Nano-silicon crystal cluster in-situ loaded lithium silicate negative electrode material and preparation method and battery thereof
By mixing the lithium material and silicon material in a preset ratio in a lithium battery and vacuum heat treatment, a nano-silicon crystal cluster is formed in situ loaded lithium silicate material, and carbon coating is carried out, the silicon volume expansion and carrier bonding strength are solved. The problem of insufficient improvements in the cycle stability and charge and discharge rate of the battery.
Patent Information
- Application Number
- CN202411162465.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-08-23
AI Technical Summary
As the negative electrode material of lithium battery, the volume expansion of silicon increases the structure during the electrochemical cycle, making it difficult to form a stable solid electrolyte interface, resulting in a degradation of cyclic performance, and the lack of chemical bonding between nano-silicon and common carriers, resulting in a cycle "dive" phenomenon.
By mixing lithium material and silicon material in a preset ratio for vacuum heat treatment and deposition treatment, nano-silicon crystal clusters are formed in situ loaded lithium silicate material, and carbon coating is carried out to form a carbon layer with high order to ensure nano-silicon The uniform distribution and binding strength of silicon crystal clusters on the lithium silicate carrier.
It improves the cycle stability and charge and discharge rate of the battery, extends the service life of the battery, reduces the internal resistance of the material, and optimizes the electrochemical performance.
Smart Images

Figure CN118666287B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium batteries, and in particular to a nano-silicon crystal cluster in-situ loaded lithium silicate negative electrode material, a preparation method of a nano-silicon crystal cluster in-situ loaded lithium silicate negative electrode material, and a battery. Background Art
[0002] As a negative electrode material for lithium batteries, silicon has shown significant advantages over traditional graphite negative electrodes, including its ultra-high theoretical specific capacity and low lithium desorption potential, which makes silicon one of the most promising options for upgrading carbon-based negative electrodes for lithium batteries. However, as a semiconductor material, silicon has low electrical conductivity, and during the electrochemical cycle, the insertion and extraction of lithium ions will cause the volume of the material to expand and shrink by more than 300%, resulting in gradual pulverization of the material, structural collapse, and ultimately the separation of the electrode active material from the current collector, loss of electrical contact, and greatly reduced battery cycle performance. In addition, due to this volume effect, it is difficult for silicon to form a stable solid electrolyte interface (SEI) film in the electrolyte. Along with the destruction of the electrode structure, a new SEI film is continuously formed on the exposed silicon surface, exacerbating the corrosion and capacity decay of silicon.
[0003] In order to deal with the volume expansion problem of silicon during the electrochemical reaction, among many solutions, selecting a suitable carrier, nano-sizing silicon particles, and coating have become key measures. Commonly used carriers include graphite, graphene, porous carbon, etc., and the silicon particles are nano-sized and loaded on the carrier. The carbon-containing carrier has good conductivity and a certain ductility. Combined with nano-silicon, the volume expansion is reduced. The synergistic effect of the two effectively improves the stability of the silicon-carbon negative electrode structure. However, there is a lack of chemical bonding between silicon and the aforementioned commonly used carriers, and nano-silicon is difficult to achieve uniform dispersion on the carrier, which may lead to the destruction of the silicon-carbon composite structure after multiple cycles of the battery, resulting in a cycle "diving" phenomenon. Summary of the invention
[0004] In response to at least some of the problems and shortcomings in the prior art, the embodiments of the present invention disclose a nano-silicon crystal cluster in-situ loaded lithium silicate negative electrode material, a method for preparing a nano-silicon crystal cluster in-situ loaded lithium silicate negative electrode material, and a battery, which have the advantages of high first efficiency, long cycle and excellent fast charging kinetics.
[0005] On the one hand, an embodiment of the present invention provides a method for preparing a nano-silicon cluster in-situ loaded lithium silicate negative electrode material, comprising: mixing a lithium material and a silicon material in a preset ratio, and then performing vacuum heat treatment and deposition treatment to obtain a nano-silicon cluster in-situ loaded lithium silicate material; the preset ratio is the molar ratio of the lithium element in the lithium material to the silicon element in the silicon material, and the range of the preset ratio is 2:(1.03~1.15); the nano-silicon cluster in-situ loaded lithium silicate material is subjected to carbon coating treatment to obtain a nano-silicon cluster in-situ loaded lithium silicate negative electrode material; the carbon source gas used in the carbon coating treatment is carbon dioxide; the nano-silicon cluster content in the nano-silicon cluster in-situ loaded lithium silicate negative electrode material is 40~50%, and the Id / Ig of the nano-silicon cluster in-situ loaded lithium silicate negative electrode material is 0.12~0.6; wherein the silicon material includes any one or more of silicon element and silicon alloy, the lithium material includes any one or more of lithium oxide and non-silicate material, and the non-silicate material is a material that can obtain lithium oxide after heat treatment.
[0006] In one embodiment of the present invention, the lithium material and the silicon material are mixed evenly in a preset ratio and then subjected to vacuum heat treatment and deposition treatment to obtain the nano-silicon crystal cluster in-situ loaded lithium silicate material, specifically comprising: mixing the lithium material and the silicon material in the preset ratio to obtain a first mixed material; placing the first mixed material in a vacuum furnace and performing the vacuum heat treatment at a temperature of 1150~1450℃, and performing the deposition treatment at a temperature of 400~650℃, and obtaining a first cooling product after cooling, wherein the vacuum degree of the vacuum furnace is less than 12 Pa, and the temperature of the first cooling product is 20~60℃; crushing and sieving the first cooling product in an inert atmosphere to obtain the nano-silicon crystal cluster in-situ loaded lithium silicate material.
[0007] In one embodiment of the present invention, the inert atmosphere includes any one or more of nitrogen, helium, argon, neon, and xenon; the median particle size of the in-situ loaded lithium silicate material of the nano-silicon cluster is 3 to 8 microns; and the lithium material includes any one or more of lithium carbonate, lithium hydroxide, lithium oxalate, lithium acetate, lithium citrate, lithium borate, and lithium aluminate.
[0008] In one embodiment of the present invention, the carbon coating treatment of the nano-silicon cluster in-situ loaded lithium silicate material to obtain the nano-silicon cluster in-situ loaded lithium silicate negative electrode material specifically includes: placing the nano-silicon cluster in-situ loaded lithium silicate material into a reactor and introducing the carbon source gas into the reactor, heating at a temperature of 400°C to 680°C, and keeping warm for 60 to 360 minutes, and obtaining a second cooling product after cooling; the second cooling product and an acidic material are subjected to acid washing treatment and drying and screening treatment to obtain the nano-silicon cluster in-situ loaded lithium silicate negative electrode material.
[0009] In one embodiment of the present invention, the acidic material comprises any one or more of hydrochloric acid, nitric acid, citric acid, and oxalic acid, the concentration of the acidic material is 0.1-0.6 mol / L, and the acid washing treatment time is 20-90 minutes.
[0010] In one embodiment of the present invention, the carbon content of the nano-silicon cluster in-situ loaded lithium silicate negative electrode material is 2-6%, and the nano-silicon cluster in-situ loaded lithium silicate negative electrode material has mesopores, and the average particle size of the mesopores is 3-7 nanometers.
[0011] On the other hand, an embodiment of the present invention provides a nano-silicon cluster in-situ loaded lithium silicate negative electrode material, comprising: a carbon coating layer, a lithium silicate carrier coated by the carbon coating layer, and a nano-silicon cluster located on the lithium silicate carrier; wherein the lithium silicate carrier comprises any one or more of Li2SiO3 and Li4SiO4, the average particle size of the nano-silicon cluster is 1~5 nanometers, the content of the nano-silicon cluster in the nano-silicon cluster in-situ loaded lithium silicate negative electrode material is 40~50%, and the Id / Ig of the nano-silicon cluster in-situ loaded lithium silicate negative electrode material is 0.12~0.6.
[0012] In one embodiment of the present invention, the carbon content in the in-situ loaded lithium silicate negative electrode material of the nano-silicon cluster is 2-6%.
[0013] In one embodiment of the present invention, the carbon coating layer has mesopores, and the average particle size of the mesopores is 3-7 nanometers.
[0014] On the other hand, an embodiment of the present invention provides a battery, comprising the nano-silicon crystal cluster in-situ loaded with lithium silicate negative electrode material prepared by the aforementioned preparation method or the aforementioned nano-silicon crystal cluster in-situ loaded with lithium silicate negative electrode material.
[0015] It can be seen from the above that the above technical features of the present invention can have one or more of the following beneficial effects:
[0016] The silicon material and the lithium material are uniformly mixed in a preset ratio and then subjected to vacuum heat treatment and deposition treatment, wherein the preset ratio is the molar ratio of the lithium element in the lithium material to the silicon element in the silicon material, and the preset ratio ranges from 2: (1.03 to 1.15). The uniformly mixed silicon material and lithium material are subjected to high-temperature vacuum heat reduction and gasification condensation to in-situ prepare a structure in which nano-silicon is dispersedly loaded in a lithium silicate carrier (Li2SiO3 and / or Li4SiO4). In this process, the difference in saturated vapor pressures of SiO and Li formed in the reaction process of the lithium source and the silicon source (LixMOy+Si—Li+SiO+MO) is utilized to control the condensation temperature at the collecting end to achieve the adjustment of the type of lithium silicate carrier (Li2SiO3 and / or Li4SiO4) (2Li+SiO—Li2O+Si; 2Li+3SiO—Li2SiO3+2Si; 4Li+4SiO—Li4SiO4+3Si) and the amount of excess active lithium on the surface. Specifically, since SiO has a lower saturated vapor pressure than Li, when the temperature of the collection chamber is high, more SiO and relatively less Li are preferentially deposited inside. At this time, the molar ratio of the Li:Si component formed inside the particle is small, while there is more excess Li outside. On the contrary, when the temperature of the collection chamber is low, there are more SiO and Li inside. At this time, the molar ratio of the Li:Si component formed inside the particle is large, while there is less excess Li outside. Then, by regulating the content of the excess Li outside, the content of C formed by the reaction with CO2 is further regulated, and the subsequent acid washing by-products are used to achieve the regulation of the porous pore size (4Li+3CO2—2Li2CO3+C or 4Li+CO2—2Li2O+C; 2H + +Li2CO3—2Li + +CO2+H2O or 2H + + Li2O—2Li ++H2O). Therefore, by precisely controlling the deposition temperature of the collection chamber, the silicon in the silicon material can be sublimated and gasified with the lithium source, and the silicon and lithium silicate can be integrated and uniformly distributed with high bonding strength to ensure the firmness of the overall structure. The deposition temperature of the collection chamber and the subsequent CO2 reaction temperature are jointly controlled to avoid the growth of high-temperature silicon grains and form nano-silicon clusters. The nano-silicon clusters are uniformly loaded on the lithium silicate carrier. The nano-silicon reduces the absolute volume expansion, and the nano-silicon clusters are in-situ loaded. The content of nano-silicon clusters in the lithium silicate negative electrode material is 40~50%, which helps to improve the material specific capacity and improve the long cycle performance, thereby extending the battery life and maintaining the stability of the performance. The lithium silicate carrier around the nano-silicon, as an excellent ion conductor, has good ion conductivity, which helps to improve the kinetic rate performance and helps the battery to maintain good performance during rapid charging and discharging, that is, improve the battery charge and discharge rate. In addition, the embodiment of the present invention is prepared by carbon coating treatment to obtain nano-silicon cluster in-situ loaded lithium silicate negative electrode material, and the carbon source gas used in the carbon coating treatment is carbon dioxide. The lithium residual on the surface of the nano-silicon cluster in-situ loaded lithium silicate material reacts with carbon dioxide, and is reduced in situ at low temperature to form a highly ordered carbon layer and lithium carbonate or other by-products. The highly ordered carbon layer covers the surface of the nano-silicon cluster in-situ loaded lithium silicate material, and the nano-silicon cluster in-situ loaded lithium silicate negative electrode material with a surface coated with a low Id / Ig highly ordered conductive carbon layer is obtained, which is beneficial to enhancing the conduction efficiency of electrons, helping to improve the charge and discharge rate and cycle stability of the battery, while reducing the internal resistance of the material and optimizing the electrochemical performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.
[0018] Figure 1 A schematic flow chart of a method for preparing a nano-silicon cluster in-situ loaded lithium silicate negative electrode material provided in an embodiment of the present invention.
[0019] Figure 2 This is a schematic structural diagram of the nano-silicon crystal clusters in-situ loaded with lithium silicate negative electrode materials prepared in Example 1 of the present invention.
[0020] Figure 3 This is the X-ray diffraction pattern of the negative electrode material prepared in Example 1 of the present invention.
[0021] Figure 4 This is a pore size distribution diagram of the nano-silicon crystal cluster in-situ loaded with lithium silicate negative electrode material prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0022] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with the specific embodiments of the present invention and the corresponding drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0023] It should be noted that the terms "first", "second", etc. in the specification and claims of the present invention and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the terms used in this way can be interchangeable where appropriate, so that the embodiments of the present invention described herein can be implemented in an order other than those illustrated or described herein. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.
[0024] It should also be noted that the division of multiple embodiments in the present invention is only for the convenience of description and should not constitute a special limitation. The features in various embodiments can be combined and referenced to each other without contradiction.
[0025] like Figure 1 As shown, an embodiment of the present invention provides a method for preparing a nano-silicon crystal cluster in-situ loaded lithium silicate negative electrode material, and the method for preparing a nano-silicon crystal cluster in-situ loaded lithium silicate negative electrode material comprises the following steps:
[0026] S1: mixing lithium material and silicon material in a preset ratio and subjecting the mixture to vacuum heat treatment and deposition treatment to obtain nano-silicon crystal clusters in-situ loaded with lithium silicate material;
[0027] S2: subjecting the nano-silicon crystal cluster in-situ loaded with lithium silicate material to carbon coating treatment to obtain the nano-silicon crystal cluster in-situ loaded with lithium silicate negative electrode material.
[0028] Specifically, in an embodiment of the present invention, the silicon material includes one or more of silicon and silicon alloy. The lithium material may include any one or more of lithium oxide and non-silicate materials that can be decomposed to obtain lithium oxide after heat treatment. The lithium material may also include any one or more of lithium carbonate, lithium hydroxide, lithium oxalate, lithium acetate, lithium citrate, lithium borate, and lithium aluminate. In step S1, the nano-silicon crystal cluster in-situ loads the lithium silicate material, for example, a mixture containing nano-silicon crystal clusters and lithium silicate, and the silicon crystal cluster is loaded on the lithium silicate matrix. Specifically, the embodiment of the present invention mixes the lithium material and the silicon material evenly according to a preset ratio so that the lithium material and the silicon material form good physical contact, and the mixed lithium material and the silicon material are subjected to vacuum heat treatment and deposition treatment. The vacuum heat treatment is, for example, under high vacuum and high temperature conditions, the lithium material and the silicon material react and sublimate, that is, from solid to gas; the deposition treatment is, for example, sublimation of Li and SiO formed by the reaction of the silicon material and the lithium material, and then the deposition chamber reduces the temperature and condenses, so that it is transformed from gas to solid.
[0029] In step S2, the nano-silicon crystal cluster in-situ loaded lithium silicate material is placed in a carbon dioxide atmosphere furnace for carbon coating treatment. At this time, the excess lithium on the surface of the nano-silicon crystal cluster in-situ loaded lithium silicate material reacts with carbon dioxide, and can be reduced in-situ at low temperature to form a layer of highly ordered carbon layer and lithium carbonate or other byproducts. The highly ordered carbon layer covers the surface of the nano-silicon crystal cluster in-situ loaded lithium silicate material, and the nano-silicon crystal cluster in-situ loaded lithium silicate negative electrode material with a conductive carbon layer with low Id / Ig and high order is obtained. The Id / Ig ratio is mainly used to indicate the defect type and density in graphene. In the Raman spectrum analysis of graphene, the d peak (Id) and the g peak (Ig) are two important characteristic peaks. The size of the Id / Ig ratio reflects the density and type of defects in graphene. When the Id / Ig ratio is large, it means that there are more defects in the graphene, and when the Id / Ig ratio is small, it means that there are fewer defects in the graphene. The Id / Ig of the nano-silicon cluster in-situ loaded lithium silicate negative electrode material prepared in an embodiment of the present invention is, for example, 0.12~0.60, and the Id / Ig is relatively low. The carbon layer has a higher degree of graphitization and structural order, which is beneficial to enhancing the conduction efficiency of electrons, helping to improve the charge and discharge rate and cycle stability of the battery, and optimizing the electrochemical performance.
[0030] In the embodiment of the present invention, a silicon material and a lithium material are uniformly mixed in a preset ratio and then subjected to vacuum heat treatment and deposition treatment, wherein the preset ratio is the molar ratio of the lithium element in the lithium material to the silicon element in the silicon material, and the preset ratio ranges from 2: (1.03 to 1.15). The uniformly mixed silicon material and lithium material are subjected to high-temperature vacuum heat reduction and gasification condensation to in-situ prepare a structure in which nano-silicon is dispersedly loaded in a lithium silicate carrier (Li2SiO3 and / or Li4SiO4). In this process, the difference in saturated vapor pressures of SiO and Li formed in the reaction process of the lithium source and the silicon source (LixMOy+Si—Li+SiO+MO) is utilized to control the condensation temperature at the collecting end to achieve the adjustment of the type of lithium silicate carrier (Li2SiO3 and / or Li4SiO4) (2Li+SiO—Li2O+Si; 2Li+3SiO—Li2SiO3+2Si; 4Li+4SiO—Li4SiO4+3Si) and the amount of excess active lithium on the surface. Specifically, since SiO has a lower saturated vapor pressure than Li, when the temperature of the collection chamber is high, more SiO and relatively less Li are preferentially deposited inside. At this time, the molar ratio of the Li:Si component formed inside the particle is small, while there is more excess Li outside. On the contrary, when the temperature of the collection chamber is low, there are more SiO and Li inside. At this time, the molar ratio of the Li:Si component formed inside the particle is large, while there is less excess Li outside. Then, by regulating the content of the excess Li outside, the content of C formed by the reaction with CO2 is further regulated, and the subsequent acid washing by-products are used to achieve the regulation of the porous pore size (4Li+3CO2—2Li2CO3+C or 4Li+CO2—2Li2O+C; 2H + +Li2CO3—2Li + +CO2+H2O or 2H + +Li2O—2Li ++ H2O). Therefore, by precisely controlling the deposition temperature of the collection chamber, the silicon in the silicon material can be sublimated and gasified with the lithium source, and the silicon and lithium silicate can be integrated and uniformly distributed with high bonding strength to ensure the firmness of the overall structure. The deposition temperature of the collection chamber and the subsequent CO2 reaction temperature are jointly controlled to avoid the growth of high-temperature silicon grains and form nano-silicon clusters. The nano-silicon clusters are uniformly loaded on the lithium silicate carrier. The nano-silicon reduces the absolute volume expansion, and the nano-silicon clusters are in-situ loaded with the lithium silicate negative electrode material. The content of nano-silicon clusters is 40~50%, which helps to improve the material specific capacity and improve the long cycle performance, thereby extending the battery life and maintaining the stability of the performance. The lithium silicate carrier around the nano-silicon, as an excellent ion conductor, has good ion conductivity, which helps to improve the kinetic rate performance and helps the battery maintain good performance during rapid charging and discharging, that is, it improves the battery's charge and discharge rate. In addition, the embodiment of the present invention is prepared by carbon coating treatment to obtain nano-silicon cluster in-situ loaded lithium silicate negative electrode material, and the carbon source gas used in the carbon coating treatment is carbon dioxide. The lithium residual on the surface of the nano-silicon cluster in-situ loaded lithium silicate material reacts with carbon dioxide, and is reduced in-situ at low temperature to form a highly ordered carbon layer and lithium carbonate or other by-products. The highly ordered carbon layer covers the surface of the nano-silicon cluster in-situ loaded lithium silicate material, and the nano-silicon cluster in-situ loaded lithium silicate negative electrode material is obtained, which has a surface coated with a low Id / Ig highly ordered conductive carbon layer, which is beneficial to enhancing the electron conduction efficiency, helping to improve the charge and discharge rate and cycle stability of the battery, and optimizing the electrochemical performance.
[0031] Specifically, the above step S1 specifically includes the following steps:
[0032] S11: uniformly mixing the lithium material and the silicon material according to a preset ratio to obtain a first mixed material;
[0033] S12: placing the first mixed material in a vacuum furnace and performing the vacuum heat treatment at a temperature of 1150-1450° C., and performing the deposition treatment at a temperature of 400-650° C., and obtaining a first cooling product after cooling;
[0034] S13: crushing and screening the first cooling product in an inert atmosphere to obtain the nano-silicon crystal cluster in-situ loaded lithium silicate material.
[0035] In step S11, the preset ratio is the molar ratio of lithium in the lithium material to silicon in the silicon material, and the range of the preset ratio is 2: (1.03-1.15), which helps to increase the dispersibility of the nano-silicon clusters in the lithium silicate carrier. Specifically, the range of the preset ratio is 2: (1.03-1.15), for example, it can be but not limited to 2: 1.03, 2: 1.04, 2: 1.05, 2: 1.06, 2: 1.08, 2: 1.12, 2: 1.15.
[0036] It should be noted that the mixing equipment used for uniform mixing in step S11 includes, for example, a plowshare mixer, a V-type mixer, a fusion machine, a ball mill and other suitable equipment.
[0037] In step S12, the first cooling product is, for example, a material with a relatively stable structure after the nano-silicon crystal cluster in-situ loaded lithium silicate material is cooled, in preparation for the next step of crushing and screening. Specifically, the temperature of the first cooling product is 20-60°C, for example, but not limited to 20°C, 30°C, 40°C, 50°C, 60°C.
[0038] Specifically, the vacuum furnace includes, for example, a heat treatment chamber and a deposition chamber, and the temperature of the heat treatment chamber is, for example, between 1150 and 1450°C, and for example, it may be, but not limited to, 1150°C, 1200°C, 1280°C, 1300°C, 1380°C, 1400°C, and 1450°C. The temperature of the deposition chamber is between 400 and 650°C, and for example, it may be, but not limited to, 400°C, 450°C, 500°C, 550°C, 600°C, and 650°C. The vacuum degree of the vacuum furnace is less than 12 Pa, and for example, it may be, but not limited to, 2Pa, 5Pa, 6Pa, and 10Pa. For example, the first mixed material is placed in the heat treatment chamber of the vacuum furnace for vacuum heat treatment, and then placed in the deposition chamber for deposition treatment.
[0039] It should be noted that the vacuum heat treatment equipment includes, for example, a horizontal vacuum furnace, a vertical vacuum furnace, a rotary vacuum furnace and other applicable equipment.
[0040] In step S13, the inert atmosphere includes, for example, nitrogen, helium, argon, neon, xenon, or a mixture of one or two thereof, and the first cooled product is crushed and screened in the inert atmosphere to prevent oxidation or other side reactions of the first cooled product and protect the chemical purity of the material.
[0041] Specifically, the first cooled product is crushed and screened, the first cooled product is crushed by a pulverizing device, and then screened according to the average particle size of the powder to obtain the nano-silicon crystal cluster in-situ loaded lithium silicate material. During the screening process, the powder should be controlled to have a similar maximum particle size and minimum particle size as much as possible to ensure the consistency and stability of the product, thereby achieving the desired particle size. Among them, the crushing classification particle size D50 (median particle size) is 3 to 8 microns. For example, D50 can be but is not limited to 3 microns, 3.2 microns, 4.3 microns, 5.6 microns, 6.5 microns, 7.2 microns, and 8 microns. Dmax (maximum particle size) is less than 25 microns. For example, Dmax can be but is not limited to 16.4 microns, 18.1 microns, 19.6 microns, 20.8 microns, 23.6 microns, and 25 microns.
[0042] It should be noted that the pulverizing equipment includes one or a combination of two of a roller mill, a ball mill, a sand mill, a jaw crusher, and a jet mill.
[0043] The embodiment of the present invention uses silicon material and non-lithium silicate lithium material that can be decomposed into lithium oxide as raw materials, and adopts vacuum sublimation and controls the deposition temperature to achieve a small particle size of the silicon crystal cluster and in-situ symbiosis with the lithium silicate carrier, so that the nano-silicon crystal cluster in-situ loaded with lithium silicate material has good structural stability and ionic conductivity.
[0044] Specifically, step S2 specifically includes the following steps:
[0045] S21: placing the nano-silicon crystal cluster in-situ loaded with lithium silicate material into a reaction furnace, introducing a carbon source gas into the reaction furnace, heating at a temperature of 400° C. to 680° C., and keeping the temperature for 60 to 360 minutes, and cooling to obtain a second cooling product;
[0046] S22: subjecting the second cooling product and the acidic material to an acid washing treatment and a drying and screening treatment to obtain the nano-silicon crystal cluster in-situ loaded lithium silicate negative electrode material.
[0047] Specifically, in step S21, the nano-silicon cluster in-situ loaded lithium silicate material is placed in a carbon dioxide atmosphere furnace for example for carbon coating treatment. At this time, the residual lithium on the surface of the nano-silicon cluster in-situ loaded lithium silicate material reacts with carbon dioxide, and is in-situ reduced at low temperature to form a highly ordered carbon layer and lithium carbonate or other by-products. The highly ordered carbon layer covers the surface of the nano-silicon cluster in-situ loaded lithium silicate material, thereby obtaining a nano-silicon cluster in-situ loaded lithium silicate negative electrode material whose surface is coated with a low Id / Ig highly ordered conductive carbon layer.
[0048] It is worth mentioning that compared with the prior art using methane, ethane, propane, butane, acetylene, etc. as carbon source gas, the embodiment of the present invention uses carbon dioxide as the carbon source gas. The carbon layer structure generated by the carbon dioxide reaction is more orderly and has fewer defects, which improves the conductivity. At the same time, using carbon dioxide as the carbon source gas is conducive to reducing dependence on fossil fuels, reducing environmental impact, and improving the overall performance and sustainability of the material.
[0049] Specifically, the carbon coating treatment includes a heating treatment and a heat preservation treatment, wherein the temperature of the heating treatment is 400-680°C, for example, but not limited to 400°C, 450°C, 500°C, 550°C, 450°C, 600°C, 680°C. The heat preservation treatment time is 60-360 minutes, for example, but not limited to 60 minutes, 75 minutes, 120 minutes, 180 minutes, 240 minutes, 330 minutes, 360 minutes.
[0050] The embodiments of the present invention can significantly improve the electronic conduction efficiency of the material by carbon coating, which helps to improve the charge and discharge rate of the battery; secondly, the carbon layer can act as a barrier to reduce the direct contact and interaction between the material and the electrolyte, thereby reducing the degree of dissolution of the material by the electrolyte and inhibiting the occurrence of side reactions; at the same time, carbon coating can effectively alleviate the huge volume expansion of silicon during charging and discharging, prevent the collapse of the electrode structure, and thus significantly improve the cycle performance of the battery.
[0051] The second cooled product is a product obtained by cooling a nano-silicon crystal cluster in situ loaded with a lithium silicate negative electrode material coated with a low Id / Ig high-order conductive carbon layer on the surface. The purpose of the cooling treatment is to ensure the structural stability of the carbon layer and to prepare for the next step of acid washing and drying and screening. The temperature of the second cooled product is, for example, close to room temperature.
[0052] In step S22, the second cooled product is acid-washed with an acidic material to remove lithium carbonate or other byproducts that may remain on the surface of the material after step S21 and form mesopores in the carbon layer, effectively improving the electronic conductivity and ensuring the integrity of the conductive network for repeated charge and discharge. The material after acid washing is taken out and dried, and then sieved to ensure that the material has uniform particles, which helps to improve the charge and discharge performance and cycle stability of the battery.
[0053] The acidic material includes any one or more of hydrochloric acid, nitric acid, citric acid, and oxalic acid, and the concentration of the acidic material is 0.1-0.6 mol / L, for example, but not limited to 0.1 mol / L, 0.5 mol / L, and 0.6 mol / L. The acid washing treatment time is 20-90 minutes, for example, but not limited to 20 minutes, 30 minutes, 40 minutes, 60 minutes, and 90 minutes.
[0054] In the embodiment of the present invention, the nano-silicon cluster in-situ loaded lithium silicate material is subjected to carbon coating treatment to obtain the nano-silicon cluster in-situ loaded lithium silicate negative electrode material, so that the active lithium deposited on the surface of the powder in-situ reacts with gas phase CO2 at low temperature to obtain a low Id / Ig high-order conductive carbon layer coated on the surface of the nano-silicon cluster in-situ loaded lithium silicate material, which effectively improves the electronic conductivity, while avoiding the risk of high lithium activity to processing and storage, and significantly improves the process adaptability and stability of the material. Moreover, the reaction temperature of the carbon coating process is low, which can effectively inhibit the growth of silicon grains, thereby significantly reducing the deformation during the charge and discharge process, enhancing the structural stability, and improving the long cycle performance. In addition, the nano-silicon cluster in-situ loaded lithium silicate negative electrode material with a conductive carbon layer coated with a low Id / Ig high-order degree on the surface is acid washed to form a porous carbon coating layer structure containing mesopores, which can effectively absorb the stress caused by the volume expansion and contraction caused by the lithium insertion and extraction, improve the integrity of the coating layer structure, and ensure good electronic conductivity. Through the synergistic effect of the above two aspects, the nano-silicon composite negative electrode material has achieved high capacity, high initial efficiency, long cycle and excellent fast charging kinetics.
[0055] On the other hand, an embodiment of the present invention provides a nano-silicon crystal cluster in-situ loaded with lithium silicate negative electrode material, including the nano-silicon crystal cluster in-situ loaded with lithium silicate negative electrode material prepared by the methods described in S1 to S2 above.
[0056] Specifically, the nano-silicon cluster in-situ loaded lithium silicate negative electrode material prepared by S1~S2 includes a nano-silicon cluster, a lithium silicate carrier loaded on the surface of the nano-silicon cluster, and a carbon coating layer coated on the surface of the lithium silicate carrier, wherein the lithium silicate carrier includes any one or more of Li2SiO3 and Li4SiO4. The carbon coating layer has mesopores, and the average particle size of the mesopores is 3~7 nanometers, for example, but not limited to 3 nanometers, 3.8 nanometers, and 7 nanometers. The carbon content in the nano-silicon cluster in-situ loaded lithium silicate negative electrode material is 2~6%, and the average particle size of the nano-silicon cluster is 1~5 nanometers, for example, but not limited to 1 nanometer, 2.3 nanometers, and 5 nanometers. The porous carbon coating layer structure containing mesopores can effectively absorb the stress caused by volume expansion and contraction caused by lithium insertion and extraction, improve the integrity of the coating layer structure, and ensure good electronic conductivity. The carbon coating layer of the nano-silicon cluster in-situ loaded lithium silicate negative electrode material has mesopores, which contribute to the uniform distribution of the electrolyte and the rapid diffusion of lithium ions. At the same time, the mesoporous structure provides additional buffer space to accommodate the volume change of silicon during the charge and discharge process, reducing the resulting mechanical stress, thereby maintaining the integrity of the electrode structure. In addition, the mesoporous structure increases the contact area between the active material and the electrolyte, further promoting the transmission of electrons and improving the charge and discharge efficiency and cycle stability of the battery.
[0057] On the other hand, an embodiment of the present invention provides a battery, the battery is, for example, a lithium-ion battery, which includes, for example, an electrolyte, a separator, a lithium-ion battery positive electrode plate, and a lithium-ion battery negative electrode plate. Among them, the lithium-ion battery negative electrode plate includes, for example, a current collector and an active layer coated on the current collector, and the active layer includes the aforementioned nano-silicon crystal cluster in-situ loaded lithium silicate negative electrode material, which will not be described in detail here. In addition, the active layer also includes a conductive agent and an adhesive.
[0058] The present invention is further described in detail below in conjunction with specific embodiments. The embodiments are only used to explain the present invention but not to limit the scope of the present invention.
[0059] Example 1
[0060] Firstly, lithium carbonate and silicon are weighed according to the molar ratio of lithium element in the lithium material to silicon element in the silicon material of 2:1.06, the lithium carbonate and silicon are evenly mixed and added into a vacuum furnace, the vacuum pump is turned on to evacuate to a vacuum degree of 5 Pa, the temperature is raised to 1280°C, and the temperature of the deposition chamber is controlled to 650°C. After the reaction is completed, the reaction is vacuum cooled to 50°C, argon is introduced until the furnace pressure returns to normal pressure, the furnace door is opened, the material is taken out and put into a nitrogen-protected air flow mill, and the nano-silicon crystal clusters with a median particle size of 5.6 microns and a maximum particle size of 19.6 microns are obtained by crushing the nano-silicon crystal clusters to obtain an in-situ loaded lithium silicate material.
[0061] The nano-silicon crystal cluster in-situ loaded with lithium silicate material is then transferred to a rotary kiln, nitrogen gas is introduced to expel the air, and then CO2 is introduced to raise the temperature to 550°C and keep it warm for 240 minutes. After cooling to room temperature, a nano-silicon crystal cluster in-situ loaded with lithium silicate negative electrode material with a surface coated with a low Id / Ig and highly ordered conductive carbon layer is obtained.
[0062] Finally, the nano-silicon cluster in-situ loaded lithium silicate negative electrode material with a conductive carbon layer with low Id / Ig and high order on the surface was added to 0.1 mol / L hydrochloric acid and stirred for reaction for 30 minutes, and the nano-silicon cluster in-situ loaded lithium silicate negative electrode material was obtained by filtration, drying and sieving.
[0063] The nano-silicon crystal cluster prepared in Example 1 is in-situ loaded with lithium silicate negative electrode material, and its structure diagram is shown in Figure 2 .from Figure 2 It can be seen that the nano-silicon crystal cluster in-situ supports the lithium silicate negative electrode material, including the nano-silicon crystal cluster 100 (i.e. Figure 2 The multiple uniformly distributed dots located inside are shown), and the lithium silicate carrier 200 (i.e. Figure 2 The portion around the multiple dots in the inner circle) and the carbon coating layer 300 (i.e. Figure 2 The outermost layer shown), and the carbon coating layer 300 has mesopores 310 (i.e. Figure 2 multiple circular holes in the outermost layer).
[0064] The nano-silicon crystal cluster prepared in Example 1 in-situ loads lithium silicate negative electrode material, and its X-ray diffraction pattern is shown in Figure 3 .from Figure 3 It can be seen that the main crystal form of the material is Li2SiO3, and the corresponding Si crystal peak at around 28.5° is broadened, indicating that the crystallization strength of the silicon cluster is weak and the silicon grain size is small. Combined with the Scherrer formula, the grain size is 2.3 nanometers.
[0065] The nano-silicon crystal clusters prepared in Example 1 are in-situ loaded with lithium silicate negative electrode materials, and their pore size distribution diagram is shown in Figure 4 .from Figure 4 It can be seen that the pore size distribution of the material is uniform, and the pore size is about 3.8 nanometers.
[0066] Example 2
[0067] Firstly, lithium hydroxide and silicon are weighed according to the molar ratio of lithium element in the lithium material to silicon element in the silicon material of 2:1.04, the lithium hydroxide and silicon are uniformly mixed and added into a vacuum furnace, the vacuum pump is turned on to evacuate to a vacuum degree of 10 Pa, the temperature is raised to 1200°C, and the temperature of the deposition chamber is controlled to 500°C at the same time. After the reaction is completed, the reaction is vacuum cooled to 30°C, argon gas is introduced until the furnace pressure returns to normal pressure, the furnace door is opened, the material is taken out and put into a nitrogen-protected air flow mill, and the nano-silicon crystal clusters with a median particle size of 3.2 microns and a maximum particle size of 16.4 microns are crushed to obtain an in-situ loaded lithium silicate material.
[0068] The nano-silicon cluster in-situ loaded lithium silicate material is then transferred to a rotary kiln, nitrogen gas is introduced to expel the air, and then CO2 is introduced to raise the temperature to 680°C and keep it warm for 330 minutes, then cooled to room temperature to obtain a nano-silicon cluster in-situ loaded lithium silicate negative electrode material with a conductive carbon layer with low Id / Ig and high order on the surface.
[0069] Finally, the nano-silicon cluster in-situ loaded lithium silicate negative electrode material with a conductive carbon layer with low Id / Ig and high order on the surface was added to 0.1 mol / L hydrochloric acid and stirred for reaction for 30 minutes, and the nano-silicon cluster in-situ loaded lithium silicate negative electrode material was obtained by filtration, drying and sieving.
[0070] Example 3
[0071] Firstly, lithium acetate and silicon are weighed according to the molar ratio of lithium element in the lithium material to silicon element in the silicon material of 2:1.12, and the lithium acetate and silicon are uniformly mixed and added into a vacuum furnace, and the vacuum pump is turned on to evacuate to a vacuum degree of 2 Pa, and the temperature is raised to 1380°C, and the temperature of the deposition chamber is controlled to 450°C. After the reaction is completed, the reaction is vacuum cooled to 30°C, and argon gas is introduced until the furnace pressure returns to normal pressure. The furnace door is opened, the material is taken out and put into a nitrogen-protected air flow mill, and the nano-silicon crystal clusters with a median particle size of 7.2 microns and a maximum particle size of 23.6 microns are obtained by crushing to obtain an in-situ loaded lithium silicate material.
[0072] The nano-silicon crystal cluster in-situ loaded with lithium silicate material is then transferred to a rotary kiln, nitrogen gas is introduced to expel the air, and then CO2 is introduced to raise the temperature to 600°C and keep it warm for 75 minutes, then cooled to room temperature to obtain a nano-silicon crystal cluster in-situ loaded with lithium silicate negative electrode material with a conductive carbon layer with low Id / Ig and high order on the surface.
[0073] Finally, the nano-silicon cluster in-situ loaded lithium silicate negative electrode material with a conductive carbon layer with low Id / Ig and high order on the surface was added into 0.1 mol / L hydrochloric acid and stirred for 60 minutes, and the nano-silicon cluster in-situ loaded lithium silicate negative electrode material was obtained by filtration, drying and sieving.
[0074] Example 4
[0075] Firstly, lithium oxalate and silicon are weighed according to the molar ratio of lithium element in the lithium material to silicon element in the silicon material of 2:1.08, and the lithium oxalate and silicon are uniformly mixed and added into a vacuum furnace, and the vacuum pump is turned on to evacuate to a vacuum degree of 2 Pa, and the temperature is raised to 1300°C, and the temperature of the deposition chamber is controlled to 550°C. After the reaction is completed, the reaction is vacuum cooled to 40°C, and argon gas is introduced until the furnace pressure returns to normal pressure. The furnace door is opened, the material is taken out and put into a nitrogen-protected air flow mill, and the nano-silicon crystal clusters with a median particle size of 4.3 microns and a maximum particle size of 18.1 microns are obtained by crushing the nano-silicon crystal clusters to obtain an in-situ loaded lithium silicate material.
[0076] The nano-silicon crystal cluster in-situ loaded with lithium silicate material is then transferred to a rotary kiln, nitrogen gas is introduced to expel the air, and then CO2 is introduced to raise the temperature to 450°C and keep it warm for 120 minutes, then cooled to room temperature to obtain a nano-silicon crystal cluster in-situ loaded with lithium silicate negative electrode material with a conductive carbon layer with low Id / Ig and high order on the surface.
[0077] Finally, the nano-silicon cluster in-situ loaded lithium silicate negative electrode material with a conductive carbon layer with low Id / Ig and high order on the surface was added to 0.1 mol / L citric acid and stirred for reaction for 40 minutes, and the nano-silicon cluster in-situ loaded lithium silicate negative electrode material was obtained by filtration, drying and sieving.
[0078] Example 5
[0079] First, lithium aluminate and silicon are weighed according to the molar ratio of lithium element in the lithium material to silicon element in the silicon material of 2:1.05. After the lithium aluminate and silicon are evenly mixed, they are added to a vacuum furnace, and the vacuum pump is turned on to evacuate to a vacuum degree of 6 Pa, and the temperature is raised to 1400°C. At the same time, the temperature of the deposition chamber is controlled to be 500°C. After the reaction is completed, the vacuum is cooled to 50°C, and argon is introduced until the furnace pressure returns to normal pressure. The furnace door is opened, the material is taken out and put into a nitrogen-protected air flow mill, and the nano-silicon crystal clusters with a median particle size of 6.5 microns and a maximum particle size of 20.8 microns are crushed to obtain an in-situ loaded lithium silicate material.
[0080] The nano-silicon cluster in-situ loaded lithium silicate material is then transferred to a rotary kiln, nitrogen gas is introduced to expel the air, and then CO2 is introduced to raise the temperature to 500°C and keep it warm for 180 minutes, then cooled to room temperature to obtain a nano-silicon cluster in-situ loaded lithium silicate negative electrode material with a conductive carbon layer with low Id / Ig and high order on the surface.
[0081] Finally, the nano-silicon cluster in-situ loaded lithium silicate negative electrode material with a conductive carbon layer with low Id / Ig and high order on the surface was added to 0.5 mol / L hydrochloric acid and stirred for 60 minutes, and the nano-silicon cluster in-situ loaded lithium silicate negative electrode material was obtained by filtration, drying and sieving.
[0082] In order to better illustrate the advantages of the embodiments of the present invention, the electrochemical performance of the nano-silicon crystal clusters in-situ loaded with lithium silicate negative electrode materials prepared in Examples 1 to 5 of the present invention was tested. The test methods used in the following experimental examples are conventional methods unless otherwise specified; the materials, reagents, etc. used are reagents and materials that can be obtained from commercial channels unless otherwise specified.
[0083] Comparative Example 1
[0084] Except that the lithium silicate in Example 1 is replaced by lithium carbonate, other conditions are the same as Example 1.
[0085] Comparative Example 2
[0086] Except that the molar ratio of the lithium element in the lithium material to the silicon element in the silicon material in Example 1 is replaced from 2:1.06 to 2:0.9, other conditions are the same as Example 1.
[0087] Comparative Example 3
[0088] Except that the temperature of the deposition chamber in Example 1 is adjusted to 680° C., other conditions are the same as those in Example 1.
[0089] Comparative Example 4
[0090] Except that the carbon coating treatment by introducing acetylene into the rotary kiln is replaced by the carbon coating treatment by introducing CO2 into the rotary kiln, other conditions are the same as those in Example 1.
[0091] 1. Experimental object: The nano-silicon crystal clusters prepared in Examples 1 to 5 of the present invention are in-situ loaded with lithium silicate negative electrode materials; the nano-silicon crystal clusters prepared in Comparative Examples 1 to 4 are in-situ loaded with lithium silicate negative electrode materials.
[0092] 2. Experimental methods:
[0093] ①The test method for the mass content of carbon element is as follows:
[0094] The mass content of amorphous carbon in the nano-silicon cluster in-situ loaded lithium silicate negative electrode materials in Examples 1 to 5 and Comparative Examples 1 to 4 was tested by a high-frequency infrared carbon-sulfur analyzer.
[0095] ②XRD test method is as follows:
[0096] The nano-silicon crystal clusters in situ loaded with lithium silicate negative electrode materials in Examples 1 to 5 and Comparative Examples 1 to 4 were made into sheets and tested using an X-ray diffraction analyzer. Angle range: 10 to 90°, scanning mode: step scanning, select slit width 1.0, and set voltage 40kW and current 40mA. The measured data were analyzed using Jade 6.5 software, and the material composition was confirmed by comparing PDF cards. Characterized by an X-ray diffraction analyzer, characteristic peaks can be observed in the range of 27.5° to 29.5°, 46.3° to 48.3°, and 55.0° to 57.0°; and the Si (111) peak at 28.6° was fitted, and the half-peak width FWHM was obtained, and then the size of the Si crystallite was calculated using the Scherrer formula.
[0097] ③The test method for silicon crystal cluster content is as follows:
[0098] Take 10g of the nano-silicon clusters in situ loaded with lithium silicate negative electrode material in Examples 1-5 and Comparative Examples 1-4 respectively, add them to 50g of 1mol / L hydrochloric acid solution, stir and disperse them at room temperature for 6h, filter, and wash the collected filter cakes with deionized water and anhydrous ethanol for 3 times, place them in an oven at 90℃ with a vacuum degree of -0.085MPa for 6h, convert lithium silicate into silicic acid, and weigh the acidified mass to be x. Then take 5g and transfer them to a nitrogen-protected tubular furnace for heat treatment at 600℃ for 2h, cool them out of the furnace, convert silicic acid into SiO2, and weigh the mass of silicon dioxide to be y. Weigh 2g of the material out of the furnace, then add 10g of 20% hydrogen fluoride ethanol-water (the volume ratio of ethanol to water is 1:5) solution to disperse for 2h to remove SiO2, and wash the collected filter cake with deionized water and anhydrous ethanol for 3 times, place it in an oven at 60℃ and vacuum degree of -0.085MPa for 4h, and weigh to obtain the mass z of the silicon crystal cluster. The content of the silicon crystal cluster is calculated as =z / 2 / (y / 5) / (x / 10).
[0099] ④ The Raman test method of nano-silicon crystal cluster in-situ loaded lithium silicate negative electrode material is as follows:
[0100] Raman spectroscopy was used to test the nano-silicon cluster in-situ loaded lithium silicate negative electrode materials in Examples 1 to 5 and Comparative Examples 1 to 3. The Raman spectra were firstly baseline-removed and then peak-searched using LabSpec software. The peak-searching parameters were adjusted to make the peak at about 1350 cm -1 The D peak at about 1600 cm -1 After fixing the peak position and performing fitting, the peak height I of the desired peak position can be obtained.
[0101] ⑤ The pore size method of nano-silicon cluster in-situ loading of lithium silicate negative electrode material is as follows:
[0102] The average pore size of the pores of the nano-silicon clusters in-situ loaded with lithium silicate negative electrode materials in Examples 1 to 5 and Comparative Examples 1 to 3 was tested using an American Micromeritics ASAP 2460 fully automatic specific surface and porosity analyzer. The gas used in the test was CO2 or N2.
[0103] ⑥The electrochemical performance test was carried out using the following method:
[0104] The materials prepared in Examples 1 to 5 and Comparative Examples 1 to 4 were used as nano-silicon cluster in-situ loaded lithium silicate negative electrode materials, mixed with a binder and a conductive agent in a mass ratio of 90:5:5, and an appropriate amount of deionized water was added as a dispersant to prepare a slurry, which was then coated on a 10-micron copper foil by a coating machine, and then dried at 90°C in a vacuum (-0.1MPa) for 6 hours. The rollers were compacted to control the compaction density at 1.50 g / cm 3 , and then use a punching machine to make a disc with a diameter of 14mm, dry it in vacuum (-0.1MPa) at 90℃ for 5h, weigh it and calculate the weight of the active material. Assemble CR2430 button cells in a glove box, use metal lithium sheets as counter electrodes, polypropylene microporous membranes as separators, 1mol / L lithium hexafluorophosphate is dissolved in ethylene carbonate and diethyl carbonate in a volume ratio of 1:1, and an electrolyte with 5.0% fluoroethylene carbonate is added. The battery was left to stand at room temperature for 12h, and then tested by constant current charge and discharge on the blue power test system, charging to 0.005V at 0.1C, then charging to 0.005V at 0.05C, and then charging to 0.005V at 0.02C. After standing for 10 minutes, discharge to 1.5V at 0.1C, and test the first reversible capacity and first efficiency at 0.1C;
[0105] ⑦ The cycle retention rate test and calculation method are as follows:
[0106] The battery that has completed the first reversible capacity and first efficiency test steps is charged to 0.005V at 0.1C, and then discharged to 1.5V at 0.2C. The cycle is repeated for 100 weeks to measure the 100-week discharge capacity. The cycle capacity retention rate is: 100-week cycle discharge capacity / first discharge capacity*100%; fast charging capability: (first cycle 0.1C lithium insertion capacity) / (first cycle 0.1C lithium insertion capacity+0.05C lithium insertion capacity+0.02C lithium insertion capacity)*100%.
[0107] The test results are shown in Tables 1 and 2. Among them, Table 1 is a data comparison of silicate types, silicon grains, silicon cluster content, carbon content, Id / Ig and pore size of Examples 1 to 5 and Comparative Examples 1 to 4. A lower Id / Ig ratio indicates a higher and more ordered structure, which helps to improve electronic conductivity and ion diffusion performance, thereby improving the charge and discharge rate and cycle stability of the battery. Table 2 is a data comparison of the 0.1C first reversible capacity, first efficiency, 100-week cycle retention rate and fast charging capability of Examples 1 to 5 and Comparative Examples 1 to 4.
[0108] Table 1 Comparison of silicate types, silicon grains, silicon cluster content, carbon content, Id / Ig and pore size between Examples 1 to 5 and Comparative Examples 1 to 4
[0109]
[0110] Table 2 Comparison of the 0.1C first reversible capacity, first efficiency, 100-cycle retention rate and fast charging capability of Examples 1 to 5 and Comparative Examples 1 to 4
[0111]
[0112] Conclusion: As can be seen from the comprehensive test data in Tables 1 and 2, the material prepared by the present application has a high silicon content component, small silicon grains, high quality carbon coating layer, good conductivity, combined with the reasonable regulation of the pores of the carbon layer, the finally prepared material has the characteristics of high capacity, high first efficiency, excellent cycle performance and good fast charging performance.
[0113] The present invention adopts silicon single substance or silicon alloy as silicon material, adopts lithium oxide and non-lithium silicate material that can be decomposed into lithium oxide as lithium material, mixes silicon material and lithium material evenly, and then uses vacuum sublimation to it, and controls the deposition temperature, so as to realize small particle size of silicon cluster, and make nano silicon cluster evenly loaded on lithium silicate carrier, nano silicon reduces absolute volume expansion, silicon and lithium silicate are integrated, evenly distributed and have high bonding strength, ensure the firmness of overall structure, effectively improve long cycle performance, thereby extending the service life of battery and maintaining performance stability. In addition, lithium silicate around nano silicon, as an excellent ion conductor, has good ion conductivity, helps to improve kinetic rate performance, helps the battery to maintain good performance during rapid charge and discharge, that is, improves the charge and discharge rate of battery. Furthermore, the present invention forms a highly ordered, low Id / Ig conductive carbon layer on the surface of lithium silicate negative electrode material loaded by nano silicon cluster through carbon coating treatment. This treatment not only improves electronic conductivity, but also reduces the processing and storage risks of active lithium. Low-temperature carbon coating inhibits silicon grain growth, reduces charge-discharge deformation, and enhances structural stability. The mesoporous carbon layer after acid washing effectively alleviates volume expansion, ensures electronic conductivity, and achieves high capacity, high efficiency, long cycle life, and excellent fast charging performance.
[0114] In summary, the nano-silicon cluster in-situ loaded lithium silicate negative electrode material provided by the embodiment of the present invention has the advantages of high first efficiency, long cycle and excellent fast charging kinetics performance.
[0115] It can be understood that the aforementioned embodiments are merely exemplary descriptions of the present invention. The technical solutions of the various embodiments can be arbitrarily combined and used in combination, provided that the technical features do not conflict, the structures do not contradict, and the purpose of the present invention is not violated.
[0116] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a nano-silicon crystal cluster in-situ loaded lithium silicate negative electrode material, characterized in that: include: The lithium material and the silicon material are mixed evenly according to a preset ratio, and then subjected to vacuum heat treatment and deposition treatment to obtain a nano-silicon crystal cluster in-situ loaded lithium silicate material; The preset ratio is a molar ratio of lithium in the lithium material to silicon in the silicon material, the preset ratio ranges from 2:(1.03 to 1.15), and the temperature of the deposition process is 400 to 650° C.; The nano-silicon crystal cluster in-situ loaded lithium silicate material is subjected to carbon coating treatment to obtain the nano-silicon crystal cluster in-situ loaded lithium silicate negative electrode material; the carbon source gas used in the carbon coating treatment is carbon dioxide; The content of nano-silicon clusters in the nano-silicon cluster in-situ loaded lithium silicate negative electrode material is 40-50%, and the Id / Ig of the nano-silicon cluster in-situ loaded lithium silicate negative electrode material is 0.12-0.6; The silicon material includes any one or more of silicon and silicon alloys, and the lithium material includes any one or more of lithium oxide and non-silicate materials. The non-silicate material is a material that can obtain lithium oxide after heat treatment.
2. The method for preparing the nano-silicon crystal cluster in-situ loaded lithium silicate negative electrode material according to claim 1, characterized in that: The lithium material and the silicon material are mixed uniformly according to a preset ratio, and then vacuum heat treatment and deposition treatment are performed to obtain the nano-silicon crystal cluster in-situ loaded lithium silicate material, specifically comprising: The lithium material and the silicon material are mixed uniformly according to the preset ratio to obtain a first mixed material; The first mixed material is placed in a vacuum furnace for vacuum heat treatment at a temperature of 1150-1450° C., and the deposition treatment is performed at a temperature of 400-650° C., and a first cooled product is obtained after cooling, wherein the vacuum degree of the vacuum furnace is less than 12 Pa, and the temperature of the first cooled product is 20-60° C.; The first cooling product is crushed and sieved in an inert atmosphere to obtain the nano-silicon crystal cluster in-situ loaded lithium silicate material.
3. The method for preparing the nano-silicon crystal cluster in-situ loaded lithium silicate negative electrode material according to claim 2, characterized in that: The inert atmosphere includes any one or more of nitrogen, helium, argon, neon, and xenon. The median particle size of the in-situ loaded lithium silicate material of the nano-silicon cluster is 3 to 8 microns; the lithium material includes any one or more of lithium carbonate, lithium hydroxide, lithium oxalate, lithium acetate, lithium citrate, lithium borate, and lithium aluminate.
4. The method for preparing the nano-silicon crystal cluster in-situ loaded lithium silicate negative electrode material according to claim 1, characterized in that: The step of subjecting the nano-silicon crystal cluster in-situ loaded with lithium silicate material to carbon coating to obtain the nano-silicon crystal cluster in-situ loaded with lithium silicate negative electrode material specifically comprises: The nano-silicon crystal cluster in-situ loaded with lithium silicate material is placed in a reaction furnace, the carbon source gas is introduced into the reaction furnace, heated at a temperature of 400° C. to 680° C., and kept warm for 60 to 360 minutes, and then cooled to obtain a second cooling product; The second cooling product and the acidic material are subjected to acid washing treatment and drying and screening treatment to obtain the nano-silicon crystal cluster in-situ loaded lithium silicate negative electrode material.
5. The method for preparing the nano-silicon crystal cluster in-situ loaded lithium silicate negative electrode material according to claim 4, characterized in that: The acidic material includes any one or more of hydrochloric acid, nitric acid, citric acid, and oxalic acid. The concentration of the acidic material is 0.1-0.6 mol / L. The time of the acid washing treatment is 20-90 minutes.
6. The method for preparing the nano-silicon crystal cluster in-situ loaded lithium silicate negative electrode material according to any one of claims 1 to 5, characterized in that: The carbon content of the nano-silicon crystal cluster in-situ loaded lithium silicate negative electrode material is 2-6%, and the nano-silicon crystal cluster in-situ loaded lithium silicate negative electrode material has mesopores, and the average particle size of the mesopores is 3-7 nanometers.
7. A nano-silicon crystal cluster in-situ loaded with lithium silicate negative electrode material, characterized in that: Prepared by the method for preparing a nano-silicon crystal cluster in-situ loaded lithium silicate negative electrode material as claimed in any one of claims 1 to 6; The nano-silicon crystal cluster in-situ loaded lithium silicate negative electrode material comprises: A carbon coating layer, a lithium silicate carrier coated by the carbon coating layer, and a nano-silicon crystal cluster located on the lithium silicate carrier; Wherein, the lithium silicate carrier includes any one or more of Li2SiO3 and Li4SiO4, and the average particle size of the nano-silicon crystal cluster is 1 to 5 nanometers.
8. A battery, characterized in that: It comprises a negative electrode plate of a lithium ion battery, wherein the negative electrode plate of the lithium ion battery comprises a current collector and an active layer coated on the current collector, wherein the active layer comprises the nano-silicon crystal cluster in-situ loaded lithium silicate negative electrode material prepared by the preparation method of the nano-silicon crystal cluster in-situ loaded lithium silicate negative electrode material according to any one of claims 1 to 6.
Citation Information
Patent Citations
Silicon-carbon negative electrode material and preparation method thereof, electrode plate and lithium ion battery
CN118693264A