Solid nuclear magnetic resonance magic angle rotating rotor battery

By designing a solid-state nuclear magnetic resonance magic angle rotating rotor battery, using a 4mm sealed sample cell and driving cap combined with fusible glue and high-purity metal wire, the problem of high-speed rotation of solid-state batteries in nuclear magnetic resonance spectrometers was solved, and high-resolution original Bit detection and battery reaction mechanism research.

CN118731079APending Publication Date: 2024-10-01DALIAN INSTITUTE OF CHEMICAL PHYSICS CHINESE ACADEMY OF SCIENCES
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310313852.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing technology cannot realize the high-speed rotation of solid-state batteries in nuclear magnetic resonance spectrometers, resulting in the inability to effectively monitor the dynamic reactions during battery charging and discharging. The signal broadening masks the signals of key species.

Method used

A solid NMR magic angle rotating rotor battery is designed, which uses a 4mm sealed solid NMR sample cell and drive cap, combined with fusible glue and high-purity metal wire, to achieve high-speed rotation and sealing of the battery through conductive wires and fixed inserts. It is suitable for Rotates at 4kHz-6kHz in a strong magnetic field of 400M-800M.

Benefits of technology

It achieves high-resolution in-situ detection in a nuclear magnetic resonance spectrometer, enables stable charge and discharge tests, obtains high-quality nuclear magnetic resonance spectra, and studies battery dynamic changes and reaction mechanisms.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118731079A_ABST
    Figure CN118731079A_ABST
Patent Text Reader

Abstract

The invention discloses a solid nuclear magnetic resonance magic angle rotating rotor battery which comprises a solid nuclear magnetic resonance sample cell with a hole in the center of the bottom, a first fixing plug-in with a hole in the axial center, a first sealant, a first metal electrode, a solid electrolyte, a second metal electrode, a second sealant and a second fixing plug-in with a hole are sequentially arranged in the shell; comprising a first conductor wire and a second conductor wire, and the first conductor wire penetrates through a bottom hole of the solid nuclear magnetic resonance sample cell, the fixed plug-in and the sealant to be in contact with the first metal electrode; and the second conductor wire penetrates through the driving cap with a hole in the center, the fixed plug-in and the sealant to be in contact with the second metal electrode. The manufacturing part of the lithium symmetrical battery is realized by melting lithium in the glove, the battery is stable in structure, high in repetition rate and good in sealing performance, the combination of magic angle rapid rotation and in-situ charging and discharging test in a nuclear magnetic resonance spectrometer can be realized, a high-resolution and high-quality nuclear magnetic resonance spectrogram can be obtained, and the dynamic change and reaction mechanism of the battery can be conveniently researched.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the fields of batteries and nuclear magnetic resonance, and in particular to a solid-state battery assembly using a solid nuclear magnetic resonance magic angle spinning rotor as a shell and an in-situ solid-state nuclear magnetic resonance test. Background Art

[0002] Metal anodes have high theoretical capacity and low electrode potential, and are one of the most promising anodes for high-energy-density secondary batteries. However, since metal anodes are very active, they will continue to react with liquid organic electrolytes during the cycle, resulting in a decrease in battery capacity. In addition, the metal ion deposition process is poorly controllable, and the resulting dendritic metal can pierce the diaphragm and cause safety accidents, which limits their practical application. In recent years, with the increasing demand for high-energy-density batteries, metal anodes have once again become a hot research topic. In order to better understand the mechanism of metal anodes throughout the charging and discharging process, clarify the generation of dendrites and battery failure, and further improve battery performance, it is of great significance to use in-situ methods to track and monitor the battery reaction process.

[0003] Nuclear magnetic resonance (NMR) is an important means of non-destructive characterization of solids, liquids, gases and other substances, and can provide both qualitative and quantitative information. As a non-destructive detection method, NMR has unique advantages in in-situ research on battery reaction processes. It is currently a very effective and convenient characterization method in the study of local structure and ion diffusion dynamics around solid materials, especially amorphous materials and light elements. For example, 7 Li / 6 Li NMR plays a vital role in studying the electrode materials and reaction mechanisms of lithium batteries. When collecting solid NMR samples, the samples need to be rotated at a high speed (called magic angle rotation, MAS) (>kHz) in the magic angle direction to obtain high-resolution NMR spectra.

[0004] At present, the most commonly used battery structure in the in-situ NMR research on the battery charging and discharging process is mainly the plastic package configuration, but the plastic package configuration can only realize the charging and discharging of the battery, and cannot meet the requirements of high-speed rotation in the nuclear magnetic spectrometer, so only static in-situ nuclear magnetic spectra can be obtained. The signal broadening in the static nuclear magnetic resonance spectrum may cover the signals of key species generated during the charging and discharging process, so it is necessary to design an in-situ solid nuclear magnetic resonance sample pool that can rotate at high speed in a strong magnetic field. Ordinary solid nuclear magnetic resonance rotors cannot perform battery charging and discharging tests, and it is difficult to use MAS NMR technology to monitor the dynamic reaction process of the battery. The present invention combines the characteristics of the battery configurations of the two, and designs a device that can be charged and discharged while meeting the requirements of high-speed rotation in the strong magnetic field of the nuclear magnetic resonance spectrometer to perform in-situ detection of solid-state batteries in nuclear magnetic resonance spectrometers.

[0005] The present invention mainly includes a solid nuclear magnetic resonance rotor (4mm), a fusible adhesive (4mm), a machinable ceramic, a high-purity metal wire (>99.9%, with a diameter of 0.25mm), a drive cap and a metal electrode. The metal wire and the drive cap in the battery can be fixed and sealed using the processed fusible adhesive. This symmetrical battery structure has many advantages such as simple assembly, good sealing, and easy use. It can quickly and effectively realize the in-situ detection of symmetrical solid-state batteries in nuclear magnetic resonance spectrometers. After a large number of repeated assembly and testing, the assembled battery in the experiment can stably operate for more than two cycles under a suitable charge and discharge current. Summary of the invention

[0006] In order to solve the problem that high-speed rotation is required for in-situ detection of solid-state battery samples on a solid-state nuclear magnetic resonance spectrometer, a solid-state nuclear magnetic resonance magic angle spinning rotor battery was invented. The present invention is suitable for a solid-state nuclear magnetic resonance spectrometer.

[0007] The technical solution adopted by the present invention is as follows:

[0008] The invention comprises a rotor, wherein the rotor comprises a driving cap with a hole in the center and a solid nuclear magnetic resonance sample cell with a sample cavity which match each other; the solid nuclear magnetic resonance sample cell has a hole in the center at the bottom;

[0009] The sample cavity of the solid nuclear magnetic resonance sample cell is provided with a first fixing plug-in with an axial center hole, a first sealant, a first metal electrode, a solid electrolyte, a second metal electrode, a second sealant, and a second fixing plug-in with a hole in sequence;

[0010] It also includes a first conductive wire and a second conductive wire. The first conductive wire passes through the bottom hole of the solid nuclear magnetic resonance sample pool, a first fixed plug-in with a hole, a first sealant and contacts the first metal electrode; the second conductive wire passes through a driving cap with a hole in the center, a second fixed plug-in with a hole, a second sealant and contacts the second metal electrode.

[0011] The invention uses a 4mm sealed solid nuclear magnetic resonance sample cell (nuclear magnetic resonance rotor) designed and processed independently as a shell, and the nuclear magnetic resonance sample cell includes a driving cap and a sample cavity, and the driving cap is located above the solid nuclear magnetic resonance sample cell. The solid nuclear magnetic resonance in-situ cell can rotate at a rate of 4kHz-6kHz in a strong magnetic field of 400M-800M.

[0012] Based on the above technical solution, further, the machinable ceramics and solid nuclear magnetic resonance sample pool are both custom-made, and are both processed with a small hole at the center, and the small hole at the bottom of the solid nuclear magnetic resonance sample pool is located at the axis position.

[0013] Based on the above technical solution, further, the material of the driver cap can be KELF or VESPEL, and a small hole is punched in the center of the commercial driver cap.

[0014] Based on the above technical solution, further, the conductive wire is a high-purity metal wire (purity>99.9%), which is light in weight, high in strength and has good conductivity.

[0015] Based on the above technical solution, further, the first conductive wire and the second conductive wire are respectively connected to an electrochemical workstation to complete the charging and discharging process.

[0016] Based on the above technical solution, further, the first fixing plug-in, the second fixing plug-in, the first sealant, the second sealant driving cap center hole or the solid nuclear magnetic resonance sample cell bottom small hole through which the conductive wire penetrates on both sides of the solid electrolyte are kept on the same axis to achieve long-term rotational stability of the rotor battery at the magic angle of the nuclear magnetic resonance spectrometer.

[0017] Based on the above technical solution, further, the machinable ceramic center small hole can be completed by using a drill bit and a manual electric drill to allow the conductive wire to pass through.

[0018] Based on the above technical solution, further, the first sealant and the first sealant material are fusible glue.

[0019] Based on the above technical solution, further, by heating and cooling the fusible adhesive, the conductive wire can be fixed and the battery can be sealed.

[0020] Based on the above technical solution, further, the first fixing plug-in and the second fixing plug-in are made of ceramic, soft clay or polytetrafluoroethylene.

[0021] Based on the above technical solution, further, the first sealant has the same size as the radial size of the sample cavity.

[0022] The lithium symmetrical battery is manufactured partially by melting lithium in a glove. The battery has a stable structure, a high repetition rate, and good sealing. It can realize the combination of rapid magic angle rotation in a nuclear magnetic resonance spectrometer and in-situ charge and discharge testing to obtain high-resolution and high-quality nuclear magnetic resonance spectra, which is convenient for studying the dynamic changes and reaction mechanisms of the battery.

[0023] The present invention designs a solid nuclear magnetic resonance in-situ rotor battery, cooperates with an electrochemical workbench, completes the charging and discharging of the battery, and realizes the solid nuclear magnetic resonance research of the in-situ solid-state battery in a sealed system. The equipment is mainly used in the currently widely used BRUKER solid nuclear magnetic resonance spectrometer. The solid nuclear magnetic resonance rotor is 4mm in size and rotates at a high speed of 4kHz. After sealing, it rotates at a high speed in a strong magnetic field to avoid oxidation of the metal electrode. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is a schematic diagram of the partial structure of a symmetrical solid-state metal battery;

[0025] Figure 2 is a schematic diagram of the rotor structure;

[0026] Figure 3 It is a schematic diagram of the battery structure inside the rotor;

[0027] Figure 4 Schematic diagram of the complete in-situ solid-state NMR magic angle spinning rotor battery structure. DETAILED DESCRIPTION

[0028] The following non-limiting embodiments may enable a person skilled in the art to more fully understand the present invention, but are not intended to limit the present invention in any way.

[0029] The in-situ solid nuclear magnetic resonance magic angle spinning rotor battery provided by the present invention realizes the collection of high-resolution nuclear magnetic resonance spectra under the in-situ charging and discharging conditions of the solid-state metal battery.

[0030] like Figure 4 As shown, a solid nuclear magnetic resonance magic angle spinning rotor battery comprises a rotor, wherein the rotor comprises a driving cap 2 with a hole in the center and a solid nuclear magnetic resonance sample cell 1 with a sample cavity that matches each other; the solid nuclear magnetic resonance sample cell has a hole in the center at the bottom;

[0031] The sample cavity of the solid NMR sample cell is provided with a first fixing plug-in 3 with an axial center hole, a first sealant 4, a first metal electrode 5, a solid electrolyte 6, a second metal electrode 7, a second sealant 8, and a second fixing plug-in 9 with a hole in sequence from the bottom;

[0032] It also includes a first conductive wire 10 and a second conductive wire 11. The first conductive wire passes through the bottom hole of the solid nuclear magnetic resonance sample cell, a first fixed plug-in with a hole, a first sealant and contacts the first metal electrode; the second conductive wire passes through a driving cap with a hole in the center, a second fixed plug-in with a hole, a second sealant and contacts the second metal electrode.

[0033] The solid-state nuclear magnetic resonance magic angle spinning rotor battery can rotate at a rate of 4kHz in a strong magnetic field;

[0034] The solid nuclear magnetic resonance sample cell is a nuclear magnetic resonance sample cell with an upper end opening, the upper end of the sample cavity is open and the lower end is sealed, and the driving cap and the sample cavity are sealed and connected by using fusible glue.

[0035] The diameters of the first fixing plug-in, the second fixing plug-in and the solid electrolyte are consistent with the inner diameter of the sample cavity.

[0036] The driving cap of the nuclear magnetic resonance sample cell with an opening at the upper end is made of KELF.

[0037] The first fixing plug-in and the second fixing plug-in are made of ceramic.

[0038] The solid NMR sample cell has a diameter of 4 mm and a length of 17.5 mm.

[0039] The first fixed plug-in, the second fixed plug-in and the solid electrolyte part in the battery can be processed into a fixed shape and size.

[0040] 1.LLZO(Li 7 La 3 Zr 2 O 12 Electrolyte) Symmetrical battery assembly

[0041] like Figure 1 As shown, the LLZO symmetric battery is manufactured in a glove box: a metal sheet is heated using a heating table, and a clean stainless steel plate is placed on the heating table.

[0042] 1) Stand the solid electrolyte LLZO upright on the edge of a clean stainless steel plate for preheating so that the solid electrolyte is heated evenly;

[0043] 2) Place a lithium metal sheet in the middle of a stainless steel plate to melt the metal from a solid state to a liquid state;

[0044] 3) Use tweezers to hold one end of the preheated solid electrolyte and place it in the liquid. Take it out after 3 to 5 seconds and switch to the other end. Perform the same operation. Cool it down to complete the metal liquid infiltration and form symmetrical metal electrodes, namely the first metal electrode and the second metal electrode.

[0045] 2. LLZO Cell Assembly in In Situ NMR Rotor

[0046] The battery shell used in the solid-state NMR in-situ rotor battery is as follows Figure 2 The rotor shown in the figure has a 0.3 mm small hole at the bottom of the rotor solid NMR sample cell and the center of the driving cap, so that the two ends of the metal wire (i.e., the first conductive wire and the second conductive wire) pass through the two ends of the rotor, as shown in the figure. Figure 3As shown, since there are still pores between the metal wire (0.25mm) (i.e., the first conductive wire and the second conductive wire) and the perforated parts inside the first and second fixed plug-ins of the ceramic, it is impossible to fix the metal wire (i.e., the first conductive wire and the second conductive wire) and seal the inside of the battery. In order to overcome this problem, a fusible glue that has been heated is added to the contact part between the first and second fixed plug-ins of the ceramic material and the metal first and second conductive wires, so that the diameter of the fusible glue is consistent with the internal diameter of the solid nuclear magnetic resonance sample cell. After the battery is assembled, the rotor cavity is placed in an oven without installing the drive cap, heated for 5 minutes at 80 degrees and squeezed, so that the colloid part is fully in contact with the metal surface (i.e., the first metal electrode, the second metal electrode) and the metal wire (i.e., the first conductive wire and the second conductive wire), and taken out after 5 minutes, and the drive cap is installed.

Claims

1. A solid-state nuclear magnetic resonance magic angle spinning rotor battery, characterized in that: The invention comprises a rotor, wherein the rotor comprises a driving cap with a hole in the center and a solid nuclear magnetic resonance sample cell with a sample cavity which match each other; the solid nuclear magnetic resonance sample cell has a hole in the center at the bottom; The sample cavity of the solid nuclear magnetic resonance sample cell is provided with a first fixing plug-in with an axial center hole, a first sealant, a first metal electrode, a solid electrolyte, a second metal electrode, a second sealant, and a second fixing plug-in with a hole in sequence; It also includes a first conductive wire and a second conductive wire. The first conductive wire passes through the bottom hole of the solid nuclear magnetic resonance sample pool, a first fixed plug-in with a hole, a first sealant and contacts the first metal electrode; the second conductive wire passes through a driving cap with a hole in the center, a second fixed plug-in with a hole, a second sealant and contacts the second metal electrode.

2. The solid-state nuclear magnetic resonance magic angle spinning rotor battery according to claim 1, characterized in that: The solid nuclear magnetic resonance sample cell is a nuclear magnetic resonance sample cell with an upper end opening, the upper end of the sample cavity is open and the lower end is sealed, and the driving cap and the sample cavity are sealed and connected by using fusible glue.

3. The solid-state nuclear magnetic resonance magic angle spinning rotor battery according to claim 1, characterized in that: The diameters of the first fixing plug-in, the second fixing plug-in and the solid electrolyte are consistent with the inner diameter of the sample cavity.

4. The solid-state nuclear magnetic resonance magic angle spinning rotor battery according to claim 3, characterized in that: The drive cap is made of KELF or VESPEL.

5. The solid-state nuclear magnetic resonance magic angle spinning rotor battery according to claim 1, characterized in that: The first fixing plug-in and the second fixing plug-in are made of ceramic, soft clay or polytetrafluoroethylene.

6. The solid-state nuclear magnetic resonance magic angle spinning rotor battery according to claim 1, characterized in that: The solid NMR sample cell has a diameter of 4 mm and a length of 17.5 mm.

7. The solid-state nuclear magnetic resonance magic angle spinning rotor battery according to claim 1, characterized in that: The first fixed plug-in, the second fixed plug-in and the solid electrolyte part in the battery can be processed into a fixed shape and size.

8. The solid-state nuclear magnetic resonance magic angle spinning rotor battery according to claim 1, characterized in that: The first sealant has the same size as the radial size of the sample cavity.

9. The solid-state nuclear magnetic resonance magic angle spinning rotor battery according to claim 1, characterized in that: The first sealant is made of fusible glue.

10. The solid-state nuclear magnetic resonance magic angle spinning rotor battery according to claim 1, characterized in that: The solid nuclear magnetic resonance magic angle spinning rotor battery rotates at a rate of 4k-6kHz in a strong magnetic field.