Chemical platinum plating solution, preparation method thereof and application thereof in chemical platinum plating of wafers
By using a chemical plating solution of ethylenediamine platinum chloride or ethylenediamine platinum iodide and thiourea dioxide, combined with specific additives, the problems of uniformity and density of platinum metal films were solved, resulting in semiconductor wafer products with high corrosion resistance and high-precision conductivity.
Patent Information
- Application Number
- CN202411154637.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-22
AI Technical Summary
Existing electroless platinum plating solutions cannot achieve uniform distribution, morphology, purity, and density control of platinum metal films, resulting in micro-pinholes and micro-cracks in the coating, which cannot meet the high-precision conductivity and high-quality electronic signal transmission performance of semiconductor wafer electronic products.
Ethylenediamine platinum chloride or ethylenediamine platinum iodide is used as a cyclic platinum salt, combined with thiourea dioxide as a reducing agent, and compounds containing amino and carboxyl groups are added as additives to form a stable cyclic complex. The pH value of the electroless platinum plating solution is controlled at 9.5~10.5, and the concentration of complexing agent and additives is optimized to ensure the uniformity and density of the platinum coating.
This method achieves excellent uniform distribution, morphology, and density of platinum metal thin films, improves the corrosion resistance and conductivity of the coating, and ensures high-precision conductivity and high-quality electronic signal transmission performance of semiconductor wafer products.
Smart Images

Figure CN118668195B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of wafer chemical platinum plating, and in particular relates to a chemical platinum plating solution, a preparation method thereof and an application thereof in wafer chemical platinum plating. Background Art
[0002] During the micromachining process of the semiconductor wafer surface, a redox chemical reaction occurs between the reducing agent and platinum ions on the wafer surface to form a platinum metal film. This method requires precise control of the uniform distribution, morphology, purity and density of the platinum metal film in order to obtain a nanostructured electronic transmission line with high corrosion resistance, high-precision conductivity and high-quality electronic signal transmission performance.
[0003] Common reducing agents used in chemical platinum plating solutions in the prior art include boron hydride compounds, aminoborane compounds, formaldehyde, hydrazine compounds or o-diphenol compounds, among which some reducing agents have strong reducing properties and are difficult to control the reaction process, resulting in uneven coating.
[0004] In the prior art, CN109415812A uses a reducing agent including potassium formate and a platinum salt including potassium tetrachloride to prepare a chemical platinum plating solution; CN110621806A uses sodium borohydride and tetraamine platinum nitrate to prepare a chemical platinum plating solution; JP2018-104755A uses sodium borohydride and dinitrodiammine platinum to prepare a chemical plating solution; JP2016-160505A uses sodium borohydride and ammonium chloroplatinate to prepare a chemical plating solution, but all of them cannot achieve uniform distribution, excellent morphology, high purity and high density of the platinum metal coating (see Comparative Examples 3 to 7 of the present invention), cannot solve the micropinholes and microcracks in the platinum coating, cannot meet the deposition formation of electronic transmission lines on the surface nanostructures of wafers, and cannot achieve high-precision conductivity and high-quality electronic signal transmission performance of platinum-plated semiconductor wafer products.
[0005] On the other hand, after preliminary searching, no prior art was found regarding the use of thiourea dioxide as a reducing agent in the preparation of chemical platinum plating solutions, nor was any prior art found regarding the use of cyclic platinum salts such as ethylenediamineplatinum chloride or ethylenediamineplatinum iodide in the preparation of chemical platinum plating solutions.
[0006] In summary, in the field of wafer chemical platinum plating technology, there is an urgent need to find a chemical platinum plating solution to solve the problems of uncontrollable uniform distribution, morphology, purity and density of chemical platinum plating films, so as to meet the market demand for the production of semiconductor wafer electronic products with high corrosion resistance, high-precision conductivity and high-quality electronic signal transmission performance. Summary of the invention
[0007] [Technical issues]
[0008] Provided is a chemical plating platinum solution which can be applied to nano-precision manufacturing of semiconductor wafer electronic products. The formed platinum metal film has excellent uniform distribution, morphology, purity and density, and obtains wafer electronic products with high corrosion resistance, high-precision conductivity and high-quality electronic signal transmission performance.
[0009] [Technical concept]
[0010] The present invention has developed a chemical platinum plating solution for wafers with stable performance and long service life. Different from the prior art, the present invention adopts cyclic platinum salts such as ethylenediamine platinum chloride (II) or ethylenediamine platinum iodide (II), and preferably a diamino compound that can form a cyclic complex (such as Formula 1) with platinum (II) as a complexing agent, which is conducive to moving the equilibrium reaction (such as reaction 1) of the reaction of generating the cyclic complex and the dissociation reaction of the cyclic complex toward the direction of generating a stable cyclic complex, thereby facilitating the maintenance of the stability of the cyclic complex in the chemical platinum plating solution. The stability of the cyclic complex is improved, that is, the decomposition rate of the cyclic complex is reduced. When the decomposition rate of the cyclic complex is less than the rate of obtaining electrons on the cathode surface and being reduced and deposited as zero-valent platinum (0), the deposited platinum particles are uniformly and orderly arranged, and the formed platinum metal lattice is dense and defect-free, and an excellent platinum coating is obtained; therefore, the formed platinum coating has excellent morphology, uniform distribution and excellent density, and the produced wafer electronic products have excellent corrosion resistance, high-precision conductivity and high-quality electronic signal transmission performance;
[0011] Furthermore, through the optimization of the additive, it is found that when the additive contains a carboxyl group and at least one of an α-amino group, a β-amino group or a γ-amino group, it can be seen from the structural characteristics of the α-amino group, the β-amino group and the γ-amino group of the additive that the N in the amino group has a strong electronegativity and can attract the platinum (II) positive ion to form an N-Pt covalent bond; at the same time, the carboxylic acid hydroxyl oxygen O also has a strong electronegativity and attracts the platinum (II) positive ion to form an O-Pt covalent bond; when the formed N-Pt and O-Pt covalent bonds are the same Pt, the formed compound is a cyclic complex with excellent stability (such as Formula 2), which also helps to alleviate and maintain the decomposition rate of the cyclic complex lower than the rate of obtaining electrons on the cathode surface and being electrolytically reduced and deposited as zero-valent platinum (0), thereby facilitating the maintenance of the stability of the chemical platinum plating solution, and can further promote the platinum coating to have better compactness and excellent corrosion resistance;
[0012] Furthermore, the present invention optimizes the concentration of the complexing agent and the additive to maintain the decomposition rate of the cyclic complex lower than the rate at which the cyclic complex obtains electrons on the cathode surface and is electrolytically reduced and deposited as zero-valent platinum (0), thereby facilitating the maintenance of the stability of the chemical platinum plating solution, and ultimately achieving a platinum coating with a nano-scale dense morphology, uniform distribution, extremely high purity and excellent density, and producing a platinum-plated semiconductor wafer product with a dense platinum coating, uniform film thickness distribution and high purity.
[0013]
[0014] Formula 1
[0015]
[0016] Reaction one.
[0017]
[0018] Formula 2
[0019] On the other hand, the present invention finds that the carbonyl oxygen C=O in the additive α-amino acid and its derivatives, β-amino acid and its derivatives or γ-aminobutyric acid and its derivatives has strong electron-withdrawing property, and can form OH hydrogen bond with the amino hydrogen of the thiourea dioxide isomer formamidine sulfinic acid in aqueous solution; the oxygen S=O in the thiourea dioxide isomer formamidine sulfinic acid also has strong electron-withdrawing property, and can also form OH hydrogen bond with the amino hydrogen of the additive α-amino acid and its derivatives, β-amino acid and its derivatives or γ-aminobutyric acid and its derivatives; therefore, the use of additives in the present invention can improve the stability of thiourea dioxide in solution. The chemical platinum plating solution of the present invention creatively uses thiourea dioxide as a reducing agent, and utilizes the specific interaction between thiourea dioxide and the additive α-amino acid and its derivatives, β-amino acid and its derivatives or γ-aminobutyric acid and its derivatives to improve the stability of thiourea dioxide in the chemical platinum plating solution.
[0020] The present invention also found that when the pH value of the chemical platinum plating solution is 7, the stability of thiourea dioxide in the solution state is high, and even if the semiconductor wafer plating part is placed in the chemical platinum plating solution, it is not easy to reduce the platinum ions to platinum. The chemical platinum plating solution of the present invention has a strong reducing property under alkaline and heating conditions, such as at a pH value of 9.5 to 10.5 and a temperature of 40°C to 60°C. Therefore, by controlling the pH value range of the chemical platinum plating solution to 9.5 to 10.5, the thiourea dioxide isomer formamidine sulfinic acid is prompted to react with six equivalents of hydroxide, so that it can immediately react with the platinum salts in the solution to deposit platinum metal, and ethylenediamine platinum chloride can be reduced to metallic platinum. At the same time, the product includes ethylenediamine (reaction equation such as reaction 2) in addition to urea, sodium sulfate, sodium chloride and water; wherein ethylenediamine can be repeatedly recycled in the chemical platinum plating solution. Among them, the thiourea dioxide isomer formamidine sulfinic acid first generates sulfoxylate under alkaline conditions. The sulfoxylate has a strong reducing property and can immediately react with platinum salts in the solution to precipitate platinum metal.
[0021]
[0022] Reaction 2.
[0023] [Technical solution]
[0024] On the one hand, a chemical platinum plating solution is provided, which comprises: a cyclic platinum salt, a reducing agent, a complexing agent, a conductive salt, a buffer, a pH regulator and ultrapure water; wherein: the concentration of the cyclic platinum salt is, in terms of platinum, 1-15 g / L; the mass ratio of the cyclic platinum salt: the reducing agent: the complexing agent is 1: (0.7-1.9): (1.9-4.4); the reducing agent is thiourea dioxide; the complexing agent is a diamino compound capable of forming a cyclic complex with platinum (II); the conductive salt is an ammonium carboxylate compound; the buffer is a polycarboxylate compound;
[0025] The pH adjusting agent is configured to: during chemical plating, adjust the pH value of the chemical platinum plating solution to 9.5-10.5; when chemical plating is not required, adjust the pH value of the chemical platinum plating solution to 7.
[0026] Ultrapure water refers to water that does not contain any atoms except oxygen and hydrogen, with a purity of 99.9999999% and an impurity content of less than 0.01 ppm.
[0027] In some embodiments, the chemical plating platinum solution further includes: an additive; the additive is a compound containing an amino group and a carboxyl group that can form a cyclic complex with platinum (II) through the amino group and the carboxyl group; the mass ratio of cyclic platinum salt: reducing agent: complexing agent: additive is 1: (0.7~1.9): (1.9~4.4): (0.038~0.308).
[0028] In some embodiments, the cyclic platinum salt includes at least one of ethylenediamine platinum chloride or ethylenediamine platinum iodide.
[0029] In some embodiments, the complexing agent includes at least one of ethylenediamine, ethylenediamine hydrochloride, ethylenediamine sulfate, 1,3-propylenediamine, 1,3-propylenediamine hydrochloride, 1,4-butylenediamine dihydrochloride, 1,2-diaminocyclohexane, diethylenediamine, or triethylenediamine.
[0030] In some embodiments, the additive is at least one of α-amino acids and their derivatives, β-amino acids and their derivatives, or γ-aminobutyric acid and its derivatives.
[0031] In some embodiments, the α-amino acid and its derivatives include: at least one of glycine sodium salt hydrate, 2-amino-3-hydroxypropionic acid, N-(2-aminoethyl)glycine, N-(3-aminopropyl)glycine, 2,3-diaminopropionic acid hydrochloride, sodium N-hydroxymethylglycine, 3-(4-pyridyl)-D-alanine dihydrochloride, DL-serine, sarcosine, sodium sarcosinate, 2,4-diaminobutyric acid and 2,5-diaminopentanoic acid.
[0032] In some embodiments, the β-amino acid and its derivatives include: at least one of β-alanine, DL-alanine, α-fluoro-β-alanine, β-alanine hydroiodide, β-alanine methyl ester hydrochloride, β-alanine ethyl ester hydrochloride, N-benzyloxycarbonyl-β-alanine, β-N-methylamino-L-alanine and L-β-homoalanine hydrochloride.
[0033] In some embodiments, the conductive salt includes at least one of ammonium acetate, 2-hydroxyammonium acetate, ammonium propionate, 2-hydroxypropionic acid monoammonium salt, ammonium malonate, 3-methylammonium butyrate or ammonium succinate and derivatives thereof.
[0034] In some embodiments, the buffer comprises at least one of citric acid, diammonium hydrogen citrate, sodium citrate, potassium citrate, ammonium citrate, tartaric acid, sodium tartrate, potassium tartrate, ammonium tartrate, diammonium ethylenediaminetetraacetate, and disodium ethylenediaminetetraacetate.
[0035] On the other hand, a method for preparing the above-mentioned chemical platinum plating solution is provided, which comprises the following steps:
[0036] (1) preparing the start-up liquid A: based on the final concentration of each component in the chemical platinum plating solution, completely dissolving the complexing agent, the conductive salt and the cyclic platinum salt in a portion of the ultrapure water under heating and stirring conditions, and adjusting the pH value of the solution to 7 using the pH adjusting agent to obtain the start-up liquid A;
[0037] (2) preparing the start-up liquid B: based on the final concentration of each component in the chemical plating platinum solution, under heating and stirring conditions, completely dissolving the buffer in another portion of ultrapure water, adjusting the pH value of the solution to 7 to obtain a buffer solution, completely dissolving the reducing agent in the buffer solution, adjusting the pH value of the solution to 7, and obtaining the start-up liquid B;
[0038] (3) Compounding: Slowly add the pre-bottle liquid B to the pre-bottle liquid A, mix well, and test the solution to a pH value of 7. Use the remaining ultrapure water to make up the volume. During chemical plating, adjust the solution pH value to 10 to obtain the chemical plating platinum solution.
[0039] In some embodiments, the chemical plating platinum solution contains an additive. When preparing the start-up solution B in step (2), the buffer is completely dissolved in another portion of ultrapure water, and then the additive is added. After all the additives are dissolved and mixed evenly, the pH value of the solution is adjusted to 7. The reducing agent is then completely dissolved in the resulting solution, and the pH value of the solution is adjusted to 7 to obtain the start-up solution B.
[0040] On the other hand, the invention provides a use of the above-mentioned chemical platinum plating solution in preparing platinum-plated semiconductor wafer products.
[0041] In some embodiments, a method for forming a platinum nanostructure coating on a semiconductor wafer surface is provided, using the aforementioned chemical platinum plating solution as a processing solution; the method comprises the following steps:
[0042] The semiconductor wafer to be electrolessly plated is installed in an electroless plating device after degreasing and acid activation treatment, and the electroless platinum plating solution is used to electrolessly plate for a certain period of time at a temperature of 40-60°C and a pH value of 9.5-10.5, so as to obtain a semiconductor wafer product with a platinum film thickness of the target platinum film; wherein:
[0043] During the batch plating continuous production process, the concentration of each component in the chemical platinum plating solution and the pH value of the chemical platinum plating solution are monitored, and the automatic replenishing equipment is linked to maintain the composition of the chemical platinum plating solution basically unchanged during the plating process;
[0044] When it is necessary to stop the plating work, the pH value of the chemical platinum plating solution is monitored, and the linked automatic replenishing equipment adjusts the pH value of the chemical platinum plating solution to 7 by adding the pH regulator; when it is necessary to continue the plating work, it is only necessary to monitor the pH value of the chemical platinum plating solution, and the linked automatic replenishing equipment adjusts the pH value of the chemical platinum plating solution to 9.5~10.5 by adding the pH regulator.
[0045] When the pH of the electroless platinum plating solution is too low, less than 7.5, the OH group used to attack the CS chemical structure in the sulfinic acid of the thiourea dioxide isomer isoformamidine -If the concentration is too low, the alkalinity required is insufficient, so the equilibrium of reaction II cannot move quickly toward the formation of platinum metal, and even the expected reaction result cannot occur. On the contrary, when the pH of the chemical plating solution is too high, greater than 12.5, the high concentration of OH - The fierce attack leads to a too-rapid reaction, producing various complex reaction products, and the expected semiconductor wafer product with platinum coating deposition cannot be obtained.
[0046] [Beneficial Effects]
[0047] (1) The present invention provides a chemical platinum plating solution, which can be applied to the nano-precision manufacturing of semiconductor wafer electronic products. The formed platinum metal film has excellent uniform distribution, morphology, purity and density, and obtains wafer electronic products with high corrosion resistance, high-precision conductivity and high-quality electronic signal transmission performance;
[0048] (2) Compared with the existing chemical plating platinum solution, rapid chemical plating of platinum can be achieved at a lower temperature of 40°C to 60°C. The speed of chemical plating of the present invention is faster, and the time required to complete the platinum coating of the same thickness is short;
[0049] (3) The chemical platinum plating solution of the present invention can control the occurrence of chemical platinum plating reaction by adjusting the pH value. Specifically, during chemical plating, the pH value of the chemical platinum plating solution is adjusted to 9.5-10.5; when chemical plating is not required, the pH value of the chemical platinum plating solution is adjusted to 7. Therefore, the chemical platinum plating solution of the present invention is easy to operate. BRIEF DESCRIPTION OF THE DRAWINGS
[0050] Figure 1 Schematic diagram of wafer plating, chip unit and film thickness test position; 10-semiconductor wafer plating, 11-chip unit;
[0051] Figure 2 for Figure 1 A magnified schematic diagram of the test position of the platinum coating thickness of the middle chip unit; wherein, the central black dot ● of the 12-chip unit;
[0052] Figure 3 is an electron microscope photograph of the platinum coating of Example 28;
[0053] Figure 4 This is an electron microscope photograph of the platinum coating of Comparative Example 2. DETAILED DESCRIPTION
[0054] Substrate: The structure of the semiconductor wafer plated article 10 to be processed by chemical plating is as follows Figure 1As shown. A wafer with a diameter of 8 inches and a thickness of 0.35 mm is used as the raw material; it has a single-sided experimental piece with 52 chemical plating areas (chip unit 11), and the circuit area of each chemical plating area is 0.5×10×7=35 mm 2 The total surface area of the chemical plating area of the semiconductor wafer plating part 10 is 52×35 mm 2 =1820 mm 2 .
[0055] Only 52 chemically plated areas of the semiconductor wafer plated part 10 to be processed by chemical plating can undergo a reduction reaction with the chemical platinum plating solution, thereby preparing a platinum-plated semiconductor wafer product.
[0056] Test method:
[0057] Platinum coating thickness test: Tested using FischerSCOPE X-RAY XDV-SDD detector manufactured by Fischer Figure 1 The thickness of the platinum coating at the central black dot ● of each chemical plating area of the semiconductor wafer plating part I to VII is as follows: Figure 2 As shown. Analyze the maximum value (Max), minimum value (Min), average value (Ave.), Max-Min and film thickness error of the platinum coating thickness data. Among them:
[0058] The coordinates of the central black dot of each chemical plating area are: 6 (3.24 mm, 18.38 mm), 10 (3.24, 10.16), 14 (3.24, 6.52) in column I; 3 (5.55, 16.54), 7 (5.55, 12.86), 13 (5.55, 7.43), 17 (5.55, 3.80) in column II; 2 (7.86 mm, 17.46 mm), 6 (7.86, 18.38), 10 (7.86, 10.16), 14 (7.86, 6.52), 18 (7.86, 2.89) in column III; 1 (10.16 mm, 18.35 , 15 (10.16, 5.61), 19 (10.16, 1.97); for column V, 4 (12.47 mm, 15.62 mm), 8 (12.47, 12), 12 (12.47, 8.36), 16 (12.47, 4.72); for column VI, 3 (14.78 mm, 16.54 mm), 7 (14.78, 12.90), 13 (12.47, 7.44), 17 (12.47, 3.80); for column VII, 6 (14.78 mm, 18.38 mm), 10 (17.09, 10.16), 14 (17.09, 6.52).
[0059] The platinum film thickness error calculation formula is:
[0060] .
[0061] Appearance inspection of platinum-plated semiconductor wafer products: Observe with a 40x optical microscope and an electron microscope at 300x magnification, and judge the results according to the following standards:
[0062] Excellent: The platinum coating is uniform, smooth, free of bubbles, pits, scratches, missing plating, seepage and other defects;
[0063] Good: The defect area is determined based on the uniformity, smoothness, bubbles, pits, scratches, plating leakage, and plating penetration of the platinum layer. The defect area is less than 3% of the overall test area.
[0064] Medium: Determine the defect area based on the uniformity, smoothness, bubbles, pits, scratches, missed plating, and seepage plating of the platinum coating. The defect area is 3% of the overall test area ≤ 5% of the overall test area.
[0065] Bad: Defect area is determined based on uniformity, smoothness, bubbles, pits, scratches, plating leakage, and seepage of the platinum coating. If the defect area is ≥ 5% of the overall test area, it is considered unqualified.
[0066] Corrosion resistance test of platinum coating on platinum-plated semiconductor wafer products: The test method of saturated sulfur dioxide according to national standard GB2423.33-2005 was used for 24 hours. After the test, the corrosion area caused by tiny pinholes and slits was detected by 3D profile measuring instrument VR-6000 manufactured by Keyence. The percentage of corrosion area to the total area of the plating area is called corrosion rate. The lower the corrosion rate, the fewer tiny pinholes and slits, and the higher the corrosion resistance of platinum-plated semiconductor wafer products. On the contrary, the higher the corrosion rate, the more tiny pinholes and slits, and the lower the corrosion resistance of platinum-plated metal.
[0067] Surface roughness test of platinum coating of platinum-plated semiconductor wafer products: The surface roughness is tested according to the national standard GB / T3505-2000. The surface roughness is tested using the 3D profile measuring instrument VR-6000 manufactured by Keyence. The results are expressed as the arithmetic mean value of the roughness Ra (unit: nm).
[0068] Platinum coating purity test of platinum-plated semiconductor wafer products: The test is carried out in accordance with the national chemical industry standard HG / T 5747-2020, and the detection is carried out by Hitachi spectrophotometer PS3500DDII / ICP-AES. The detection limit of the equipment is ≤0.1 ppb. The platinum coating purity calculation formula is as follows. The present invention studied the purity of the platinum coating deposited on the surface of semiconductor wafers and found that the higher the purity of the platinum coating, the better its surface resistance to sulfur dioxide corrosion. Conversely, the lower the purity, the worse its corrosion resistance.
[0069] .
[0070] In each embodiment and comparative example of the present invention, the total content of impurity metals in the platinum salt is required to be ≤0.1 ppm; the solvent ultrapure water adopts ultrapure water of the highest level EW-Ⅰ of the national electronic grade water standard, with a resistivity of ≥18 MΩ*cm (25°C).
[0071] Example 1
[0072] 1. A method for preparing a chemical platinum plating solution, comprising the following steps:
[0073] (1) Preparation of starter solution A: Based on the final concentration of each component in the chemical platinum plating solution, 6.7 g / L of ethylenediamine hydrochloride, 35 g / L of ammonium acetate, and 3.9 g / L of ethylenediamine platinum (II) chloride (calculated as platinum), the complexing agent ethylenediamine hydrochloride, the conductive salt ammonium acetate, and the platinum salt ethylenediamine platinum (II) chloride are completely dissolved in an appropriate amount of ultrapure water under heating (50 °C) and stirring conditions, and the pH value of the solution is adjusted to 7 with ammonia water to obtain starter solution A;
[0074] The present invention has found that when the ApH value of the cylinder opening liquid is 7, the solution is very stable and can be stored for a long time without turbidity and precipitation.
[0075] (2) Preparation of starter solution B: Based on the final concentration of each component in the chemical plating platinum solution, the buffer ammonium citrate is completely dissolved in an appropriate amount of ultrapure water at 23 g / L ammonium citrate and 1.1 g / L thiourea dioxide under heating (50 °C) and stirring conditions. After adjusting the pH value of the solution to 7, the reducing agent thiourea dioxide is completely dissolved in the buffer solution and the pH value of the solution is adjusted to 7 to obtain starter solution B.
[0076] (3) Compounding: Slowly add the pre-bottle liquid B to the pre-bottle liquid A, mix well, and test the solution pH to 7. Use ultrapure water to make up the volume. During chemical plating, adjust the solution pH to 10.0 to obtain a chemical plating platinum solution.
[0077] It is noteworthy that in Example 1, no additives (such as 2-amino-3-hydroxypropionic acid) were added.
[0078] 2. The chemical plating solution comprises: 6.7 g / L ethylenediamine hydrochloride, 35 g / L ammonium acetate, 3.9 g / L ethylenediamine platinum (II) chloride (calculated as platinum), 23 g / L ammonium citrate, 1.1 g / L thiourea dioxide, and the solvent is ultrapure water;
[0079] During chemical plating, a pH adjuster (such as ammonia water and / or sodium hydroxide solution) is used to adjust the pH value of the chemical plating platinum solution to 10.0;
[0080] When chemical plating is not required, a pH adjuster (such as at least one of ammonia water, sodium hydroxide solution or sulfuric acid solution) is used to adjust the pH value of the chemical platinum plating solution to 7.
[0081] 3. The use of the above chemical platinum plating solution in the preparation of a platinum-plated semiconductor wafer product, wherein a platinum nanostructured coating is formed on the surface of the platinum-plated semiconductor wafer product, and the use comprises the following steps:
[0082] The semiconductor wafer plated part 10 to be chemically plated is installed in the chemical plating equipment after degreasing and acid activation treatment, and the above-mentioned chemical platinum plating solution is used for chemical plating for 47 minutes at a temperature of 55°C and a pH value of 9.5-10.5 (for example, 10.0) to obtain a semiconductor wafer product with a platinum film thickness of ≥800 nm.
[0083] Example 2 to Example 11 Optimization of reducing agent concentration
[0084] A chemical plating platinum solution and a preparation method thereof are described with reference to Example 1, except that the concentration of the reducing agent thiourea dioxide is adjusted according to Table 1.
[0085] Table 1
[0086]
[0087] The application of the above chemical platinum plating solution in the preparation of platinum-plated semiconductor wafer products is described in Example 1.
[0088] Test Example 1:
[0089] The platinum-plated semiconductor wafer products obtained in Examples 1 to 11 were tested for platinum coating thickness (unit: nm), and the results are shown in Table 2.
[0090] Table 2
[0091]
[0092] The platinum-plated semiconductor wafer products obtained in Examples 1 to 11 were subjected to appearance inspection, corrosion resistance test, platinum coating surface roughness test and platinum coating purity test, and the results are shown in Table 3.
[0093] Table 3
[0094]
[0095] As shown in Table 2 and Table 3, according to the test results of applying the chemical platinum plating solutions of Examples 1 to 11 to prepare platinum-plated semiconductor wafer products, the concentration of thiourea dioxide in the present invention has a great influence on the comprehensive performance of the platinum-plated semiconductor wafer products. When the concentration of thiourea dioxide is 2.7-7.6 g / L (see Examples 3-9), it has excellent comprehensive performance: the film thickness distribution is highly uniform, the error of the maximum film thickness compared to the target setting value of 800 nm is ≤1.6%, the appearance inspections under a microscope of 40 times and an electron microscope of 300 times are both excellent, the corrosion rate of sulfur dioxide gas corrosion for 24 hours is 0.0%, the roughness of the platinum coating is 126-129 nm, and the purity of the platinum coating is as high as 99.9999%. However, when the concentration of thiourea dioxide is too low (see Examples 1-2) or too high (see Examples 10-11), the appearance inspections under a microscope of 40 times and an electron microscope of 300 times cannot reach both excellent, the corrosion rate of sulfur dioxide gas corrosion for 24 hours is 0.8-2.5%, that is, corrosion of varying degrees occurs, and the purity of the platinum coating is also lower than 99.9999%, and the comprehensive performance is poor. Therefore, the concentration of the reducing agent thiourea dioxide is 2.7-7.6 g / L, preferably 3.2-6.5 g / L; the most preferred range is 3.8-5.4 g / L.
[0096] Example 12-22 Complexing agent concentration optimization
[0097] A chemical plating platinum solution and a preparation method thereof, referring to Example 1, the only difference is that the concentration of the reducing agent thiourea dioxide is 4.3 g / L, and the concentration of the complexing agent ethylenediamine hydrochloride is adjusted according to Table 4.
[0098] Table 4
[0099]
[0100] It is worth noting that in order to unilaterally optimize the concentration of the complexing agent ethylenediamine hydrochloride, no additives (such as 2-amino-3-hydroxypropionic acid) were added in Examples 12 to 22.
[0101] The application of the above chemical platinum plating solution in the preparation of platinum-plated semiconductor wafer products is described in Example 1.
[0102] Test Example 2:
[0103] The platinum-plated semiconductor wafer products obtained in Examples 12 to 22 were tested for platinum coating thickness (unit: nm), and the results are shown in Table 5.
[0104] Table 5
[0105]
[0106] The platinum-plated semiconductor wafer products obtained in Examples 12 to 22 were subjected to appearance inspection, corrosion resistance test, platinum coating surface roughness test and platinum coating purity test, and the results are shown in Table 6.
[0107] Table 6
[0108]
[0109] As can be seen from Tables 5 and 6, according to the test results of applying the chemical platinum plating solutions of Examples 12 to 22 to prepare platinum-plated semiconductor wafer products, the concentration of ethylenediamine hydrochloride in the present invention has a great influence on the comprehensive performance of the platinum-plated semiconductor wafer products. When the concentration of ethylenediamine hydrochloride is 7.3-17.1 g / L (see Examples 14-20), it has excellent comprehensive performance: the film thickness distribution is highly uniform, the error of the maximum film thickness compared to the target setting value of 800 nm is ≤1.6%, the appearance inspections under a microscope of 40 times and an electron microscope of 300 times are both excellent, the corrosion rate of sulfur dioxide gas corrosion for 24 hours is 0.0%, the roughness of the platinum coating is 127-133 nm, and the purity of the platinum coating is as high as 99.9999%. However, when the concentration of ethylenediamine hydrochloride is too low (see Examples 12-13) or too high (see Examples 21-22), the appearance inspections under a microscope of 40 times and an electron microscope of 300 times cannot reach both excellent, the corrosion rate of sulfur dioxide gas corrosion for 24 hours is 3.7-2.1%, that is, corrosion of varying degrees occurs, and the purity of the platinum coating is also lower than 99.9999%, and the comprehensive performance is poor. Thus, the concentration of ethylenediamine hydrochloride is 7.3-17.1 g / L, preferably 9.2-15.8 g / L; the most preferred range is 11.2-14.5 g / L.
[0110] Example 23-33 Additive Concentration Optimization
[0111] A chemical plating platinum solution and a preparation method thereof, referring to Example 1, the only difference is that the concentration of the reducing agent thiourea dioxide is 4.3 g / L, the concentration of the complexing agent ethylenediamine hydrochloride is 13.2 g / L, and in addition, an additive 2-amino-3-hydroxypropionic acid is added to the chemical plating platinum solution, and the concentration (g / L) of the 2-amino-3-hydroxypropionic acid is set according to Table 7.
[0112] Among them, in the preparation method of the chemical plating platinum solution of Examples 23 to 33, the additive 2-amino-3-hydroxypropionic acid is added as follows: when preparing the cylinder starter liquid B in step (2), the buffer ammonium citrate is completely dissolved in an appropriate amount of ultrapure water, and then the additive 2-amino-3-hydroxypropionic acid is added. After all of them are dissolved and mixed evenly, the pH value of the solution is adjusted to 7, and then the reducing agent thiourea dioxide is completely dissolved in the resulting solution, and the pH value of the solution is adjusted to 7 to obtain the cylinder starter liquid B.
[0113] Table 7
[0114]
[0115] The application of the above chemical platinum plating solution in the preparation of platinum-plated semiconductor wafer products is described in Example 1.
[0116] Test Example 3:
[0117] The platinum-plated semiconductor wafer products obtained in Examples 23 to 33 were tested for platinum coating film thickness (unit: nm), and the results are shown in Table 8.
[0118] Table 8
[0119]
[0120] The platinum-plated semiconductor wafer products obtained in Examples 23 to 33 were subjected to appearance inspection, corrosion resistance test, platinum coating surface roughness test and platinum coating purity test, and the results are shown in Table 9.
[0121] Table 9
[0122]
[0123] As can be seen from Tables 8 and 9, according to the test results of the chemical platinum plating solutions of Examples 12 to 22 being applied to the preparation of platinum-plated semiconductor wafer products, when the present invention contains the additive 2-amino-3-hydroxypropionic acid, the concentration of the additive 2-amino-3-hydroxypropionic acid has a great influence on the comprehensive performance of the platinum-plated semiconductor wafer products. When the concentration of 2-amino-3-hydroxypropionic acid is between 0.15 and 1.20 g / L (see Examples 25 to 31), the film has excellent comprehensive performance: the film thickness distribution is highly uniform, the error of the maximum film thickness compared to the target setting value of 800 nm is ≤1.6%, the appearance inspections under a microscope of 40 times and an electron microscope of 300 times are both excellent, the corrosion rate of sulfur dioxide gas corrosion for 24 hours is 0.0%, the roughness of the platinum coating is 122 to 125 nm, and the purity of the platinum coating is as high as 99.9999%. However, when the concentration of the additive 2-amino-3-hydroxypropionic acid is too low (see Examples 23 to 24) or too high (see Examples 32 to 33), the appearance inspections under a microscope of 40 times and an electron microscope of 300 times cannot reach both excellent, the corrosion rate of sulfur dioxide gas corrosion for 24 hours is 0.5 to 1.7%, i.e., corrosion of varying degrees occurs, and the purity of the platinum coating is also lower than 99.9999%, and the comprehensive performance is poor. Therefore, the concentration of the additive 2-amino-3-hydroxypropionic acid is 0.15~1.2 g / L, preferably 0.3~1.05 g / L; the most preferred range is 0.45~0.85 g / L.
[0124] Comparing the formulations of Examples 25 to 31 with that of Example 17, the only difference is that different concentrations of 2-amino-3-hydroxypropionic acid are added. Performance comparison shows that the system of the present invention contains an appropriate concentration of 2-amino-3-hydroxypropionic acid. Compared with the system without additives (such as 2-amino-3-hydroxypropionic acid), the surface roughness of the platinum coating prepared under the same conditions is significantly improved, which confirms that the appropriate concentration of additives (such as 2-amino-3-hydroxypropionic acid) can significantly improve the compactness of the deposited platinum coating while ensuring the uniformity of the high film thickness distribution of the platinum coating, thereby helping to reduce coating defects and improve product quality.
[0125] In summary, in the chemical plating platinum solution provided by the present invention, the concentration of ethylenediamine platinum (II) chloride is 3.9 g / L (in terms of platinum), the concentration range of the reducing agent thiourea dioxide is 2.7~7.6 g / L, the concentration range of the complexing agent ethylenediamine hydrochloride is 7.3~17.1 g / L, and the concentration range of the additive 2-amino-3-hydroxypropionic acid is 0.15~1.20 g / L; thus, the mass ratio of ethylenediamine platinum (II) chloride (in terms of platinum): thiourea dioxide: ethylenediamine hydrochloride: 2-amino-3-hydroxypropionic acid: is 3.9: (2.7~7.6): (7.3~17.1): (0.15~1.20) = 1: (0.7~1.9): (1.9~4.4): (0.038~0.308).
[0126] When the concentration of ethylenediamineplatinum(II) chloride is changed in the chemical platinum plating solution of the present invention, the concentrations of the reducing agent thiourea dioxide, the complexing agent ethylenediamine hydrochloride and the additive 2-amino-3-hydroxypropionic acid need to be calculated according to the above-mentioned mass ratio to exert the effective performance of the chemical platinum plating solution of the present invention.
[0127] From the above analysis, it can be seen that from the perspective of being used to prepare platinum-plated semiconductor wafer products with excellent platinum coating appearance and excellent comprehensive performance, the best formula of the chemical platinum plating solution of the present invention is shown in Example 28, namely:
[0128] The chemical plating platinum solution includes: 3.9 g / L of ethylenediamine platinum chloride (II) (calculated as platinum), 13.2 g / L of ethylenediamine hydrochloride, 35 g / L of ammonium acetate, 23 g / L of ammonium citrate, 4.3 g / L of thiourea dioxide, 0.65 g / L of 2-amino-3-hydroxypropionic acid, and the solvent is ultrapure water; during chemical plating, a pH regulator (such as ammonia water and / or sodium hydroxide solution) is used to adjust the pH value of the chemical plating platinum solution to 10.0; when chemical plating is not required, a pH regulator (such as at least one of ammonia water, sodium hydroxide solution or sulfuric acid solution) is used to adjust the pH value of the chemical plating platinum solution to 7. Analysis shows that the mass ratio of ethylenediamine platinum chloride (II) (calculated as platinum): thiourea dioxide: ethylenediamine hydrochloride: 2-amino-3-hydroxypropionic acid is 3.9:4.3:13.2:0.65=1:1.1:3.4:0.167.
[0129] Based on this, in the batch plating production process of the chemical plating platinum solution of the present invention, as platinum (II) and reducing agent are consumed, the concentration of each component in the system is tested regularly by an automatic analysis device, and then the automatic replenishing device is linked to replenish each component to maintain the composition of the chemical plating platinum solution basically unchanged.
[0130] Embodiments 34 to 40
[0131] A chemical plating platinum solution and a preparation method thereof. Referring to Example 28, the concentrations of the complexing agent, conductive salt, platinum salt, buffer, reducing agent, additives, etc. remain unchanged. The only difference is that the composition of each component is changed as shown in Table 10. The unit of concentration of each component is g / L.
[0132] The application of the above chemical platinum plating solution in the preparation of platinum-plated semiconductor wafer products is described in Example 1.
[0133] Table 10
[0134]
[0135] Table 10
[0136]
[0137] Comparative Examples 1 to 7
[0138] The chemical plating solutions and preparation methods thereof provided in Comparative Examples 1 and 2 are similar to those in Example 28, and the concentrations of the complexing agent, conductive salt, platinum salt, buffer, reducing agent, additives, etc. remain unchanged, except that:
[0139] Comparative Example 1 used diammine dichloroplatinum instead of ethylenediamine platinum chloride.
[0140] Comparative Example 2 used sodium borohydride instead of thiourea dioxide.
[0141] Comparative Example 3: A chemical plating solution was prepared according to Example 1 of document CN109415812A, and the reducing agent was potassium formate; the platinum salt was potassium platinum tetrachloride.
[0142] Comparative Example 4: A chemical plating solution was prepared according to the example of using sodium borohydride and tetraammine platinum nitrate in document CN110621806A;
[0143] Comparative Example 5: A chemical plating solution was prepared according to the example of using sodium borohydride and dinitrodiammine platinum in the document JP2018-104755A;
[0144] Comparative Example 6: A chemical plating solution was prepared according to the example of sodium formate and tetraammineplatinum dichloride in JP2017-75379A;
[0145] Comparative Example 7: A chemical plating solution was prepared according to the example of using sodium borohydride and ammonium chloroplatinate in the document JP2016-160505A;
[0146] The application of the above chemical platinum plating solution in the preparation of platinum-plated semiconductor wafer products is as shown in Example 1, and the pH adjustment and plating time are adjusted as shown in Table 11.
[0147] Table 11 Chemical plating solutions of Comparative Examples 1 to 7
[0148]
[0149] Table 11
[0150]
[0151] Test Example 4:
[0152] The platinum coating film thickness (unit: nm) of the platinum-plated semiconductor wafer products obtained in Examples 34 to 40 and Comparative Examples 1 to 7 was tested, and the results are shown in Table 12.
[0153] Table 12
[0154]
[0155] The platinum-plated semiconductor wafer products obtained in Examples 34 to 40 and Comparative Examples 1 to 7 were subjected to appearance inspection, corrosion resistance test, platinum coating surface roughness test and platinum coating purity test. The results are shown in Table 13.
[0156] Table 13
[0157]
[0158] As can be seen from Tables 12 and 13, Examples 34 to 40 confirm that a cyclic platinum salt (such as ethylenediamine platinum chloride and ethylenediamine platinum iodide) is used, thiourea dioxide is used as a reducing agent, ethylenediamine hydrochloride, ethylenediamine sulfate, 1,3-propylenediamine hydrochloride, 1,4-butylenediamine dihydrochloride, 1,2-diaminocyclohexane, diethylenediamine or triethylenediamine, which can form a cyclic complex with a platinum (II) salt, is used as a complexing agent, and 2-amino-3-hydroxypropionic acid, N- Compounds containing amino and carboxyl groups, such as (2-aminoethyl)glycine, β-alanine hydroiodide, γ-aminobutyric acid, 2,3-diaminopropionic acid hydrochloride, 2,4-diaminobutyric acid or 2,5-diaminopentanoic acid, which can form a cyclic complex with platinum through amino and carboxyl groups, are used as additives. The chemical platinum plating solution at a specific dosage ratio is used to prepare platinum-plated semiconductor wafer products with excellent comprehensive performance: the film thickness distribution is high in uniformity, and the maximum film thickness is 800% lower than the target setting value. The error of nm is ≤1.6%, the appearance inspections of 40x microscope and 300x electron microscope are both excellent, the corrosion rate of sulfur dioxide gas corrosion for 24 hours is 0.0%, the roughness of the platinum coating is 121~125 nm, and it has a flat, smooth and dense surface state. The purity of the platinum coating is as high as 99.9999%. It can be seen that the prepared platinum-plated semiconductor wafer product has formed a platinum metal coating with uniform film thickness distribution, smooth surface, high purity, brightness, high density, no pinholes, no slits, excellent corrosion resistance and excellent morphology. Based on this, it can effectively prevent defects such as unstable signal transmission, high resistance, and excessive power loss of electronic products caused by defects such as pinholes or slits, better ensure that the platinum-plated semiconductor wafer products achieve high-precision conductivity and high-quality electronic signal transmission performance, improve the stability and reliability of semiconductor wafer electronic products, and better meet the needs of high-tech, high-quality, and high-precision electronic chemical plating products.
[0159] The reasons for improving the performance of chemical platinum plating by the present invention include: in the chemical platinum plating solution of the present invention, ethylenediamine platinum chloride or ethylenediamine platinum iodide is used as the platinum salt, and different diamino compounds are used to form five-membered to seven-membered platinum complexes; in addition, when α-amino acid acids are selected as the additive, a five-membered platinum complex can also be formed; when β-amino acid acids are selected as the additive, a six-membered platinum complex can also be formed; when γ-amino acid acids are selected as the additive, a seven-membered platinum complex can also be formed. These five-membered to seven-membered platinum complexes help to improve the stability of the chemical platinum plating solution, thereby achieving excellent film thickness distribution uniformity and excellent corrosion resistance.
[0160] However, based on the preferred embodiment 28, after replacing ethylenediamineplatinum chloride with diamminedichloroplatinum, Comparative Example 1 has poor quality of platinum coating due to the lack of key cyclic platinum salt: the film thickness error is 1.9%, the appearance inspection under 40x microscope and 300x electron microscope cannot reach double excellence, the corrosion rate of sulfur dioxide gas corrosion for 24 hours is 1.9%, and the purity of the platinum coating is less than 99.98%, and the overall performance is poor, making it impossible to achieve high-precision conductivity and high-quality electronic signal transmission performance for platinum-plated semiconductor wafer products.
[0161] Comparative Example 2 is based on the preferred embodiment 28, but sodium borohydride is used instead of thiourea dioxide. Due to the lack of the key thiourea dioxide, the quality of the platinum coating in Comparative Example 2 is poor: the appearance inspection under a 40x microscope and a 300x electron microscope fails to reach double excellence, the corrosion rate of sulfur dioxide gas corrosion for 24 hours is 2.3%, the roughness of the platinum coating is 143 nm, and the purity of the platinum coating is less than 99.97%. The overall performance is poor, and the high-precision conductivity and high-quality electronic signal transmission performance of the platinum-plated semiconductor wafer product cannot be achieved.
[0162] The above results confirm that the use of cyclic platinum salts such as ethylenediamineplatinum chloride and a specific reducing agent, thiourea dioxide, in the chemical platinum plating solution of the present invention is crucial to achieving the excellent performance of the present invention.
[0163] Taking Example 28 and Comparative Example 2 as examples, the microscopic morphology of the obtained platinum coating was characterized. The results are as follows: Figure 3 and Figure 4As shown. By comparison, it can be seen that the platinum coating obtained in Example 28 of the present invention has the characteristics of smooth and bright surface, high density, no pinholes, and no slits; it is consistent with the results of its excellent appearance test results, uniform film thickness distribution, low coating roughness, strong corrosion resistance, and high platinum purity, confirming the nano-scale dense morphology, uniform distribution and excellent density of the platinum coating. The platinum coating obtained in Comparative Example 2 shows that the surface shows slits, the surface flatness is destroyed, the crystalline particles on the surface can be vaguely observed, it is relatively rough, and the uniformity and density are poor; it is also consistent with the results that its appearance test results do not meet the standards, the uniformity of the film thickness distribution decreases, the coating roughness is high, the corrosion resistance is poor, and the coating metal platinum does not reach high purity.
[0164] By comparing Comparative Examples 3 to 7 representing the existing platinum chemical plating technology, it can be seen that Comparative Examples 3 to 7 are unable to solve the micro pinholes and micro cracks existing in the platinum coating, as shown in the results of the sulfur dioxide corrosion test with a corrosion rate of 2.1 to 3.5%; the roughness of the platinum coating is 151 to 192 nm, and the purity of the platinum coating can only reach a purity level of 99.9% at most, which is far lower than the high purity of 99.9999% of the present invention.
Claims
1. A chemical plating solution, characterized in that include: Cyclic platinum salt, reducing agent, complexing agent, conductive salt, buffer, pH regulator and ultrapure water; wherein: The cyclic platinum salt comprises at least one of ethylenediamine platinum chloride (II) or ethylenediamine platinum iodide (II); the concentration of the cyclic platinum salt is 1-15 g / L in terms of platinum; the mass ratio of the cyclic platinum salt: the reducing agent: the complexing agent is 1: (0.7-1.9): (1.9-4.4); The reducing agent is thiourea dioxide; The complexing agent is a diamino compound capable of forming a cyclic complex with platinum (II); The conductive salt is an ammonium carboxylate compound; The buffer is a polycarboxylate compound; The pH adjuster is configured as: During chemical plating, the pH value of the chemical plating platinum solution is adjusted to 9.5-10.5; When chemical plating is not required, the pH value of the chemical plating solution is adjusted to 7.
2. The chemical plating solution according to claim 1, characterized in that Also includes: additive; The additive is a compound containing amino and carboxyl groups that can form a cyclic complex with platinum (II) through the amino and carboxyl groups; The mass ratio of cyclic platinum salt: reducing agent: complexing agent: additive is 1: (0.7~1.9): (1.9~4.4): (0.038~0.308).
3. The chemical plating solution according to claim 1 or 2, characterized in that: The complexing agent includes at least one of ethylenediamine, ethylenediamine hydrochloride, ethylenediamine sulfate, 1,3-propylenediamine, 1,3-propylenediamine hydrochloride, 1,4-butylenediamine dihydrochloride, 1,2-diaminocyclohexane, diethylenediamine or triethylenediamine.
4. The chemical plating solution according to claim 2, characterized in that The additive is at least one of α-amino acids and their derivatives, β-amino acids and their derivatives, or γ-aminobutyric acid and its derivatives.
5. The chemical plating solution according to claim 4, characterized in that The α-amino acids and their derivatives include: At least one of glycine sodium salt hydrate, 2-amino-3-hydroxypropionic acid, N-(2-aminoethyl)glycine, N-(3-aminopropyl)glycine, 2,3-diaminopropionic acid hydrochloride, sodium N-hydroxymethylglycine, 3-(4-pyridyl)-D-alanine dihydrochloride, DL-serine, sarcosine, sodium sarcosinate, 2,4-diaminobutyric acid and 2,5-diaminopentanoic acid.
6. The chemical plating solution according to claim 4, characterized in that The β-amino acids and their derivatives include: At least one of β-alanine, DL-alanine, α-fluoro-β-alanine, β-alanine hydroiodide, β-alanine methyl ester hydrochloride, β-alanine ethyl ester hydrochloride, N-benzyloxycarbonyl-β-alanine, β-N-methylamino-L-alanine and L-β-homoalanine hydrochloride.
7. The method for preparing the chemical platinum plating solution according to any one of claims 1 to 6, characterized in that: The steps include: (1) preparing the start-up liquid A: based on the final concentration of each component in the chemical platinum plating solution, the complexing agent, the conductive salt and the cyclic platinum salt are completely dissolved in a portion of ultrapure water under heating and stirring conditions, and the pH value of the solution is adjusted to 7 using the pH adjusting agent to obtain the start-up liquid A; (2) preparing the start-up liquid B: based on the final concentration of each component in the chemical plating platinum solution, under heating and stirring conditions, completely dissolving the buffer in another portion of ultrapure water, adjusting the pH value of the solution to 7 to obtain a buffer solution, completely dissolving the reducing agent in the buffer solution, adjusting the pH value of the solution to 7, and obtaining the start-up liquid B; (3) Compounding: Slowly add the pre-bottle liquid B to the pre-bottle liquid A, mix well, and test the solution to a pH value of 7. Use the remaining ultrapure water to make up the volume. During chemical plating, adjust the solution pH value to 10 to obtain the chemical plating platinum solution.
8. The method for preparing the chemical platinum plating solution according to claim 7, characterized in that: When preparing the cylinder starter liquid B in step (2), the buffering agent is completely dissolved in another portion of ultrapure water, and then the additive is added. After all the additives are dissolved and mixed evenly, the pH value of the solution is adjusted to 7. The reducing agent is then completely dissolved in the resulting solution, and the pH value of the solution is adjusted to 7 to obtain the cylinder starter liquid B.
9. Use of the chemical platinum plating solution according to any one of claims 1 to 6 in the preparation of platinum-plated semiconductor wafer products.