A method for improving the activity of blast furnace hearth

By calculating the permeability index of the furnace cylinder and adjusting the molten iron composition and blast furnace operating parameters, the problem of hysteresis of the blast furnace cylinder activity judgment is solved, the furnace cylinder stability and production efficiency are improved, and energy consumption and cost are reduced.

CN118638975BActive Publication Date: 2024-11-01山西建龙实业有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411076888.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-01
Estimated Expiration
2044-08-07

AI Technical Summary

Technical Problem

The prior art has a hysteresis when judging the activity of blast furnace cylinders, resulting in missed the optimal time for adjustment treatment, resulting in a decrease in the activity of the furnace cylinders, causing problems such as suspended materials, air outlet damage, and reduced blast furnace production efficiency, energy consumption and cost increase. .

Method used

By calculating the liquid permeability index of the dead material column of the furnace cylinder, combining the physical heat THM of molten iron and the composition, adjusting the coke ratio, coal ratio, coke mass, spray coal particle size, air outlet structure, fabric sequence and slag composition to ensure the carbon content of molten iron At 4.50-5.00%, the physical heat is between 1490-1510℃, and the ratio of silicon, sulfur, magnesium and aluminum are controlled, the air volume and wind speed are optimized, and the liquid permeability of the furnace cylinder is enhanced.

Benefits of technology

The furnace condition is adjusted in a timely manner, avoiding the missed optimal adjustment time, improving the activity and stability of the furnace cylinder, reducing the energy consumption and cost of blast furnaces, avoiding damage to suspended materials and air outlets, and improving production efficiency.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention belongs to the technical field of iron smelting, and in particular to a method for improving the activity of a blast furnace hearth, comprising the following contents: in the process of producing molten iron in the blast furnace, when the liquid permeability index DMI≥260, it is continuously maintained; when 210<the liquid permeability index DMI<260, the blast furnace coke ratio is increased and the blast furnace coal ratio is reduced; when the liquid permeability index DMI≤210, the following measures are taken: (1) increasing the blast furnace coke ratio and reducing the coal ratio; (2) optimizing the quality of coke and coal injection; (3) reducing the lump ore ratio; (4) controlling the silicon and sulfur content of molten iron, the physical heat of molten iron, and the slag composition; (5) adjusting the sintering ingredients; (6) stabilizing the blast furnace air volume; (7) reducing the tuyere area; (8) adjusting the order of material distribution; (9) improving the material line; (10) adopting the A+2B composite material system to expand the ore batch. The method avoids blast furnace hanging material, hearth inactivity and tuyere damage, and improves the production efficiency of the blast furnace.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of iron smelting, and in particular relates to a method for improving the activity of a blast furnace hearth. Background Art

[0002] The continuous active state of the blast furnace hearth is the basic guarantee for the continuous and stable operation of the blast furnace condition. Therefore, the activity of the blast furnace hearth has always been the focus of blast furnace smelting workers. At present, the judgment of the activity of the blast furnace hearth is mainly judged by monitoring the temperature changes of the thermocouples installed at the center between the semi-graphite carbon bricks and the microporous carbon bricks at the bottom of the blast furnace to judge the activity state of the hearth. However, the temperature and its changes monitored by the thermocouples here have already indicated the actual state of the blast furnace hearth state, and cannot timely, accurately and real-time predict the development trend of the hearth permeability. This method of comprehensively judging the hearth state by monitoring the temperature and change trend of the thermocouples at the bottom of the furnace has a certain lag in the analysis and prediction of the hearth state, and it is easy to miss the best time to adjust the furnace condition. Once there is a problem with the hearth (accumulation in the hearth, etc.), the stability of the blast furnace condition will decrease, resulting in fluctuations in the furnace condition, causing economic losses in blast furnace production. During the blast furnace smelting process, as the blast furnace smelting continues, when the carbon content of the molten iron in the furnace hearth increases, the probability of forming graphite nuclei during crystallization of the molten iron increases, thereby increasing the temperature at which the molten iron in the furnace hearth begins to crystallize and the ability of graphite carbon to precipitate, reducing the liquid permeability of the furnace hearth, reducing the activity of the furnace hearth, and weakening the stability of the furnace condition, causing accidents such as suspended material in the blast furnace, inactive furnace hearth, damaged tuyere, and abnormal blast furnace condition, resulting in reduced blast furnace production efficiency and increased energy consumption and costs. Summary of the invention

[0003] The purpose of the present invention is to provide a method for improving the activity of a blast furnace hearth, so as to solve the problem that the existing method has a lag in the analysis and prediction of the hearth state, which is easy to miss the best time to deal with the furnace condition, resulting in the deterioration of the hearth activity and the reduction of the stability of the blast furnace condition, causing accidents such as suspended materials in the blast furnace, inactive hearth, damaged tuyere and abnormal blast furnace condition, and the problem that the fluctuation of the furnace condition causes the reduction of productivity and the increase of energy consumption and cost.

[0004] In order to achieve the above object, the present invention adopts the following technical scheme:

[0005] A method for improving the activity of a blast furnace hearth, comprising the following contents:

[0006] In the process of continuous smelting of molten iron in the blast furnace, the higher the DMI value of the dead material column permeability index of the furnace, the better the dead material column permeability of the furnace, the stronger the slag and iron discharge capacity of the furnace, and the more conducive to improving the furnace state. The physical thermal index T of the molten iron must be used. HM As a basic guarantee, the physical heat of molten iron T HM The temperature between 1490°C and 1510°C is more suitable. The DMI value of the dead material column in the furnace is evaluated as follows:

[0007] When the dead material column liquid permeability index DMI ≥ 260, it indicates that the dead material column liquid permeability of the furnace is relatively good and continues to maintain;

[0008] When 210<Dead material column liquid permeability index DMI<260, it indicates that the dead material column liquid permeability of the furnace is low and the furnace activity is reduced, and micro-adjustments are needed: increase the blast furnace coke ratio by 5-15kg / t, reduce the blast furnace coal ratio by 5-15kg / t, and improve the dead material column liquid permeability;

[0009] When the dead material column permeability index DMI ≤ 210, it indicates that the dead material column permeability of the furnace is greatly reduced, the furnace activity is low, and the activity needs to be improved in time. The measures are as follows:

[0010] (1) Increase the coke ratio of blast furnace and reduce the coal ratio: Increase the coke ratio of blast furnace by 10-20kg / t and reduce the coal ratio by 10-20kg / t;

[0011] (2) Optimize the quality of coke and improve the quality of PCI: reduce the proportion of rammed coke, and the proportion of top-loading coke (Shan Jiao, Mei Jin, Taida) ≥ 25%; reduce the proportion of bituminous coal by 10%-30%, and the high calorific value of mixed PCI coal reaches ≥ 7600cal / kg, and the particle size of PCI coal -200 mesh >75.0%;

[0012] (3) Adjustment of blast furnace charging structure: reduce the proportion of lump ore and stop using poor quality raw ore; increase the proportion of good quality pellets and improve the total proportion of pellets;

[0013] (4) The silicon content of molten iron is controlled at 0.40-0.60%, the sulfur content of molten iron is controlled at 0.030-0.045%, the magnesium-aluminum ratio of slag is increased, the magnesium-aluminum ratio is controlled at 0.65-0.70, the binary basicity R2 of slag is reduced, R2 is controlled at 1.15-1.19, and the quaternary basicity of slag is 1.02-1.05;

[0014] (5) Adjust the sintering ore mix and reduce the proportion of high-titanium concentrate to 1% to ensure that the titanium content of molten iron is ≤0.070%;

[0015] (6) Stable blast furnace air volume: air volume > 2950m 3 / min, wind speed ≥245m / s, blow the furnace;

[0016] (7) Reduce the blast furnace tuyere area, increase the number of Φ110mm tuyere by 2-4, reduce the number of Φ115mm tuyere by 2-4, increase the tuyere wind speed, and enhance the ability of the furnace gas to penetrate into the center;

[0017] (8) Adjust the order of material distribution: arrange coke pieces and lump ore in the middle ring, pellets in the outer ring, and coke in the center;

[0018] (9) Improve gas utilization: improve the material line;

[0019] (10) Adopt A+2B composite material system and expand ore batches. The size of ore batches shall be based on the blast furnace material rate of 6.00-6.10 batches / hour. A: JJ↓kk↓, B: JJ↓kk↓kk↓, where JJ↓ represents 2 cars of coke and kk↓ represents 2 cars of ore. This will improve the thickness of the coke layer in the soft melt layer, reduce the interface effect and enhance the stability of the furnace condition.

[0020] Preferably, the furnace dead material column liquid permeability index DMI calculation formula is:

[0021] DMI=△C / 2.57×10 -3 +T HM -1430+190×(1.23-R2), △C is the absolute value of the difference between the actual carbon content [C] of the molten iron and the saturated carbon content Csat, △C=|[C](%)-Csat(%)|, T HM is the molten iron temperature, in °C; R2 is the binary basicity of blast furnace slag = CaO / SiO2.

[0022] Preferably, in the measure (9), the material line is increased to 1.5 meters.

[0023] Preferably, the measure (10) further includes increasing the oxygen enrichment content of the blast furnace.

[0024] The theoretical basis for this method is:

[0025] 1. Predict by using the change of molten iron [C]

[0026] The process of carbon dissolving in solid or liquid iron is called molten iron carburizing reaction. This process is an endothermic reaction. The higher the temperature, the faster and more intense the reaction. When the charge melts, part of the iron ore in the upper part of the blast furnace is gradually reduced to metallic iron. Carburizing in the furnace can be roughly divided into three stages:

[0027] The first stage is the carburization of sponge iron. At 400℃~600℃, the sponge iron in the blast furnace undergoes a CO smoke carbon precipitation reaction, and the solid sponge iron begins to undergo the following carburization process, 2CO→CO2 +[C], in which part of the carbon participates in the reduction reaction, and part of the carbon is adsorbed on the sponge iron and enters the pig iron, that is, 2CO+3Fe=Fe3C+CO2. When the reaction reaches equilibrium, the carbon content in the sponge iron can reach 1.5%, and the carburization amount in this stage accounts for about 1.5% of the total carburization amount.

[0028] The second stage is carburization of liquid iron. The initially carburized metallic iron continues solid phase carburization with the hot coke at about 1400℃, begins to melt into molten iron, and drips through the coke into the furnace.

[0029] The third stage is the carburizing process in the furnace. Only a small amount of carburizing is carried out in the furnace, generally only 0.1%-0.5%.

[0030] In the process of molten iron dripping into the furnace in the above stages, in addition to the carburizing reaction, silicon, manganese, and phosphorus also enter the pig iron, and harmful impurities such as sulfur are removed to form the final composition of pig iron. Slag has a decisive influence on the furnace condition of the blast furnace and the quality of pig iron. If you want to make good iron, you must make good slag. However, experiments show that the carbon content of unmelted sponge iron is less than 1.0%. When it melts, it has good contact reaction conditions with coke and other materials during the dripping process, and carburization proceeds rapidly: 3Fe+C=Fe3C. The carbon content in the furnace waist can reach 2.5%-3.0%; it reaches the maximum near saturation in the lower part of the dripping zone; it is partially oxidized in the tuyere area, and there is still a small amount of carburization process in the furnace.

[0031] The relationship between the final carbon content in the molten iron and the temperature: On the Fe-C equilibrium phase diagram, the eutectic point saturated carbon content is 4.30% at 1153°C. As the temperature increases, the saturated carbon content increases. The calculation formula is: %[C]=1.30+2.57×10 -3 T HM , where T HM The temperature of molten iron is ℃. The stronger the permeability of the furnace, the more active it is, and the higher the temperature of molten iron.

[0032] The [C] in the molten iron is mainly the carburizing reaction of the molten iron, which is an endothermic reaction. The higher the physical heat of the molten iron THM, the more intense the reaction, and the relative increase in the molten iron [C]; the physical heat of the molten iron T HM Mainly reflects the heat reserve of the furnace, the physical heat of molten iron T HM The higher it is, the more sufficient the furnace heat is, the better the furnace permeability is, and the more active it is.

[0033] (1) When molten iron [C] ≥ 4.50-4.60%, it indicates that the physical heat of molten iron T HM Sufficient heat and good furnace permeability are conducive to improving the furnace state;

[0034] (2) When the molten iron [C] is less than 4.40-4.50%, it indicates that the furnace permeability is reduced and improvement measures are needed.

[0035] 2. Impact of graphite carbon in molten iron

[0036] 2.1 Calculate the saturated carbon Csat of molten iron by molten iron composition and molten iron temperature

[0037] The influence of alloying elements on the solubility of carbon in liquid Fe-C alloys further calibrates and improves the saturated carbon Csat formula of molten iron:

[0038] Csat=1.30+2.57×10 -3 T HM-0.31[Si]-0.33[P]-0.40[S]-0.053[Ni]-0.074[Cu]+0.027[Mn]+0.17[Ti]+0.063[Cr]+0.135[V].

[0039] 2.2 The influence of molten iron composition on the crystallization temperature of molten iron in the furnace and the ability of graphite carbon precipitation, and the prediction of the influence on the liquid permeability of the furnace

[0040] A large amount of graphite carbon precipitation in the furnace will reduce the furnace permeability and affect the furnace state, which is also a major factor causing the accumulation of the furnace. The amount of graphite carbon precipitation in the furnace mainly depends on the ability of carbon in the molten iron to be converted into graphite carbon.

[0041] 2.3 Effect of molten iron [C]

[0042] As the carbon content of molten iron increases, the probability of forming graphite nuclei during crystallization increases, thereby increasing the temperature at which molten iron in the furnace begins to crystallize and the ability of graphite carbon to precipitate. The temperature at which molten iron begins to crystallize and the amount of graphite carbon precipitated in pig iron increase with the increase in the carbon content of pig iron.

[0043] As the [C] content of molten iron increases, the probability of forming graphite nuclei during crystallization increases, which increases the temperature at which the molten iron in the furnace begins to crystallize and the ability of graphite carbon to precipitate, and reduces the liquid permeability of the furnace.

[0044] When molten iron [C]>5.00%, it indicates that the precipitation of graphite carbon in molten iron is intensified, affecting the working state of the furnace. Improvement measures:

[0045] (1) Physical heat of molten iron T HM >1515-1520℃ to control and slow down the precipitation of graphite carbon in molten iron;

[0046] (2) According to the furnace conditions, the blast furnace coke ratio is reduced by 3-5kg / t, the blast furnace coal ratio is increased by 5-8kg / t, and the theoretical combustion temperature of the tuyere is appropriately reduced;

[0047] The final molten iron [C] is controlled at 4.50-5.00%, and the molten iron physical thermal T HM 1490-1510℃ is more suitable.

[0048] 3. Influence of molten iron [Si] and [Ti]

[0049] 3.1 Effect of molten iron [Si]

[0050] The silicon atoms in the molten iron have a strong bonding force with the iron atoms. Silicon can weaken the bonding force between Fe and C atoms, increase the temperature of the eutectic point, and significantly reduce the carbon content of the eutectic point, prompting the precipitation of graphite carbon, which is particularly obvious in the eutectic transformation stage. Therefore, with the increase of silicon content in the molten iron, the temperature at which the molten iron begins to crystallize and the graphite carbon content of pig iron both increase.

[0051] 3.2 Effect of molten iron [Ti]

[0052] The main function of [Ti] in molten iron is to increase the amount of graphite carbon precipitation and raise the temperature at which molten iron begins to crystallize. [Ti] in molten iron easily combines with carbon to form TiC, which increases impurities in molten iron and is beneficial to graphitization and graphite carbon precipitation. The generated TiC, TiN and TiNC can also enter the slag to make the slag viscous and reduce the liquid permeability of the furnace.

[0053] 3.3 Control measures for molten iron [Si]+[Ti]

[0054] With the increase of [Si] and [Ti] in molten iron, the crystallization temperature of molten iron and the graphite carbon content of pig iron both increase. Among them, [Ti] has a much greater impact on the crystallization temperature of molten iron and the graphite carbon content of pig iron than [Si]: the crystallization temperature of molten iron [Ti] is 3.6 times that of [Si]; the graphite carbon content of molten iron [Ti] is 5.6 times that of [Si], which has a great impact on the liquid permeability of the furnace. [Ti] must be strictly controlled, and [Ti] is required to be ≤0.08%.

[0055] In the blast furnace operation process, [Si]+[Ti] is used for control, and the control range is: 0.33-0.55% (where [Ti]≤0.080%)

[0056] When [Si]+[Ti]>0.60%, improvement measures are taken:

[0057] (1) Adjustment of the ingredient structure: reduce the proportion of high-titanium concentrate used in sintering and reduce the proportion of high-titanium balls in blast furnaces;

[0058] (2) Control the blast furnace iron [Si]; the lower limit [Si] cannot be lower than 0.30% continuously. The physical thermal conductivity T HM Not less than 1490℃ to ensure sufficient heat in the furnace.

[0059] 4. Effect of molten iron physical heat and [S]

[0060] 4.1 Effect of molten iron [S]

[0061] [S] in molten iron forms MnS and FeS in pig iron, most of which are distributed on the grain boundaries in the form of eutectics, which hinders the diffusion of carbon atoms; [S] can also increase the bonding force between iron and carbon atoms, strongly preventing graphitization;

[0062] When [S]≤0.030%, the graphite carbon content increases rapidly as [S] decreases; when [S]>0.030%, the graphite carbon content in pig iron can be controlled within a range of less than 1.5%, and its rate of change becomes gentle. Based on this, it can be considered that the [S] content in blast furnace molten iron should not be continuously less than 0.030%;

[0063] According to the actual production needs, it is more appropriate to control the molten iron [S] at 0.020-0.040%, and the slag binary basicity R2 is controlled in the range of 1.18-1.24. By adjusting the magnesium-aluminum ratio (its control range is 0.55-0.65), the slag quaternary basicity R4 is ensured to be 1.03-1.06 to meet the needs of slag desulfurization and alkali metal removal. At the same time, the heat demand for furnace desulfurization is considered to ensure the physical heat T of the molten iron. HM 1490-1510℃ is more suitable.

[0064] 4.2 Selection of furnace thermal system

[0065] On the one hand, the composition of molten iron determines the graphite carbon content of pig iron and the temperature at which molten iron begins to crystallize; on the other hand, controlling the furnace thermal system and slag composition can control the molten iron composition. Therefore, choosing an appropriate furnace thermal system to control the appropriate molten iron composition is one of the means to prevent furnace accumulation.

[0066] Compared with the prior art, the present invention has the following beneficial effects:

[0067] (1) Using the formula DMI = △C / 2.57×10 -3 +T HM -1430+190×(1.23-R2) Calculation of the dead material column permeability index DMI can accurately determine the activity of the blast furnace hearth, and take timely measures to adjust the furnace condition to avoid missing the best time to deal with the furnace condition;

[0068] (2) By increasing the blast furnace coke ratio, reducing the proportion of ramming coke, using top-loading coke, reducing the proportion of lump ore, increasing the total proportion of pellets, adopting the A+2B composite material system and reasonably expanding the ore batch, the thickness of the coke layer in the soft melting layer can be ensured and stabilized, the interface effect can be reduced, the gas utilization rate can be improved, and the furnace condition stability can be enhanced;

[0069] (3) Appropriately increase the [Si] and [S] content of molten iron and the magnesium-aluminum ratio of slag, combine with controlling the binary basicity and quaternary basicity of slag, and at the same time, considering that the physical heat of molten iron is 1490-1510℃, control the crystallization temperature of molten iron and the graphite carbon content of pig iron, and improve the liquid permeability of the furnace;

[0070] (4) Reduce the tuyere area, stabilize the air volume, increase the tuyere wind speed, and combine it with increasing the oxygen enrichment of the blast furnace tuyere to improve the combustion efficiency of the pulverized coal in the furnace, invigorate the furnace, and improve the stability of the furnace condition;

[0071] (5) After adopting this method, it is possible to avoid the occurrence of suspended materials in the blast furnace, inactive hearth, and damaged tuyere, thereby improving the activity of the blast furnace hearth, increasing the stability of the furnace condition, improving the blast furnace production efficiency, and reducing the blast furnace energy consumption and cost. DETAILED DESCRIPTION

[0072] The technical solution of the present invention is further described below in conjunction with embodiments.

[0073] This method has been applied and implemented in the process of producing molten iron in the furnace of the 5# blast furnace, controlling the molten iron [C] to 4.60%, [Si]+[Ti]=0.489%, of which [Ti] is 0.039%, and [S] is 0.035%, including the following contents:

[0074] The ore (iron-containing raw materials, auxiliary materials) and coke are weighed and prepared in proportion under the blast furnace trough and placed in the weighing hopper. They are then transported to the ore and coke centralized hoppers through the ore belt and coke belt. The material car is then used to transport the ore and coke to the furnace top receiving hopper separately and alternately. The top density of the furnace is opened to enter the material tank, and then the material tank is pressurized. After the blast furnace material line reaches the specified value, the probe is raised to zero. Finally, the lower density and material flow regulating valves are opened. The ore and coke are separately, individually and alternately distributed on the upper material surface of the blast furnace through the furnace top distribution chute according to the distribution matrix. The blast furnace blast cold air and oxygen-enriched air are sent to the hot blast furnace through the cold air system. After the hot blast furnace undergoes heat exchange to generate hot air, they are sent to the blast furnace tuyere through the hot air supply system to supply air to the blast furnace. At the same time, the blast furnace coal injection is sent to the tuyere through the coal injection system, and then sprayed to the blast furnace tuyere hearth area through the tuyere coal gun. At high temperature, carbon in coke and pulverized coal burns with oxygen in the hot air blown in from the tuyere to generate carbon monoxide. The blast furnace charge (ore, coke, etc.) is smelted in the furnace from top to bottom. During the descending process, it meets the rising blast furnace gas, and heat transfer and reduction occur successively. When the ore melts, part of the iron ore in the upper part of the blast furnace is gradually reduced to metallic iron. In addition to the carburizing reaction, silicon, titanium, manganese, sulfur, and phosphorus also enter the pig iron. With the increase of silicon and titanium in the molten iron, the crystallization temperature of the molten iron and the graphite carbon content of the pig iron both increase. The sulfur in the molten iron forms MnS and FeS in the pig iron, most of which are distributed on the grain boundaries in the form of eutectics.

[0075] Physical heat of molten iron T HM Controlled at 1506℃, the saturated carbon content Csat is 5.01%, the actual carbon content of molten iron is 4.60%, R2=1.23, △C=|[C](%)-Csat(%)|=|4.60-5.01|=0.41, using the formula DMI=△C / 2.57×10 -3 +T HM -1430+190×(1.23-R2) calculates the dead material column liquid permeability index DMI of the furnace hearth. The dead material column liquid permeability index DMI is 235, indicating that the dead material column of the furnace hearth has low permeability and the furnace hearth activity is reduced. Minor adjustments are required: the blast furnace coke ratio is increased to 315kg / t, the blast furnace coal ratio is adjusted to 180kg / t, and the dead material column liquid permeability index DMI is calculated to be 268, which is maintained continuously.

[0076] As the process continues, the dead column permeability index decreases, using the formula DMI = △C / 2.57×10 -3 +T HM -1430+190×(1.23-R2) calculates the dead material column liquid permeability index DMI of the furnace hearth. The dead material column liquid permeability index DMI is 206, indicating that the dead material column liquid permeability of the furnace hearth is greatly reduced and the furnace hearth activity is low. The steps to improve the furnace hearth activity are as follows:

[0077] (1) The blast furnace coke ratio increased from 315kg / t to 325kg / t, and the blast furnace coal ratio decreased from 180kg / t to 160kg / t;

[0078] (2) Reduce the proportion of ramming coke to 25% of mountain coke; adjust the proportion of bituminous coal from 60% to 50%, adjust the high calorific value of the mixed PCI coal to 7600 cal / kg, and the PCI coal particle size of -200 mesh to 80.0%;

[0079] (3) The lump ore ratio was adjusted to 3%, the poor quality raw tower blocks were discontinued, and the total pellet ratio was adjusted to 8%;

[0080] (4) Increase the magnesium-aluminum ratio of the slag, control the magnesium-aluminum ratio at 0.68, reduce the binary basicity R2 of the slag, control R2 to 1.17, and the quaternary basicity R4 of the slag to 1.03;

[0081] (5) Adjust the sintering ore mix and reduce the proportion of high-titanium concentrate to 1% to ensure that the titanium content of molten iron is 0.070%;

[0082] (6) Air volume is 3000m 3 / min, wind speed is 249m / s, blowing the furnace;

[0083] (7) Reduce the blast furnace tuyere area, increase the number of Φ110mm tuyere from 9 to 11, reduce the number of Φ115mm tuyere from 11 to 9, and reduce the tuyere area from 0.1998m 2 Shrink to 0.1979m 2 , increase the wind speed at the tuyere and enhance the ability of the furnace gas to penetrate into the center;

[0084] (8) Coke pieces and lump ore are placed in the middle ring, pellets are placed in the outer ring, and good quality coke is placed in the center;

[0085] (9) The material line is gradually raised to 1.50 meters to improve gas utilization;

[0086] (10) Expanding the ore batch: adopting A+2B composite material system (A: JJ↓kk↓, B: JJ↓kk↓kk↓, where JJ↓ represents 2 cars of coke and kk↓ represents 2 cars of ore) and controlling the blast furnace material rate at 6.00-6.10 batches / hour, expanding the ore batch, and increasing the blast furnace oxygen enrichment from 13500m3 / h increased to 14000-14500m 3 / h, and the ore batch is gradually expanded from 47 tons to 50 tons, ensuring and stabilizing the thickness of the soft melting layer coke layer, reducing interface effects and enhancing furnace stability.

[0087] The liquid permeability index DMI of the furnace dead material column was calculated again and was 266, indicating that the liquid permeability of the furnace dead material column was relatively good and maintained continuously.

[0088] Harmful impurities such as sulfur are removed to form the final pig iron.

[0089] After adopting this solution, the furnace permeability is significantly improved, the furnace condition stability is improved, and the benefits are as follows:

[0090] (1) Improve gas utilization: Before the implementation of the above plan, the gas utilization rate of furnace 5 was 44.88% on average in February 2024. After the implementation of the above plan in March, the gas utilization rate of furnace 5 reached an average of 45.24%, with a maximum of 46.30%. The gas utilization increased by 0.36% and the gas utilization rate increased by 1%. The coke ratio decreased by 5kg / t and 1.80kg / t, reducing the molten iron cost by RMB 3.78 / t.

[0091] Benefit calculation process (coke unit price 2100 yuan / t, or 2.10 yuan / kg):

[0092] Reduce coke ratio: 5kg / t*0.36=1.80kg / t; reduce molten iron cost by 1.80kg / t*2.10 yuan / kg=3.78 yuan / t.

[0093] (2) Improve the pulverized coal combustion rate: Before the above plan was implemented, the average fixed C in the bag dust ash of the 5# furnace was 26.98% in February 2024. After the above plan was implemented in the 5# furnace in March, the average fixed C in the bag dust ash was 22.53%, a relative decrease of 4.45%. The benefits are (ash-iron ratio is 25kg / t, coke fixed carbon is 86.0%), the coke ratio is reduced by 1.29kg / t, and the molten iron cost is reduced by 2.71 yuan / t.

[0094] Benefit calculation process (coke unit price 2100 yuan / t, or 2.10 yuan / kg):

[0095] Coke saving ratio: 25kg / t*4.45% / 86.00%=1.29kg / t; reduction of molten iron cost 1.29kg / t*2.1 yuan / kg=2.71 yuan / t.

[0096] (3) When the above plan was not implemented, there were 2 overhangs in the blast furnace in February 2024, and 2 tuyere damages in February. After the above plan was implemented in March, the blast furnace had 0 overhangs and 0 tuyere damages, which reduced the erosion and damage of the furnace lining refractory materials, was beneficial to the longevity of the blast furnace, and reduced the safety hazards of blast furnace production.

Claims

1. A method for improving the activity of a blast furnace hearth, characterized in that: It includes the following: In the process of preparing molten iron, the higher the DMI value of the dead material column permeability index of the furnace, the better the dead material column permeability of the furnace, the stronger the slag iron discharge capacity of the furnace, and the more conducive to improving the furnace state. As a basic guarantee, the physical thermal T HM At 1490-1510°C, the calculation formula of the furnace dead material column liquid permeability index DMI is: DMI=△C / 2.57×10 -3 +T HM -1430+190×(1.23-R2), △C is the absolute value of the difference between the actual carbon content [C] of the molten iron and the saturated carbon content Csat, △C=|[C](%)-Csat(%)|, T HM is the molten iron temperature, in °C; R2 is the binary basicity of blast furnace slag = CaO / SiO2; the evaluation of the DMI value of the dead material column permeability index of the furnace cylinder is as follows: When the dead material column liquid permeability index DMI ≥ 260, it indicates that the dead material column liquid permeability of the furnace is relatively good and it is maintained continuously; When 210<Dead material column liquid permeability index DMI<260, it indicates that the dead material column liquid permeability of the furnace is low and the furnace activity is reduced, and micro-adjustments are needed: increase the blast furnace coke ratio by 5-15kg / t, reduce the blast furnace coal ratio by 5-15kg / t, and improve the dead material column liquid permeability; When the dead material column permeability index DMI ≤ 210, it indicates that the dead material column permeability of the furnace is greatly reduced, the furnace activity is low, and the activity needs to be improved in time. The measures are as follows: (1) Increase the coke ratio of blast furnace and reduce the coal ratio: Increase the coke ratio of blast furnace by 10-20kg / t and reduce the coal ratio by 10-20kg / t; (2) Optimize the quality of coke and improve the quality of PCI: reduce the proportion of ramming coke, and the proportion of top-loading coke should be ≥25%; reduce the proportion of bituminous coal by 10%-30%, and the high calorific value of mixed PCI coal should reach ≥7600cal / kg, and the particle size of PCI coal should be -200 mesh>75.0%; (3) Adjustment of blast furnace charging structure: reduce the proportion of lump ore, stop using poor quality raw ore, and increase the amount of good quality pellets; (4) The silicon content of molten iron is controlled at 0.40-0.60%, the sulfur content of molten iron is controlled at 0.030-0.045%, the magnesium-aluminum ratio of slag is increased, the magnesium-aluminum ratio is controlled at 0.65-0.70, the binary basicity R2 of slag is reduced, R2 is controlled at 1.15-1.19, and the quaternary basicity of slag is 1.02-1.05; (5) Adjust the sintering ore mix and reduce the proportion of high-titanium concentrate to 1% to ensure that the titanium content of molten iron is ≤0.070%; (6) Stable blast furnace air volume: air volume > 2950m 3 / min, wind speed ≥245m / s, blow the furnace; (7) Reduce the blast furnace tuyere area, increase the number of Φ110mm tuyere by 2-4, reduce the number of Φ115mm tuyere by 2-4, increase the tuyere wind speed, and enhance the ability of the furnace gas to penetrate into the center; (8) Adjust the order of material distribution: arrange coke pieces and lump ore in the middle ring, pellets in the outer ring, and coke in the center; (9) Improve gas utilization: improve the material line; (10) Adopt A+2B composite material system and expand ore batches. The size of ore batches shall be based on the blast furnace material rate of 6.00-6.10 batches / hour. A: JJ↓kk↓, B: JJ↓kk↓kk↓, where JJ↓ represents 2 cars of coke and kk↓ represents 2 cars of ore. This will improve the thickness of the coke layer in the soft melt layer, reduce the interface effect and enhance the stability of the furnace condition.

2. A method for improving the activity of a blast furnace hearth according to claim 1, characterized in that: In the measure (9), the feed line is raised to 1.5 meters.