference from Example 3 is that in the electrolytic etching, the time ratio of the forward current to the reverse current is 40ms:1ms;
[0100] Comparative Example 28: The difference from Example 3 is that in electrolytic etching, direct current is used for etching, and the current density is calculated based on the anode area, and the current density is 1A / dm 2 ;
[0101] Comparative Example 29: The difference from Example 3 is that during the electrolytic etching, the temperature of the electrolytic etching solution is 40°C.
[0102] The performance test was performed on the test circuit boards of Comparative Examples 23-29, and the test results are shown in Table 6 below:
[0103] Table 6 Performance test results of circuit boards of comparative examples 23-29
[0104]
[0105] The above descriptions are merely embodiments of the present invention and are not intended to limit the patent scope of the present invention. Any equivalent process changes made using the contents of the present invention's specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection of the present invention.
Claims
1. A circuit board electrolytic etching solution comprising the following components: Methanesulfonic acid 50-200g / L; Copper methanesulfonate 30-90g / L; Ferric chloride 2-6g / L; Dispersant 0.01-0.1g / L; Wetting agent 0.1-1g / L; Shore protection agent 10-50g / L; Water balance; The bank protection agent includes 1,2,4-triazole, diaminobenzothiazole and cyclohexanehexol hexaphosphate; In the bank protection agent, the mass ratio of 1,2,4-triazole, diaminobenzothiazole and cyclohexanehexol hexaphosphate is 1:(1.5-2.5):(1.5-2.5); The bank protection agent is a compound of 1,2,4-triazole, diaminobenzothiazole, cyclohexanehexol hexaphosphate, ethanol and water; In the bank protection agent, the mass of ethanol is 15-25 times the total mass of 1,2,4-triazole, diaminobenzothiazole and cyclohexanehexol hexaphosphate, and the mass of water is 90-120 times the total mass of the three. The dispersant is selected from at least one of propoxylated propynyl alcohol and glycerol; The wetting agent is polyethylene glycol with a molecular weight of 1000-20000.
2. The method for preparing the circuit board electrolytic etching solution according to claim 1, characterized in that: The steps include: a. Add methanesulfonic acid into an appropriate amount of water and mix and dissolve; b. Add copper methanesulfonate to the solution obtained in step a and mix and dissolve; c. Add ferric chloride to the solution obtained in step b and mix and dissolve; d. Add the wetting agent to the solution obtained in step c and mix and dissolve; e. Add the shore protection agent to the solution obtained in step d and mix and dissolve; f. Add the dispersant to the solution obtained in step e to mix and dissolve, and add water to the standard volume to obtain the circuit board electrolytic etching solution.
3. A circuit board electrolytic etching method, characterized in that: In a vertical continuous electrolysis device, the circuit board electrolytic etching solution as claimed in claim 1 is used as the electrolytic etching solution, the circuit board to be electrolytically etched after circuit development is used as the anode, the stainless steel plate or the titanium plate is used as the cathode, and the etching is performed using positive and negative pulse currents; The area ratio of the anode to the cathode is 1: (1-5); the current density is calculated based on the anode area, and the anode forward current density ranges from 0.5A to 2A / dm 2 , the ratio of forward current density to reverse current density is 1:(0.8-1.2), and the ratio of forward current to reverse current time is (15-30)ms:1ms.
4. The circuit board electrolytic etching method according to claim 3, characterized in that: The electrolytic etching solution circulates and is sprayed on the etching surface of the circuit board perpendicular to the anode.
Citation Information
Cited By
Method for preparing PCB (Printed Circuit Board) fine circuit through high-efficiency pulse electrolytic chemical synergy etching
CN119629871A