A sodium ion battery positive electrode material and its preparation method and application

By constructing a coating layer of P2, P3 and tunnel-type three-phase structures on the surface of the core material of the sodium-ion battery cathode material, the problems of structural degradation and capacity attenuation of the layered oxide cathode material in the sodium-ion battery are solved, and a better solution is achieved. High initial discharge specific capacity and cycle stability.

CN118610441BActive Publication Date: 2024-10-18GANZHOU NOVA TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411067010.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-10-18
Estimated Expiration
2044-08-06

AI Technical Summary

Technical Problem

Layered oxide cathode materials in sodium-ion batteries have complex phase transitions during the deintercalation and deintercalation of Na+, the Ginger Taylor effect caused by Mn3+, and poor interfacial stability, resulting in serious structural degradation and too rapid capacity fading, making them unable to meet actual production applications. needs.

Method used

The core material NaNix1Mny1O2 is used as the O3 phase, and a coating layer of P2, P3 and tunnel-type three-phase structures is constructed on its surface. By mixing the precursors of the core material and coating material and sintering with flux, a stable multi-phase structure is formed. Enhance material stability and Na+ diffusion channels.

Benefits of technology

It improves the initial discharge specific capacity and cycle stability of the material, suppresses the capacity fading of the P3-type structure during the charge and discharge process, widens the Na+ diffusion channel, alleviates harmful phase changes, and improves the material performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118610441B_ABST
    Figure CN118610441B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of sodium ion battery materials, and discloses a sodium ion battery positive electrode material and its preparation method and application. The positive electrode material includes a core and a coating layer coated on at least part of the surface of the core; the core is in an O3 phase; the coating material of the coating layer is in a three-phase structure of P2, P3 and tunnel type. By combining the core and the coating layer, the initial specific capacity of the positive electrode material can be increased and harmful phase changes can be alleviated. In addition, the present invention also discloses a preparation method of the above-mentioned sodium ion battery positive electrode material, a mixed core material, Na t Ni x2 Mn y2 M 1‑x2‑y2 The positive electrode material can be obtained by sintering the precursor of the O2 coating material and the flux. The preparation process is simple and controllable, and the cost is low.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of sodium ion battery materials and relates to a positive electrode material, in particular to a sodium ion battery positive electrode material and a preparation method and application thereof. Background Art

[0002] Layered oxide cathode materials have the advantages of low cost, simple preparation method, environmental friendliness, and safe transportation, and are widely used in large-scale energy storage devices. However, there are many problems with layered oxide cathode materials, such as Na + The complex phase transition during the deintercalation process, Mn 3+ The resulting Jan-Taylor effect and poor interface stability lead to serious structural degradation of the positive electrode material of the sodium-ion battery during operation, and the capacity decays too quickly, which cannot meet the needs of actual production applications.

[0003] In the prior art, the commonly used modification methods for these problems are doping and coating. Coating can effectively block the direct contact between the active material and the electrolyte, but it will also increase the Na + The diffusion energy barrier reduces the initial discharge specific capacity of the material. Summary of the invention

[0004] In view of the above problems existing in the prior art, in the first aspect, the present invention provides a positive electrode material for a sodium ion battery; in the second aspect, the present invention provides a method for preparing the positive electrode material for a sodium ion battery; finally, the present invention provides a battery.

[0005] In a first aspect, the present invention provides a sodium ion battery positive electrode material, comprising a core and a coating layer coated on at least a portion of the surface of the core; the chemical expression of the core is NaNi x1 Mn y1 A 1-x1-y1 O2 is an O3 phase, wherein 0.3≤x1≤0.5, 0.3≤y1≤0.5, 1-x1-y1>0, and A is one or more of Fe, Mg, Cu, and Ti; the chemical formula of the coating material of the coating layer is Na t Ni x2 Mn y2 M 1-x2-y2 O2 is a three-phase structure of P2, P3 and tunnel type, among which 0.44≤t≤0.8, 0.3≤x2≤0.7, 0.3≤y2≤0.7, 1-x2-y2>0, and M is one or more of Mo, Zn, Mg, Cu, Ti, Zr, and W.

[0006] In a second aspect, the present invention provides a method for preparing the above-mentioned sodium ion battery positive electrode material, comprising: t Ni x2 Mn y2M 1-x2-y2 The precursor of the O2 coating material and the flux are mixed and sintered.

[0007] Preferably, Na is prepared by the following method t Ni x2 Mn y2 M 1-x2-y2 Precursor of O2 coating material: sodium, nickel, manganese and M elements in sodium source, nickel source, manganese source and M source are mixed according to stoichiometric ratio to obtain mixed powder, oxalic acid solution is added to the mixed powder for reaction and then dried to obtain the Na t Ni x2 Mn y2 M 1-x2-y2 Precursor for O2 coating materials.

[0008] Preferably, the sodium source is any one or more of sodium carbonate, sodium hydroxide, sodium oxalate and sodium carboxylate.

[0009] Preferably, the nickel source is any one or more of nickel hydroxide, nickel oxalate and nickel carboxylate.

[0010] Preferably, the manganese source is any one or more of manganese carbonate, manganese oxalate, manganese dioxide and manganese carboxylate.

[0011] Preferably, when M in the M source is Mo, Zn, Mg, Cu, Ti, or Zr, the M source is any one or more of oxalate, carbonate, or a soluble oxide containing M; when M in the M source is W, the M source is any one or more of tungstic acid or ammonium metatungstate.

[0012] Preferably, the liquid-to-solid ratio of the oxalic acid solution and the mixed powder of the sodium source, nickel source, manganese source and M source is 20-60:1 mL / g.

[0013] Preferably, the concentration of the oxalic acid solution is 4-8 mol / L.

[0014] Preferably, the drying temperature is 70-120° C. and the drying time is 12-24 hours.

[0015] Preferably, the flux is one or both of strontium carbonate and strontium oxide.

[0016] Preferably, the core material, the Na t Ni x2 Mn y2 M 1-x2-y2 The mass ratio of the precursor of the O2 coating material to the flux is 1:5~50%:0.06~0.12%.

[0017] Preferably, in step 2, the high temperature sintering is performed in two stages, and the sintering temperature of the first stage is higher than the sintering temperature of the second stage.

[0018] More preferably, the sintering temperature of the first stage is 700-950° C., and the sintering time is 12-24 h; the sintering temperature of the second stage is 300-500° C., and the sintering time is 10-18 h.

[0019] Finally, the present invention provides a battery, comprising the above-mentioned positive electrode material or the positive electrode material prepared by the above-mentioned method for preparing the positive electrode material.

[0020] Compared with the prior art, one or more technical solutions provided by the present invention have at least one of the following beneficial technical effects:

[0021] (1) The core of the positive electrode material for sodium ion batteries provided by the present invention is in the O3 phase, and the coating material of the coating layer is a mixed three-phase of P2, P3 and tunnel type. The high initial efficiency of the P2 type structure complements the low initial discharge capacity of the tunnel type structure. The tunnel type structure can inhibit the excessive capacity decay of the P3 type structure during the charge and discharge process, and can improve the initial discharge specific capacity and cycle stability of the material. The core and the coating layer cooperate to facilitate the entry of doping elements into the lattice of the core material, enhance the stability of the O3 type material structure, and broaden the Na + Diffusion channel, Na in the coating + It can compensate for the loss of active sodium in the core material during the charging and discharging process and alleviate harmful phase changes.

[0022] (2) The preparation process provided by the present invention only requires mixing the core material, Na t Ni x2 Mn y2 M 1-x2-y2 The positive electrode material can be obtained by sintering the precursor of the O2 coating layer and the flux. The residual alkali remaining on the surface of the core material can be used as a sodium source to firmly build the coating layer on the surface of the positive electrode material, thereby preventing the active material from being further corroded.

[0023] (3) The layered oxide positive electrode material provided by the present invention has high capacity, a simple and controllable preparation process and low cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is a SEM image of the positive electrode material prepared in Example 1;

[0025] Figure 2 is the NaNi used in Example 1 0.3 Mn 0.3 Cu 0.4 XRD pattern of O2 core material;

[0026] Figure 3 XRD diagrams of the positive electrode materials prepared in Example 1 and Example 2;

[0027] Figure 4 The Na obtained in Comparative Example 2 0.65 Ni 0.3 Mn 0.3 W 0.4 XRD pattern of O2 cathode material;

[0028] Figure 5 This is a test chart of the discharge specific capacity of batteries assembled from the positive electrode materials prepared in Examples 1 to 4 and Comparative Examples 1 to 2 provided by the present invention. DETAILED DESCRIPTION

[0029] The present invention provides the following specific technical solutions.

[0030] In a first aspect, the present invention provides a sodium ion battery positive electrode material, comprising a core and a coating layer coated on at least a portion of the surface of the core; the chemical expression of the core is NaNi x1 Mn y1 A 1-x1-y1 O2 is an O3 phase, wherein 0.3≤x1≤0.5, 0.3≤y1≤0.5, 1-x1-y1>0, and A is one or more of Fe, Mg, Cu, and Ti; the chemical formula of the coating material of the coating layer is Na t Ni x2 Mn y2 M 1-x2-y2 O2 is a three-phase structure of P2, P3 and tunnel type, among which 0.44≤t≤0.8, 0.3≤x2≤0.7, 0.3≤y2≤0.7, 1-x2-y2>0, and M is one or more of Mo, Zn, Mg, Cu, Ti, Zr, and W.

[0031] In the existing technology, coating can effectively block the direct contact between active materials and electrolyte, but it will also increase Na + The inventors found that the coating material has three-phase structures of P2, P3 and tunnel type at the same time. The high initial efficiency of the P2 type structure complements the low initial discharge capacity of the tunnel type structure, which greatly improves the Na + The tunnel structure can suppress the problem of too fast capacity decay of the P3 structure during the charge and discharge process, making it have a more stable electrochemical interface, which can improve the initial discharge capacity and cycle stability of the material. The three-phase structure of the coating material and the O3 phase of the core material are conducive to the entry of doped elements into the lattice of the core material, enhancing the stability of the O3 material structure and widening the Na + Diffusion channel, Na in coating material + It can compensate for the loss of active sodium in the core material during the charging and discharging process, alleviate harmful phase changes, and further improve material performance.

[0032] In a second aspect, the present invention provides a method for preparing the above-mentioned sodium ion battery positive electrode material, comprising: t Ni x2 Mn y2 M 1-x2-y2 The precursor of the O2 coating material and the flux are mixed and sintered.

[0033] The inventors have found that the mixed nuclear material and Na t Ni x2 Mn y2 M 1-x2-y2 The precursor of the O2 coating material is sintered, and the residual alkali remaining on the surface of the core material can be used as a sodium source, so that the coating material is firmly constructed on the surface of the positive electrode material, preventing the active material from being further corroded.

[0034] Preferably, Na is prepared by the following method t Ni x2 Mn y2 M 1-x2-y2 Precursor of O2 coating material: sodium, nickel, manganese and M elements in sodium source, nickel source, manganese source and M source are mixed according to stoichiometric ratio to obtain mixed powder, oxalic acid solution is added to the mixed powder for reaction and then dried to obtain the Na t Ni x2 Mn y2 M 1-x2-y2 Precursor for O2 coating materials.

[0035] Preferably, the sodium source is any one or more of sodium carbonate, sodium hydroxide, sodium oxalate and sodium carboxylate.

[0036] Preferably, the nickel source is any one or more of nickel hydroxide, nickel oxalate and nickel carboxylate.

[0037] Preferably, the manganese source is any one or more of manganese carbonate, manganese oxalate, manganese dioxide and manganese carboxylate.

[0038] Preferably, when M in the M source is Mo, Zn, Mg, Cu, Ti, or Zr, the M source is any one or more of oxalate, carbonate, or a soluble oxide containing M; when M in the M source is W, the M source is any one or more of tungstic acid or ammonium metatungstate.

[0039] Preferably, the liquid-to-solid ratio of the oxalic acid solution and the mixed powder of the sodium source, nickel source, manganese source and M source is 20:1-60:1 mL / g.

[0040] Preferably, the concentration of the oxalic acid solution is 4-8 mol / L.

[0041] Preferably, the flux is one or both of strontium carbonate and strontium oxide.

[0042] Preferably, the core material, the Na t Ni x2 Mn y2 M 1-x2-y2 The mass ratio of the precursor of the O2 coating material to the flux is 1:5~50%:0.06~0.12%.

[0043] Preferably, the high temperature sintering is a two-stage sintering, and the sintering temperature of the first stage is higher than the sintering temperature of the second stage.

[0044] The inventors have found through research that the first stage of sintering allows the raw materials to melt together and the ions to diffuse into each other to form a coating material. Lowering the sintering temperature in the second stage of sintering is beneficial to the formation of P2, P3, and tunnel-type multi-phases in the coating material.

[0045] More preferably, the sintering temperature of the first stage is 700-950° C., and the sintering time is 12-24 h; the sintering temperature of the second stage is 300-500° C., and the sintering time is 10-18 h.

[0046] Finally, the present invention provides a battery, comprising the above-mentioned positive electrode material or the positive electrode material prepared by the above-mentioned method for preparing the positive electrode material.

[0047] In order to make the technical problems to be solved, technical solutions and technical advantages of the present invention more clear, they will be described in detail below with reference to specific examples, but the protection scope of the present invention is not limited to the following specific embodiments.

[0048] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.

[0049] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.

[0050] Embodiment 1:

[0051] A method for preparing a sodium positive electrode material comprises the following steps:

[0052] Step 1, weigh Na2CO3, Ni(OH)2, MnO2, H2WO4 according to the molar ratio of sodium, nickel, manganese, and tungsten atoms of 6.5:3:3:4 and mix them evenly to obtain a mixed powder B. Take 10g of the mixed powder B and add it to 200mL of 4mol / L oxalic acid solution, stir evenly, and after the reaction is completed (no more gas is generated), transfer it to a drying oven at 120°C and dry it for 8h to obtain a precursor of the coating layer.

[0053] Step 2, take 5gNaNi 0.3 Mn 0.3 Cu 0.4 O2 core material, 1.5g coating layer precursor, 0.006g strontium carbonate, mixed in a ball mill for 1 hour (rotation speed 300rpm), placed in a muffle furnace at 825℃ for 16h, then cooled to 450℃ at a rate of 3℃ / min, kept for 12h, and finally cooled to room temperature with the furnace to obtain a sodium ion battery positive electrode material with a multi-phase coating layer, the chemical formula of which is: NaNi 0.3 Mn 0.3 Cu 0.4 O2@Na 0.65 Ni 0.3 Mn 0.3 W 0.4 O2.

[0054] Figure 1 is a SEM image of the positive electrode material obtained in Example 1. Figure 1 It can be observed that the positive electrode material prepared by the preparation method provided by the present invention is in block shape and has good coating condition.

[0055] Figure 2 is the NaNi used in Example 1 0.3 Mn 0.3 Cu 0.4 XRD pattern of O2 core material, Figure 2 It can be seen that the NaNi provided by the present invention x1 Mn y1 A 1-x1-y1 The O2 core material is in the O3 phase.

[0056] Embodiment 2:

[0057] The difference from Example 1 is that in step 2, NaNi 0.3 Mn 0.3 Cu 0.4 The O2 core material, the precursor of the coating layer and strontium carbonate are kept at 825℃ in a muffle furnace for 16 hours and then cooled with the furnace to obtain the positive electrode material, whose chemical formula is: NaNi 0.3 Mn 0.3 Cu 0.4 O2@Na 0.65 Ni 0.3 Mn 0.3 W 0.4 O2.

[0058] Figure 3 is the XRD diagram of the positive electrode materials prepared in Example 1 and Example 2, Figure 3It can be seen that the positive electrode materials prepared in Example 1 and Example 2 both have four crystal phase structures of O3, P2, P3 and tunnel type. Comparing the XRD curves of the positive electrode materials prepared in Example 1 and Example 2, it can be seen that the three-phase peaks of P2, P3 and tunnel type in the positive electrode material prepared in Example 1 are stronger, indicating that the two-stage sintering process provided by the present invention is more conducive to generating a mixed three-phase structure of P2, P3 and tunnel type.

[0059] Combination Figure 3 The XRD curve of the positive electrode material prepared in Example 1 and Figure 2 The XRD curve of the core material used in Example 1 can indirectly prove that the coating material of the positive electrode material is a mixed three-phase structure of P2, P3 and tunnel type.

[0060] Embodiment 3:

[0061] Step 1, weigh Na2CO3, Ni(OH)2, MnO2, and MoO3 according to the molar ratio of sodium, nickel, manganese, and molybdenum of 6.5:3.5:3.5:3, and mix them evenly to obtain a mixed powder B. Take 5g of the mixed powder B and add it to 100mL of 4mol / L oxalic acid solution, stir evenly, and after the reaction is completed (no more gas is generated), transfer it to a drying oven at 70°C and dry it for 8h to obtain a precursor of the coating layer.

[0062] Step 2, take 5gNaNi 0.3 Mn 0.3 Mg 0.4 O2 core material, 0.25g coating layer precursor, 0.003g strontium oxide, mixed in a ball mill for 1 hour (rotation speed is 300rpm), placed in a muffle furnace at 950℃ for 12h, then cooled to 500℃ at a rate of 3℃ / min, kept for 10h, and finally cooled to room temperature with the furnace to obtain a sodium ion battery positive electrode material with a multi-phase coating layer, whose chemical formula is: NaNi 0.4 Mn 0.4 Mg 0.2 O2@Na 0.65 Ni 0.35 Mn 0.35 Mo 0.3 O2.

[0063] Embodiment 4:

[0064] Step 1, weigh Na2CO3, Ni(OH)2, MnO2, and MgC2O4 according to the molar ratio of sodium, nickel, manganese, and magnesium of 6.1:3.7:3.7:2.6, and mix them evenly to obtain a mixed powder B, add 5 g of the mixed powder B to 100 mL of 4 mol / L oxalic acid solution, stir evenly, and after the reaction is completed (no more gas is generated), transfer to a drying oven at 120°C and dry for 8 hours to obtain a precursor of the coating layer.

[0065] Step 2, take 5gNaNi 0.3 Mn 0.3 Fe 0.4 O2 core material, 2.5g coating layer precursor, 0.004g strontium carbonate, mixed in a ball mill for 1 hour (rotation speed 300rpm), placed in a 700℃ muffle furnace for 12h, then cooled to 300℃ at a rate of 3℃ / min, kept for 10h, and finally cooled to room temperature with the furnace to obtain a sodium ion battery positive electrode material with a multi-phase coating layer, the chemical formula of which is: NaNi 0.33 Mn 0.33 Fe 0.34 O2@Na 0.61 Ni 0.37 Mn 0.37 Mg 0.26 O2.

[0066] Comparative Example 1:

[0067] A sodium positive electrode material, NaNi used in Example 1 0.3 Mn 0.3 Cu 0.4 The O2 core material is the positive electrode material.

[0068] Comparative Example 2:

[0069] Step 1: weigh Na2CO3, Ni(OH)2, MnO2, and H2WO4 according to the molar ratio of sodium, nickel, manganese, and tungsten of 6.5:3:3:4, and mix them evenly to obtain mixed powder B. Add 10g of mixed powder A to 200mL of oxalic acid solution with a concentration of 4mol / L, stir evenly, and transfer to a drying oven at 120°C for 8h after the reaction is completed (no more gas is produced) to obtain a precursor. Then place the precursor in a muffle furnace at 750°C for 16h, then cool it to 450°C at a rate of 3°C / min, keep it warm for 12h, and finally cool it to room temperature with the furnace to obtain a sodium ion battery positive electrode material with tunnel type, P2 type, and P3 type three-phase, and its chemical formula is: Na 0.65 Ni 0.3 Mn 0.3 W 0.4 O2.

[0070] Figure 4 The Na obtained in Comparative Example 2 0.65 Ni 0.3 Mn 0.3 W 0.4 XRD pattern of O2 cathode material, Figure 4It can be seen that the positive electrode material prepared in Comparative Example 2 has three crystalline phase structures of P2, P3 and tunnel type, which can further confirm that the coating layer of the positive electrode material provided by the present invention has three crystalline phase structures of P2, P3 and tunnel type.

[0071] The positive electrode materials prepared in Examples 1 to 4 and Comparative Examples 1 to 2 were assembled into batteries in the following manner:

[0072] In a clean room with humidity below 10%, 0.4g of positive electrode material, 0.5g of polyvinylidene fluoride (PVDF) and 0.5g of acetylene black were weighed, and the three materials were ground in a mortar for 10 minutes, and then 2mL of N-methylpyrrolidone was dripped into them to make them completely dissolved, and then evenly coated on the surface of the Al foil with a scraper. The aluminum foil was then placed in a vacuum oven at 90°C and dried for 10 hours. After drying, the active substance on the aluminum foil was about 3mg / cm 2 , and then transferred to a cutting machine to make a circular electrode with a diameter of 12 mm. The sodium metal sheet was used as the anode of the battery, the electrolyte was NC-019 model NaClO4, and the porous glass fiber (Whatman, GF / D) was used as the diaphragm. The button battery was assembled in a glove box filled with argon.

[0073] The batteries assembled from the positive electrode materials prepared in Examples 1 to 4 and Comparative Examples 1 to 2 were tested at 25° C., a voltage of 2 to 4 V, and a rate of 1C. Figure 5 The discharge capacity test diagram of the battery assembled from the positive electrode materials prepared in Examples 1 to 4 and Comparative Examples 1 to 2 is shown in FIG. Figure 5 It can be seen that the battery assembled from the positive electrode material provided by the present invention has a higher initial specific capacity and improved cycle stability.

[0074] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A sodium ion battery cathode material, It is characterized in that It comprises a core and a coating layer coated on at least a portion of the surface of the core; the chemical expression of the core is NaNi x1 Mn y1 A 1-x1-y1 O 2 , is an O3 phase, wherein 0.3≤x1≤0.5, 0.3≤y1≤0.5, 1-x1-y1>0, A is any one or more of Fe, Mg, Cu, and Ti; the chemical formula of the coating material of the coating layer is Na t Ni x2 Mn y2 M 1-x2-y2 O 2 , which is a three-phase structure of P2, P3 and tunnel type, among which 0.44≤t≤0.8, 0.3≤x2≤0.7, 0.3≤y2≤0.7, 1-x2-y2>0, and M is any one or more of Mo, Zn, Mg, Cu, Ti, Zr, and W.

2. The method for preparing the positive electrode material for a sodium ion battery according to claim 1, It is characterized in that include: The nuclear material, Na t Ni x2 Mn y2 M 1-x2-y2 O 2 The precursor of the cladding material and the flux are mixed and sintered; The flux is one or both of strontium carbonate and strontium oxide; The core material, the Na t Ni x2 Mn y2 M 1-x2-y2 O 2 The mass ratio of the precursor of the coating material to the flux is 1:5%~50%:0.06%~0.12%; Na was prepared by the following method t Ni x2 Mn y2 M 1-x2-y2 O 2 Precursor of coating material: sodium, nickel, manganese and M elements in sodium source, nickel source, manganese source and M source are mixed in stoichiometric ratio to obtain mixed powder, oxalic acid solution is added to the mixed powder for reaction and then dried to obtain the Na t Ni x2 Mn y2 M 1-x2-y2 O 2 Precursors of coating materials; The liquid-to-solid ratio of the oxalic acid solution to the mixed powder of the sodium source, nickel source, manganese source and M source is 20-60:1 mL / g; the concentration of the oxalic acid solution is 4-8 mol / L; The sintering is carried out in two stages. The sintering temperature of the first stage is 700-950° C. and the sintering time is 12-24 hours. The sintering temperature of the second stage is 300-500° C. and the sintering time is 10-18 hours.

3. The method for preparing the positive electrode material for a sodium ion battery according to claim 2, It is characterized in that The sodium source is any one or more of sodium carbonate, sodium hydroxide, sodium oxalate, and sodium carboxylate; the nickel source is any one or more of nickel hydroxide, nickel oxalate, and nickel carboxylate; the manganese source is any one or more of manganese carbonate, manganese oxalate, manganese dioxide, and manganese carboxylate; when M in the M source is Mo, Zn, Mg, Cu, Ti, or Zr, the M source is any one or more of oxalate, carbonate, and soluble oxide containing M; when M in the M source is W, the M source is any one or more of tungstic acid or ammonium metatungstate.

4. A battery, It is characterized in that The positive electrode material comprises the positive electrode material according to claim 1 or the positive electrode material prepared by the preparation method of the positive electrode material according to any one of claims 2 to 3.

Citation Information

Patent Citations

  • Na2MnPO4F coated O3 type layered sodium ion battery positive electrode material and preparation method thereof

    CN115763766A

  • Core-shell structure sodium ion battery positive electrode material and preparation method and application thereof

    CN117976884A