Immobilized laccase and preparation method thereof
By using mesoporous UiO-66-NH2(Zr) carrier and embedding method in Cu-PABA immobilized laccase, the problem of low reaction efficiency of Cu-PABA immobilized laccase was solved, and high catalytic activity and suitable for large-scale use were achieved. Immobilized laccase for large-scale applications.
Patent Information
- Application Number
- CN202410683347.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-29
- Publication Date
- 2024-10-01
AI Technical Summary
In the existing technology, the Cu-PABA metal-organic framework-immobilized laccase has limited specific surface area and small pores, which limits its ability to adsorb substrates, resulting in low reaction efficiency and is not suitable for large-scale or industrial processes.
Mesoporous UiO-66-NH2(Zr) was used as a carrier to prepare immobilized laccase through the embedding method. The mesoporous structure was synthesized using precursor, pore expander and soft film plate agent to improve the catalytic activity and reaction of laccase. efficiency.
An immobilized laccase with high catalytic activity and high reaction efficiency is achieved, which is suitable for large-scale application. It also overcomes the problem of low reaction efficiency of Cu-PABA immobilized laccase and is suitable for large-scale or industrial processes.
Smart Images

Figure BDA0004867004780000081 
Figure BDA0004867004780000091 
Figure BDA0004867004780000121
Abstract
Description
Technical Field
[0001] The invention belongs to the field of enzyme engineering, and in particular relates to immobilized laccase and a preparation method thereof. Background Art
[0002] Free laccase is sensitive to the external environment, easily inactivated in aqueous solution and difficult to recover, making it difficult to apply laccase on a large scale. Most studies focus on immobilizing laccase, ignoring the limitation of overprotection on laccase activity, such as immobilizing laccase by encapsulation / embedding method, but the activity expression of immobilized laccase is limited.
[0003] Jiang Shan and other researchers used Cu 2+ The immobilization of laccase with a metal organic skeleton (Cu-PABA) as the center not only solves the problem of easy inactivation of free laccase, but also promotes the expression of laccase activity after immobilization (Study on the decolorization and degradation of azo dyes by Cu-PABA immobilized laccase, Master's thesis of Wuhan University of Science and Technology, Jiang Shan). However, this method of immobilizing laccase still has the following shortcomings: the specific surface area of the Cu-PABA metal organic skeleton is limited, and the pores of the Cu-PABA metal organic skeleton are small, which limits the adsorption capacity of the immobilized laccase to the substrate and hinders the contact between the substrate and the enzyme active center. Therefore, the reaction efficiency of Cu-PABA immobilized laccase is relatively low and is not suitable for large-scale or industrial processes.
[0004] Therefore, there is an urgent need to develop immobilized laccase with good activity and high response efficiency and a preparation method thereof. Summary of the invention
[0005] The present invention aims to solve one of the technical problems in the related art to at least a certain extent. To this end, the present invention provides an immobilized laccase and a preparation method thereof. The immobilized laccase of the present invention has good catalytic activity and high reaction efficiency, and is suitable for large-scale application. The preparation method of the immobilized laccase of the present invention is simple to operate, low in cost, and high in immobilization rate.
[0006] The present invention is based on the inventor's discovery and understanding of the following facts and problems:
[0007] The inventors found in the process of developing immobilized laccase that the mesoporous UiO-66-NH 2 (Zr) was used as a carrier to immobilize laccase, and the immobilized laccase had good catalytic activity and high reaction efficiency. 2 The inventors tried to prepare immobilized laccase by embedding method and unexpectedly found that the mesoporous UiO-66-NH 2 (Zr)-immobilized laccase not only has the advantage of high stability, but also overcomes the disadvantage of low reaction efficiency.
[0008] Further experiments found that the reaction efficiency of immobilized laccase prepared by the embedding method was comparable to that of immobilized laccase prepared by the adsorption method, and was suitable for large-scale or industrial process-related applications.
[0009] Therefore, in the first aspect of the present invention, the present invention provides an immobilized laccase. According to an embodiment of the present invention, the mesoporous UiO-66-NH 2 (Zr); laccase. The immobilized laccase according to the embodiment of the present invention has good catalytic activity and high reaction efficiency, and is suitable for large-scale application.
[0010] According to an embodiment of the present invention, the mesoporous UiO-66-NH 2 The raw materials of (Zr) include: precursor, pore expanding agent and soft film plate agent.
[0011] According to an embodiment of the present invention, the precursor includes: zirconium dichloride octahydrate, aminoterephthalic acid, and p-xylene; the pore expanding agent is: hexadecane; and the soft film plate agent is: F127.
[0012] In some specific embodiments of the present invention, the mesoporous UiO-66-NH 2 (Zr) is obtained by the following method:
[0013] The p-xylene and F127 are dissolved in an aqueous solution, wherein the aqueous solution comprises glacial acetic acid, ethanol and water to obtain a first solution; zirconium dichloride octahydrate and hexadecane are dissolved in the first solution to obtain a second solution; aminoterephthalic acid and the second solution are mixed to obtain a solution containing mesoporous UiO-66-NH 2 In some specific embodiments, the mass ratio of p-xylene to F127 is (1-2):1, preferably 11:10.
[0014] In some specific embodiments, the added amount of p-xylene is 5 to 10 mg / mL, preferably 7.0 to 7.5 mg / mL.
[0015] In some specific embodiments, the added amount of F127 is 4 to 9 mg / mL, preferably 6.3 to 6.9 mg / mL.
[0016] In some specific embodiments, the volume ratio of glacial acetic acid, ethanol and water is (2-5):(1-3):(16-32), preferably 2:1:30.
[0017] In some specific embodiments, based on the volume of the first dissolving solution, the amount of zirconium dichloride octahydrate added is 0.01-0.02 g / mL, preferably 0.015 g / mL; based on the volume of the first dissolving solution, the amount of hexadecane added is 1-3% by volume, preferably 2% by volume.
[0018] In some specific embodiments, based on the volume of the first dissolving solution, the amount of aminoterephthalic acid added is 2 to 10 mg / mL, preferably 5 to 7 mg / mL, and more preferably 6.3 to 6.7 mg / mL.
[0019] In some more specific embodiments of the present invention, the method further comprises: separating solid components from the reaction product. Exemplarily, the solid components can be separated from the reaction product by centrifugation.
[0020] In some more specific embodiments of the present invention, the method further comprises: washing the solid component with N,N-dimethylformamide and anhydrous ethanol in sequence, and drying to obtain the mesoporous UiO-66-NH 2 (Zr). The reagent N,N-dimethylformamide is used to remove unreacted aminoterephthalic acid and p-xylene, and the reagent anhydrous ethanol is used to remove N,N-dimethylformamide.
[0021] According to an embodiment of the present invention, the mesoporous UiO-66-NH 2 The mass ratio of (Zr) to the laccase is (4-16):1, preferably 10:1.
[0022] In the second aspect of the present invention, the present invention provides a method for preparing the above-mentioned immobilized laccase. According to an embodiment of the present invention, the method is an adsorption method or an embedding method. The method according to the embodiment of the present invention is simple to operate, low in cost, and high in immobilization rate.
[0023] Those skilled in the art will appreciate that the features and advantages described above for immobilized laccase are also applicable to this method and will not be described in detail herein.
[0024] According to an embodiment of the present invention, the embedding method includes: dissolving p-xylene and F127 in an aqueous solution, wherein the aqueous solution includes: glacial acetic acid, ethanol and water to obtain a first dissolving solution; dissolving zirconium dichloride octahydrate and hexadecane in the first dissolving solution to obtain a second dissolving solution; mixing the laccase solution with the second dissolving solution to obtain a first mixed solution; mixing aminoterephthalic acid with the first mixed solution to obtain a second mixed solution; and subjecting the second mixed solution to an immobilization reaction to obtain an immobilized laccase. The method of the present invention, through the above reaction steps, further controls the mesoporous structure of the immobilized laccase, improves the immobilization efficiency of the laccase, and obtains an immobilized laccase with high reaction efficiency, good catalytic activity and good stability.
[0025] According to an embodiment of the present invention, the mass ratio of p-xylene to F127 is: (1-2):1, preferably 11:10.
[0026] According to an embodiment of the present invention, the added amount of p-xylene is 5 to 10 mg / mL, preferably 7.0 to 7.5 mg / mL.
[0027] According to an embodiment of the present invention, the added amount of F127 is 4 to 9 mg / mL, preferably 6.3 to 6.9 mg / mL.
[0028] According to an embodiment of the present invention, the volume ratio of glacial acetic acid, ethanol and water is (2-5):(1-3):(16-32), preferably 2:1:30.
[0029] According to an embodiment of the present invention, based on the volume of the first dissolving solution, the addition amount of the zirconium dichloride octahydrate is 0.01-0.02 g / mL, preferably 0.015 g / mL; based on the volume of the first dissolving solution, the addition amount of the hexadecane is 1-3% by volume, preferably 2% by volume.
[0030] According to an embodiment of the present invention, based on the volume of the second dissolving solution, the added amount of the laccase is 5 to 15 g / mL, preferably 9 to 11 g / mL.
[0031] According to an embodiment of the present invention, based on the volume of the first mixed solution, the amount of aminoterephthalic acid added is 2 to 10 mg / mL, preferably 5 to 7 mg / mL, and more preferably 6.3 to 6.7 mg / mL.
[0032] According to an embodiment of the present invention, the temperature of the immobilization reaction is 10-45°C, preferably 45°C.
[0033] In some specific embodiments, the embedding method further comprises: separating a solid component from the reactants of the immobilization reaction, washing the solid component with N,N-dimethylformamide and anhydrous ethanol in sequence, and obtaining the mesoporous UiO-66-NH 2 (Zr) immobilized laccase.
[0034] Additional aspects and advantages of the present invention will be given in part in the following description and in part will be obvious from the following description, or will be learned through practice of the present invention. DETAILED DESCRIPTION
[0035] The embodiments of the present invention are described in detail below. The embodiments described below are exemplary and are only used to explain the present invention, and should not be understood as limiting the present invention.
[0036] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0037] In this document, the terms “include” or “comprising” are open expressions, that is, including the contents specified in the present invention but not excluding other contents.
[0038] As used herein, the terms "optionally", "optional" or "optionally" generally mean that the subsequently described event or circumstance may but need not occur, and that the description includes instances where the event or circumstance occurs and instances where it does not.
[0039] Terms and Definitions
[0040] In this article, the term "laccase" is a polyphenol oxidase that has shown broad application prospects in the fields of paper industry, wastewater treatment, food industry, organic synthesis, bioenergy, bioenergy, textile industry, biosensors, pharmaceutical field, edible fungus production, wine clarification, etc. According to the source, laccase can be divided into three major categories, namely plant laccase, animal laccase and microbial laccase.
[0041] In this article, the term "immobilized enzyme technology" refers to a technology that fixes the enzyme on a certain carrier so that it can catalyze reactions in a certain space and can be reused.
[0042] In this article, the term "immobilized laccase" refers to the process of immobilizing laccase on a carrier (such as mesoporous UiO-66-NH 2(Zr)) after which the enzyme derivative product was obtained.
[0043] The present invention provides immobilized laccase and a preparation method thereof, which will be described in detail below.
[0044] Immobilized laccase
[0045] The present invention provides an immobilized laccase. According to an embodiment of the present invention, the immobilized laccase comprises: mesoporous UiO-66-NH 2 (Zr); laccase. The immobilized laccase according to the embodiment of the present invention has good catalytic activity and high reaction efficiency, and is suitable for large-scale application.
[0046] In this text, the term "mesoporous material" refers to materials with pore sizes ranging from 2 to 50 nm. 2 (Zr)" and common metal organic frameworks (MOFs) UiO-66-NH 2 Compared with (Zr), it has a well-developed and ordered pore structure and a high specific surface area.
[0047] According to an embodiment of the present invention, the mesoporous UiO-66-NH 2 The raw materials of (Zr) include: precursor, pore expanding agent and soft film plate agent.
[0048] In this article, the term "precursor" refers to a starting substance that can be converted into a target compound or material through further chemical changes during a chemical reaction or synthesis process. Precursors can be molecules, ions, compounds or mixtures that play a key role in the synthesis process.
[0049] In this article, the term "pore expander" is a chemical additive used to adjust the pore size of porous materials. By introducing a pore expander during the synthesis process, the pore size can be effectively controlled and increased. The pore expander changes the size, aggregation and stacking morphology of the micelles at the initial stage of synthesis, thereby changing the position of the zirconium source hydrolysis self-assembly and the space corresponding to the micelle occupancy, and finally forming a mesoporous structure with different pore size distributions.
[0050] In this article, the term "soft film" refers to a template whose specific structure is maintained by weak interactions between or within molecules, such as micelles, vesicles, liquid crystals, etc. They form an ordered structure in solution, guide the growth of precursors, and ultimately generate nanostructured materials with a certain shape. Soft film agents are used to synthesize mesoporous materials, such as mesoporous silica, mesoporous carbon, etc. They achieve synergistic co-assembly of organic-inorganic components through interactions with precursors, such as electrostatic interactions, hydrogen bonds, van der Waals forces, or coordination effects.
[0051] According to an embodiment of the present invention, the precursor includes: zirconium dichloride octahydrate; aminoterephthalic acid; p-xylene; the pore-enlarging agent is hexadecane; and the soft film agent is F127. 2 (Zr) metal organic frameworks (MOFs). Among them, the pore expander can also be used as part of the precursor to optimize the mesoporous UiO-66-NH 2 (Zr) Pore structure of the material.
[0052] In this paper, the term "F127" refers to Pluronic F127, which is composed of polyoxyethylene (PEO) and polyoxypropylene (PPO), a non-ionic triblock copolymer, which is usually used as a soft template for the synthesis of ordered mesoporous materials.
[0053] In some specific embodiments of the present invention, the mesoporous UiO-66-NH 2 (Zr) is obtained by the following method:
[0054] The p-xylene and F127 are dissolved in an aqueous solution, wherein the aqueous solution comprises glacial acetic acid, ethanol and water to obtain a first solution; zirconium dichloride octahydrate and hexadecane are dissolved in the first solution to obtain a second solution; aminoterephthalic acid and the second solution are mixed to obtain a solution containing mesoporous UiO-66-NH 2 (Zr) reaction product.
[0055] In some more specific embodiments of the present invention, the method further comprises: separating solid components from the reaction product. Exemplarily, the solid components can be separated from the reaction product by centrifugation.
[0056] In some more specific embodiments of the present invention, the method further comprises: washing the solid component with N,N-dimethylformamide and anhydrous ethanol in sequence, and drying to obtain the mesoporous UiO-66-NH 2 (Zr). The reagent N,N-dimethylformamide is used to remove unreacted aminoterephthalic acid and p-xylene, and the reagent anhydrous ethanol is used to remove N,N-dimethylformamide. In some specific embodiments, the mass ratio of p-xylene to F127 is: (1-2):1, preferably 11:10.
[0057] In some specific embodiments, the added amount of p-xylene is 5 to 10 mg / mL, preferably 7.0 to 7.5 mg / mL.
[0058] In some specific embodiments, the added amount of F127 is 4 to 9 mg / mL, preferably 6.3 to 6.9 mg / mL.
[0059] In some specific embodiments, the volume ratio of glacial acetic acid, ethanol and water is (2-5):(1-3):(16-32), preferably 2:1:30.
[0060] In some specific embodiments, based on the volume of the first dissolving solution, the amount of zirconium dichloride octahydrate added is 0.01-0.02 g / mL, preferably 0.015 g / mL; based on the volume of the first dissolving solution, the amount of hexadecane added is 1-3% by volume, preferably 2% by volume.
[0061] In some specific embodiments, based on the volume of the first dissolving solution, the amount of aminoterephthalic acid added is 2 to 10 mg / mL, preferably 5 to 7 mg / mL, and more preferably 6.3 to 6.7 mg / mL.
[0062] According to an embodiment of the present invention, the mesoporous UiO-66-NH 2 The mass ratio of (Zr) to the laccase is (4-16):1, preferably 10:1. The immobilized laccase obtained within the above mass ratio range has good activity and high reaction efficiency.
[0063] method
[0064] The present invention provides a method for preparing the above-mentioned immobilized laccase. According to an embodiment of the present invention, the method is an adsorption method or an embedding method. The method according to the embodiment of the present invention is simple to operate, low in cost, and high in immobilization rate.
[0065] Those skilled in the art will appreciate that the features and advantages described above for immobilized laccase are also applicable to this method and will not be described in detail herein.
[0066] According to an embodiment of the present invention, the embedding method comprises:
[0067] Dissolve p-xylene and F127 in an aqueous solution, the aqueous solution comprising glacial acetic acid, ethanol and water, to obtain a first solution. This step is used to obtain an aqueous solution with uniform distribution of F127 as the mesoporous UiO-66-NH 2 (Zr) synthesized soft film plate agent can achieve self-assembly after the precursor is converted into the target compound.
[0068] Dissolve zirconium oxychloride octahydrate and hexadecane in the first solution to obtain a second solution. The zirconium oxychloride octahydrate precursor is used as a zirconium source to provide metal zirconium for metal organic frameworks (MOFs). Hexadecane is used as a pore expander to control the mesoporous UiO-66-NH 2 (Zr) pore formation and pore size.
[0069] The laccase solution and the second dissolving solution are mixed to obtain a first mixed solution. This step is used to evenly disperse the laccase in the reaction system, which is beneficial to improve the fixation rate of the laccase and realize the fixation and embedding of the laccase in the mesoporous UiO-66-NH 2 (Zr) in.
[0070] The aminoterephthalic acid is mixed with the first mixed solution to obtain a second mixed solution; the second mixed solution is subjected to an immobilization reaction to obtain an immobilized laccase. This step finally synthesizes the mesoporous UiO-66-NH 2 (Zr) material, and finally embedding laccase in the mesoporous material.
[0071] According to an embodiment of the present invention, the mass ratio of p-xylene to F127 is: (1-2):1, preferably 11:10.
[0072] According to an embodiment of the present invention, the added amount of p-xylene is 5 to 10 mg / mL, preferably 7.0 to 7.5 mg / mL.
[0073] According to an embodiment of the present invention, the added amount of F127 is 4 to 9 mg / mL, preferably 6.3 to 6.9 mg / mL.
[0074] By controlling the solvent and concentration of the soft template, ordered mesoporous UiO-66-NH 2 (Zr) material.
[0075] According to an embodiment of the present invention, the volume ratio of acetic acid, ethanol and water is (2-5): (1-3): (16-32), preferably 2: 1: 30. Acetic acid provides an acidic environment for the reaction system, which is conducive to the uniform dispersion of zirconium dichloride octahydrate in the first dissolving solution.
[0076] It should be noted that, unless otherwise specified, the ethanol in this article is anhydrous ethanol.
[0077] In some preferred embodiments, the water is deionized water.
[0078] According to an embodiment of the present invention, based on the volume of the first dissolving solution, the addition amount of the zirconium dichloride octahydrate is 0.01-0.02 g / mL, preferably 0.015 g / mL; based on the volume of the first dissolving solution, the addition amount of the hexadecane is 1-3% by volume, preferably 2% by volume.
[0079] By selecting the zirconium source and controlling the type and concentration of the pore-enlarging agent, mesoporous UiO-66-NH with a fixed pore size can be further obtained. 2 (Zr) material.
[0080] According to an embodiment of the present invention, based on the volume of the second dissolving solution, the added amount of the laccase is 5 to 15 g / mL, preferably 9 to 11 g / mL.
[0081] According to an embodiment of the present invention, based on the volume of the first mixed solution, the amount of aminoterephthalic acid added is 2 to 10 mg / mL, preferably 5 to 7 mg / mL, and more preferably 6.3 to 6.7 mg / mL.
[0082] According to an embodiment of the present invention, the temperature of the immobilization reaction is 10-45°C, preferably 45°C. This facilitates the immobilization of laccase on the mesoporous UiO-66-NH 2 (Zr), and it is beneficial to display the enzyme active center on the surface of the material, further improving its catalytic activity.
[0083] According to an embodiment of the present invention, the embedding method further comprises: separating a solid component from the reactant of the immobilization reaction, washing the solid component with N,N-dimethylformamide and anhydrous ethanol in sequence, and obtaining the mesoporous UiO-66-NH 2 Thus, unreacted aminoterephthalic acid, p-xylene and other reagents were further removed, and N,N-dimethylformamide was further removed by ethanol to obtain pure mesoporous UiO-66-NH 2 (Zr) immobilized laccase to further improve its stability.
[0084] In the examples and comparative examples of the present invention, the catalytic activity of laccase was determined by the following method:
[0085] Laccase activity refers to the amount of enzyme required to oxidize 1 μmol of ABTS per minute at room temperature. Specifically, a certain mass of free laccase / immobilized laccase is weighed, 6 mL of the corresponding pH buffer solution and 3 mL of 1.0 mmol / L ABTS solution are added successively, mixed and reacted for 10 minutes, and the absorbance of the solution is measured at 420 nm. With ABTS as a substrate, laccase catalyzes the oxidation of ABTS to ABTS+, and the absorption coefficient of ABTS+ at 420 nm is much higher than that of ABTS. The activity of free laccase / immobilized laccase is measured by UV-visible spectrophotometry.
[0086] The enzyme activity calculation formula is as follows:
[0087]
[0088] Wherein, ΔA is the absorbance value of the solution after the reaction at 420 nm;
[0089] Δt is the reaction time, in min;
[0090] V is the total volume of the reaction solution, in mL;
[0091] M is the mass of added enzyme, in g;
[0092] E is the molar extinction coefficient of ABTS, 36000 L mol -1 cm -1 .
[0093] In the examples and comparative examples of the present invention, the reaction efficiency of immobilized laccase was determined by the following method: a certain mass of laccase@mesoporous UiO-66-NH 2 (Zr), 6 mL of the corresponding pH buffer solution and 3 mL of 1.0 mmol / L ABTS solution were added successively, mixed and reacted for 10 minutes, and the absorbance of the solution was measured at 420 nm. With ABTS as the substrate, laccase catalyzes the oxidation of ABTS to ABTS+, and the absorption coefficient of ABTS+ at 420 nm is much higher than that of ABTS.
[0094] In the examples and comparative examples of the present invention, the immobilization rate of the immobilized laccase method was determined by the following method: 2 mL of the supernatant after centrifugation of the immobilized laccase was taken into a 10 mL sample tube, 4 mL of Coomassie Brilliant Blue solution was added, and after staining for 5 minutes, the absorbance was measured at 595 nm using a UV-visible spectrophotometer. The measured absorbance value was substituted into the standard curve to calculate the concentration of laccase in the supernatant.
[0095] Mesoporous-UiO-66-NH 2 The immobilization rate (M) of (Zr)-immobilized laccase was calculated by the following formula:
[0096]
[0097] in,
[0098] M0 is the total mass of added laccase, mg;
[0099] C1 is the concentration of laccase in the supernatant, mg / mL;
[0100] V1 is the volume of the supernatant, mL;
[0101] M1 is the mesoporous UiO-66-NH after M0 drying 2 (Zr) Total mass of immobilized laccase, mg.
[0102] In the examples and comparative examples of the present invention, the thermal stability of immobilized laccase was determined by the following method: 8 portions of 30 mg of immobilized laccase and 10 mg of free laccase were weighed, and kept at 20-90°C for 2 hours, and all samples were measured in triplicate to determine the activity of laccase at different temperatures. The free laccase and immobilized laccase with the highest enzyme activity in the thermal stability test were taken as 100%, and their relative enzyme activities were calculated.
[0103] In the examples and comparative examples of the present invention, the acid-base stability of the immobilized laccase was determined by the following method: 7 portions of 30 mg of immobilized laccase and 10 mg of free laccase were weighed, and stored for 2 hours in an environment with a pH of 3 to 9, respectively. All samples were prepared in triplicate, and the activity of the laccase under different pH environments was determined. The free laccase and the immobilized laccase with the highest enzyme activity in the acid-base stability test were taken as 100%, and their relative enzyme activities were calculated.
[0104] The scheme of the present invention will be explained below in conjunction with the embodiments. It will be appreciated by those skilled in the art that the following embodiments are only used to illustrate the present invention and should not be considered as limiting the scope of the present invention. Where specific techniques or conditions are not indicated in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. The reagents or instruments used are not indicated by the manufacturer and are all conventional products that can be obtained commercially.
[0105] Example 1: Synthesis of mesoporous UiO-66-NH by embedding method 2 (Zr) Immobilized Laccase
[0106] In this example, mesoporous UiO-66-NH 2 (Zr) Immobilized Laccase:
[0107] 0.055 g of p-xylene (ODMB) and 0.050 g of F127 were dissolved in a mixed solution of 1 ml of glacial acetic acid, 0.5 ml of anhydrous ethanol and 6 ml of deionized water. Ultrasonication was used to form a clear and transparent solution. 0.11 g of zirconium dichloride octahydrate (ZrOCl 2 8H 2 O) and 0.15 ml hexadecane, stir for 10 minutes, then add 80 mg laccase, and after the solution is uniform, put it into an oil bath at 45 ° C, and then add 0.050 g aminoterephthalic acid (NH 2 -BDC) for 10 h.
[0108] The flake-like mesoporous UiO-66-NH 2 (Zr) immobilized laccase, and then washed once with N,N-dimethylformamide (DMF) and anhydrous ethanol to obtain the final product. The supernatant of the centrifugation step was collected and used to determine the immobilized laccase rate.
[0109] The obtained mesoporous-UiO-66-NH was characterized by SEM. 2 (Zr) immobilized laccase.
[0110] The results showed that: (1) the immobilized laccase had a mesoporous structure and presented a lamellar core-shell structure, and the laccase was immobilized by the embedding method. (2) the immobilization rate of the laccase in this example was 53%.
[0111] Example 2: Synthesis of mesoporous UiO-66-NH by adsorption 2 (Zr) Immobilized Laccase
[0112] In this example, mesoporous UiO-66-NH 2 (Zr) Immobilized Laccase:
[0113] 0.055 g ODMB and 0.050 g F127 were dissolved in a mixed solution of 1 ml glacial acetic acid, 0.5 ml anhydrous ethanol and 6 ml deionized water. The solution was ultrasonicated to form a clear transparent solution. 0.11 g zirconium dichloride octahydrate (ZrOCl 2 8H 2 O) and 0.15 ml hexadecane, and after the solution is uniform, put it into an oil bath at 45 °C and add 0.050 g aminoterephthalic acid (NH 2 -BDC) was reacted for 10 h, and mesoporous UiO-66-NH 2 The crude product (Zr) was washed once with N,N-dimethylformamide (DMF) and once with anhydrous ethanol to obtain mesoporous UiO-66-NH 2 (Zr) Final product.
[0114] 80 mg of laccase was prepared into PBS enzyme solution and mixed with mesoporous UiO-66-NH 2 The final product (Zr) was combined by electrostatic interaction and centrifuged to obtain the flake core-shell mesoporous UiO-66-NH 2 (Zr) immobilized laccase. The supernatant of the centrifugation step was collected and used to determine the immobilized laccase rate.
[0115] The obtained mesoporous-UiO-66-NH was characterized by SEM. 2 (Zr) immobilized laccase.
[0116] The results showed that: (1) the immobilized laccase had a mesoporous structure and a core-shell structure, and the laccase was immobilized by adsorption. (2) The immobilization rate of the laccase in this example was 33%.
[0117] Example 3: Synthesis of mesoporous UiO-66-NH by embedding method 2 Optimization of experimental conditions for (Zr) immobilized laccase
[0118] This example refers to Example 1 and further investigates the effects of different laccase addition amounts on immobilized laccase.
[0119] The difference from Example 1 is that this example sets 7 different laccase addition amounts: 25 mg, 50 mg, 60 mg, 70 mg, 80 mg, 90 mg, and 100 mg.
[0120] The results of enzyme activity test showed that the enzyme activity of the immobilized laccase prepared with 80 mg of laccase added was 100%, and the relative enzyme activities of the immobilized laccase prepared with different laccase addition amounts were detected and calculated as: 34%, 42%, 45%, 70%, 100%, 83%, and 79%.
[0121] The above test results show that: (1) The optimal enzyme addition amount is 70-100 mg. (2) The laccase fixation rate of this example is 53%.
[0122] Example 4: Synthesis of mesoporous UiO-66-NH by embedding method 2 Optimization of experimental conditions for (Zr) immobilized laccase
[0123] This example refers to Example 1 and further investigates the effect of different addition amounts of the pore-enlarging agent hexadecane on the immobilized laccase.
[0124] The difference from Example 1 is that this example sets four different hexadecane addition amounts: 0.075 mL, 0.1 mL, 0.15 mL, and 0.225 mL.
[0125] The results of enzyme activity detection showed that the enzyme activity of the immobilized laccase prepared with 0.15 mL of hexadecane added was 100%, and the relative enzyme activities of the immobilized laccase prepared with different amounts of hexadecane added were detected and calculated as: 71%, 83%, 100%, and 85%.
[0126] The above test results show that: (1) the optimal amount of hexadecane added is 0.15 mL. (2) the laccase fixation rate of this example is 53%.
[0127] Example 5: Synthesis of mesoporous UiO-66-NH by embedding method 2 Optimization of experimental conditions for (Zr) immobilized laccase
[0128] This example refers to Example 1 and further investigates the effect of different addition amounts of the soft film plate agent F127 on immobilized laccase.
[0129] The difference from Example 1 is that this example sets 6 different F127 addition amounts: 0.03g, 0.0375g, 0.045g, 0.05g, 0.052g, and 0.0675g.
[0130] The results of enzyme activity test showed that the enzyme activity of the immobilized laccase prepared with 0.05g F127 addition was 100%, and the relative enzyme activities of the immobilized laccase prepared with different F127 addition amounts were detected and calculated as: 64%, 72%, 75%, 100%, 83%, and 79%.
[0131] The above test results show that: (1) The optimal amount of F127 added is 0.05g and 0.052g. (2) The laccase fixation rate of this example is 53%.
[0132] Comparative Example 1: Synthesis of Cu-PABA immobilized laccase by embedding method
[0133] Referring to the study on decolorization and degradation of azo dyes by Cu-PABA immobilized laccase, Cu-PABA immobilized laccase was synthesized according to the following optimal experimental conditions: molar ratio (Cu 2+ ∶PABA) was 1.25:1, the amount of PVP was 0.3 g, the methanol concentration in the solvent was 20%; the amount of laccase added was 1.75 mg / mL, the immobilization time was 2.917 hours, and the pH was 5.16.
[0134] Study on the enzymatic properties of the immobilized laccase of Example 1, Example 2 and Comparative Example 1
[0135] Table 1: Results of investigation on enzymatic properties of immobilized laccase in Example 1, Example 2 and Comparative Example 1
[0136]
[0137] The above results show that: (1) the mesoporous UiO-66-NH 2 (Zr) fixed laccase, good catalytic activity and high reaction efficiency. Compared with comparative example 1, the mesoporous UiO-66-NH 2 (Zr) fixed laccase, its catalytic activity increased by 23%, and the reaction efficiency increased by 15%. (2) Mesoporous UiO-66-NH 2 The (Zr)-immobilized laccase has good thermal stability and acid-base stability, which is comparable to the performance of the known Cu-PABA-immobilized laccase.
[0138] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. An immobilized laccase, characterized in that: include: Mesoporous UiO-66-NH2(Zr); Laccase.
2. The immobilized laccase according to claim 1, characterized in that The raw materials for synthesizing the mesoporous UiO-66-NH2(Zr) include: a precursor, a pore-enlarging agent, and a soft film plate agent; The precursor includes: zirconium dichloride octahydrate, aminoterephthalic acid, and p-xylene; the pore-enlarging agent is: hexadecane; the soft film plate agent is: F127; Optionally, the mesoporous UiO-66-NH2(Zr) is obtained by the following method: Dissolve p-xylene and F127 in an aqueous solution, wherein the aqueous solution comprises glacial acetic acid, ethanol and water to obtain a first solution; dissolve zirconium dichloride octahydrate and hexadecane in the first solution to obtain a second solution; mix aminoterephthalic acid with the second solution to obtain a reaction product comprising the mesoporous UiO-66-NH2(Zr); Optionally, the mass ratio of p-xylene to F127 is: (1-2):1, preferably 11:10; Optionally, the amount of p-xylene added is 5 to 10 mg / mL, preferably 7.0 to 7.5 mg / mL; Optionally, the amount of F127 added is 4 to 9 mg / mL, preferably 6.3 to 6.9 mg / mL; Optionally, the volume ratio of glacial acetic acid, ethanol and water is (2-5):(1-3):(16-32), preferably 2:1:30; Optionally, based on the volume of the first dissolving solution, the amount of zirconium dichloride octahydrate added is 0.01 to 0.02 g / mL, preferably 0.015 g / mL; based on the volume of the first dissolving solution, the amount of hexadecane added is 1 to 3% by volume, preferably 2% by volume; Optionally, based on the volume of the first dissolving solution, the amount of aminoterephthalic acid added is 2 to 10 mg / mL, preferably 5 to 7 mg / mL, and more preferably 6.3 to 6.7 mg / mL; Further, the method further comprises: separating solid components from the reaction product; Furthermore, the method further comprises: washing the solid component with N,N-dimethylformamide and anhydrous ethanol in sequence, and obtaining the mesoporous UiO-66-NH2(Zr) after drying.
3. The immobilized laccase according to claim 1, characterized in that The mass ratio of the mesoporous UiO-66-NH2(Zr) to the laccase is (4-16):1, preferably 10:
1.
4. The method for preparing immobilized laccase according to any one of claims 1 to 3, characterized in that: The method is an adsorption method or an embedding method.
5. The method according to claim 4, characterized in that The embedding method comprises: Dissolving p-xylene and F127 in an aqueous solution, wherein the aqueous solution comprises: glacial acetic acid, ethanol and water, to obtain a first solution; dissolving zirconium dichloride octahydrate and hexadecane in the first dissolving solution to obtain a second dissolving solution; Mixing the laccase solution with the second dissolving solution to obtain a first mixed solution; Mixing aminoterephthalic acid with the first mixed solution to obtain a second mixed solution; The second mixed solution is subjected to an immobilization reaction to obtain immobilized laccase.
6. The method according to claim 5, characterized in that The mass ratio of p-xylene to F127 is (1-2):1, preferably 11:
10.
7. The method according to claim 5, characterized in that Based on the volume of the aqueous solution, the added amount of the p-xylene is 5 to 10 mg / mL, preferably 7.0 to 7.5 mg / mL.
8. The method according to claim 5, characterized in that Based on the volume of the aqueous solution, the added amount of F127 is 4 to 9 mg / mL, preferably 6.3 to 6.9 mg / mL.
9. The method according to claim 5, characterized in that The volume ratio of the glacial acetic acid, ethanol and water is (2-5):(1-3):(16-32), preferably 2:1:
30.
10. The method according to claim 5, characterized in that Based on the volume of the first dissolving solution, the addition amount of the zirconium dichloride octahydrate is 0.01-0.02 g / mL, preferably 0.015 g / mL; based on the volume of the first dissolving solution, the addition amount of the hexadecane is 1-3% by volume, preferably 2% by volume.
11. The method according to claim 5, characterized in that Based on the volume of the second dissolved liquid, the added amount of the laccase is 5 to 15 g / mL, preferably 9 to 11 g / mL.
12. The method according to claim 5, characterized in that Based on the volume of the first mixed solution, the amount of aminoterephthalic acid added is 2 to 10 mg / mL, preferably 5 to 7 mg / mL, and more preferably 6.3 to 6.7 mg / mL.
13. The method according to claim 5, characterized in that The temperature of the immobilization reaction is 10-45°C, preferably 45°C.
14. The method according to claim 5, characterized in that The embedding method further comprises: separating solid components from the reactants of the immobilization reaction, washing the solid components with N,N-dimethylformamide and anhydrous ethanol in sequence, and obtaining the mesoporous-UiO-66-NH2(Zr) immobilized laccase.