TSV through hole morphology and etching method thereof

By adjusting the BOSCH process parameters, the shell pattern morphology of the through-silicon hole is changed from the bracket shape to the water drop shape, which solves the problems of the inner wall roughness and uneven side walls of the through-hole in laser drilling and deep silicon etching technology, and improves the The effects of PVD and electroplating improve the reliability of through holes and the performance of three-dimensional integrated systems.

CN118737952APending Publication Date: 2024-10-01HUBEI JIUFENGSHAN LAB
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410615848.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-17
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing deep silicon etching technology is difficult to produce through silicon holes with small apertures and high aspect ratios, and laser drilling causes roughness in the inner walls of the through holes and severe thermal damage. The side walls in the deep silicon etching process are not smooth, which affects the TSV. performance and reliability of three-dimensional integrated systems.

Method used

By adjusting the traditional BOSCH process parameters, the shell pattern morphology of the through silicon via is changed from a symmetrical bracket shape to an asymmetrical drop shape, reducing the sidewall curvature, improving the coverage and adhesion of the PVD and electroplating processes, using the PVD process Perform seed layer deposition.

Benefits of technology

Achieved better through-hole sidewall smoothness, improved PVD seed layer coverage and electroplating layer adhesion, reduced voiding in the electroplating process, and improved through-hole reliability and three-dimensional integrated system performance .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118737952A_ABST
    Figure CN118737952A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of deep silicon etching, in particular to a TSV through hole morphology and an etching method thereof. The TSV through hole comprises n water-drop-shaped shell patterns which are distributed in a circulating mode, and n is larger than or equal to 1. In each water-drop-shaped shell pattern, the maximum etching length in the horizontal direction is X, the etching depth in the vertical direction is Y, X divides the etching depth Y in the vertical direction into two parts, namely Y1 and Y2, and X is larger than or equal to Y1 and smaller than Y2; wherein the horizontal direction is the direction perpendicular to the axial direction of the through hole. According to the deep silicon etching shell pattern structure, a new way is opened, the problem that follow-up PVD and electroplating processes are difficult can be solved by redesigning the shape of the deep silicon etching shell pattern, the structure can be achieved only by changing parameters of a traditional deep silicon etching process (bosch), cost is low, and efficiency is high.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of deep silicon etching, and in particular to a TSV through-hole morphology and an etching method thereof. Background Art

[0002] As electronic devices develop towards miniaturization, multifunctionality and high power density, through silicon via (TSV) technology is gaining more and more attention in the industry. Through silicon via technology is a method of using vertical through silicon vias to penetrate the substrate to achieve electrical conduction, and is the core process for interconnecting stacked chips in three-dimensional integrated circuits.

[0003] The processing of through holes on the wafer is the core of TSV technology. At present, there are two main through hole processing technologies: laser drilling and deep reactive ion etching. The characteristics of the two are shown in Table 1 below:

[0004] Table 1 Hot spots of different through-hole fabrication technologies

[0005] Manufacturing process Aperture Width ratio Roughness Uniformity Through hole angle Production efficiency cost Laser drilling >20μm >20 generally Difference About 85 degrees Low generally Deep silicon etching <5μm 20 good good 90 degrees high high

[0006] As a process that does not require a mask, laser technology avoids the process steps of photoresist coating, photolithography exposure, development and debonding, and has made significant progress. However, laser drilling also has its shortcomings. First, it cannot meet the needs of making through-holes with smaller apertures and high aspect ratios. Second, silicon will solidify quickly after melting, which can easily form nodules on the surface of the through-hole, making the inner wall of the through-hole rough and difficult to deposit a continuous insulating layer / seed layer. Third, the sub-surface thermal damage of the inner wall of the through-hole in laser technology is relatively large, which affects the reliability of the hole after filling, and the dimensional accuracy of the through-hole is less than 5μm. For details, please refer to Figure 1 , 2 ,in Figure 1 This is the laser drilling morphology. Figure 2 It is the subsurface thermal damage area of ​​laser drilling.

[0007] Deep silicon etching processes include wet etching and dry etching. The advantage of wet etching is that the obtained structure has larger geometric dimensions and better mechanical properties. Wet etching is widely used in devices such as acceleration sensors and pressure sensors due to its advantages such as simple process and low cost. However, a large amount of chemicals are required in the wet etching process, which will pollute the environment, and it is only suitable for thicker line widths (greater than 3μm). Unlike the good directionality of dry etching, due to the isotropic etching principle of wet etching, the fidelity of the etched pattern is ultimately not ideal.

[0008] The deep silicon etching process (BOSCH) dry etching technology is the current mainstream through silicon via etching method. Deep silicon etching can form vertical through holes with a very high aspect ratio. However, since two steps containing different plasmas are used alternately for etching during the process, the side walls of the through holes formed are not smooth, uneven, and wave-like, also known as scalloping or roughness, and their size generally ranges from tens of nanometers to hundreds of nanometers. Scalloping patterns will cause the subsequent filling of each layer of PVD seed layer material and the interface between them to be uneven, which will seriously affect the performance of TSV and the reliability of three-dimensional integrated systems.

[0009] In order to solve the above problems, the commonly used means in the prior art is to flatten the sidewalls of the silicon vias. For example, the invention patent with publication number CN103972161B discloses a SiCoNi etching method for modifying the morphology of silicon vias, and the invention patent with publication number CN105140174A also discloses a method for flattening the sidewalls of TSV vias. Flattening the sidewalls of silicon vias has been proven to be a feasible solution and is widely adopted by the industry. However, this method is complicated to operate, requires the use of new equipment, adds new operating steps, has high manufacturing costs, and is inefficient. Summary of the invention

[0010] Based on this, the present invention takes a different approach and solves the above-mentioned problem by redesigning the morphology of deep silicon etching shell patterns. Moreover, the structure can be realized simply by changing the parameters of the traditional Bosch, which is low-cost and high-efficiency.

[0011] The technical solution of the present invention to solve the above technical problems is as follows: a TSV through hole morphology, wherein the TSV through hole comprises n circularly arranged "water drop-shaped" shell patterns, where n≥1;

[0012] In each "water drop-shaped" shell pattern, the maximum etching length in the horizontal direction is X, and the etching depth in the vertical direction is Y. X divides the etching depth Y in the vertical direction into two, namely Y1 and Y2, wherein Y1≤X<Y2; wherein the horizontal direction is the direction perpendicular to the axial direction of the through hole.

[0013] As a preferred implementation, the TSV through hole has an etching length X in the horizontal direction of 100 nm and an etching depth Y in the vertical direction of 250 nm.

[0014] As another preferred implementation, the etching length X in the horizontal direction is 100 nm, the etching depth Y in the vertical direction is 250 nm, Y1 is 100 nm, and Y2 is 150 nm.

[0015] Furthermore, the "water drop-shaped" shell pattern is a structure that is wide at the top and narrow at the bottom, or narrow at the top and wide at the bottom.

[0016] The present invention also provides a method for etching the above-mentioned TSV through-hole morphology, which is specifically achieved by adjusting etching parameters in the Bosch process.

[0017] The present invention also provides the method for depositing an electroplating layer in the TSV through hole as described above, preferably a PVD process.

[0018] Furthermore, when the water drop-shaped shell pattern is a structure that is narrow at the top and wide at the bottom, a PVD machine with an enhanced negative bias voltage at the bottom is used for deposition.

[0019] Furthermore, when the water drop-shaped shell pattern is a structure that is wide at the top and narrow at the bottom, a PVD machine without an enhanced negative bias at the bottom is used for deposition.

[0020] The present invention changes the shell pattern morphology in the traditional TSV through hole to make it present an asymmetric "water drop pattern" morphology. The change can be achieved only by adjusting the etching parameters and is more conducive to PVD and electroplating processes. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 A topographical diagram of a through hole formed by laser drilling in the prior art;

[0022] Figure 2 It is the sub-surface thermal damage area of ​​the material after laser drilling in the prior art;

[0023] Figure 3 Schematic diagram of the morphology of shell patterns of different shapes and sizes;

[0024] Figure 4 A morphology diagram of the TSV through hole described in the present invention;

[0025] Figure 5 for Figure 3 SEM cross-sectional images of shell patterns of different shapes and sizes after electroplating. DETAILED DESCRIPTION

[0026] In order to facilitate understanding of the present application, the present application will be described more fully below with reference to the relevant drawings. Embodiments of the present application are provided in the drawings. However, the present application can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present application more thorough and comprehensive.

[0027] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application.

[0028] like Figure 4As shown, the TSV through hole morphology provided by the present invention includes n circularly arranged "water drop-shaped" shell patterns, wherein n≥1.

[0029] The definition of the teardrop shape in the present invention is as follows: based on the cut edge of the shell pattern, the etching length in the horizontal direction is X (that is, the maximum etching length in the horizontal direction is X), and the etching depth in the vertical direction is Y. X divides the etching depth Y in the vertical direction into two, namely Y1 and Y2, wherein Y1≤X<Y2, the horizontal direction is the direction perpendicular to the axial direction of the through hole, and the vertical direction is the axial direction of the through hole.

[0030] The present invention adjusts the size and shape of the shell-patterned scallop from the traditional "bracket shape" to a "water drop shape". When the size of the scallop remains at 100nm, the "water drop shape" can reduce the curvature of the curve of the side wall after etching, thereby enabling the PVD seed layer to be better sputtered from the bottom into the side wall of the upper half of the arc, thereby improving the coverage of the PVD.

[0031] It can be understood that the "tear drop shape" can be either a "wide on top and narrow on the bottom" structure or a "narrow on top and wide on the bottom", which can be determined according to different PVD equipment. For PVD machines that do not contain an enhanced negative bias at the bottom, the metal ions may not be attracted to the bottom and sputtered onto the side walls, but directly sputtered onto the side walls. In this case, the positive "tear drop shape" shell pattern that is wide on the top and narrow on the bottom is more conducive to the deposition of the PVD process, and this is also suitable for through holes with a relatively small aspect ratio.

[0032] The above structure is based on the traditional Bosch process only. By adjusting the etching parameters in a personalized way, such as reducing the E1 / E2 time (etching the passivation layer / Si time) or pressure, gas and other parameters in the Bosch process, the morphology of the traditional deep silicon etching shell pattern can be changed from a symmetrical "bracket shape" to a "water drop shape", which greatly reduces the curvature of the shell pattern at the maximum bending degree, which is beneficial to the subsequent deposition of the seed layer. Specifically, for example, in the parameters of the original Bosch process, the etching time of E1 is increased, and the etching time of the original E2 is reduced, that is, the time for bombarding the passivation layer and the time for Si etching in each cycle are increased, so that the original symmetrical shell pattern can be changed from a bracket shape to an asymmetric water drop shape.

[0033] Figure 3 The three different morphologies of deep silicon etched shell patterns were subjected to the same PVD (Ti / W) + AU electroplating process, and then the cross-section was observed by SEM. The results are as follows: Figure 5 shown.

[0034] Depend on Figure 5It can be seen that when the shell pattern is a 200nm "bracket shape", after the PVD+ electroplating process, there are large voids in the upper half of the arc side wall, proving that the PVD layer is not sputtered, resulting in poor adhesion of the electroplating layer and the formation of voids; when the shell pattern is a 100nm "bracket shape", after the PVD+ electroplating process, there are obvious voids at the connection between the two arcs, indicating that the PVD seed layer is not sputtered uniformly; when the shell pattern is a 100nm "water drop shape", a seed layer with a thickness of about 10nm can still be seen at the place where the side wall arc curvature is the largest, so no obvious voids are seen after the electroplating process. The above well illustrates that by adjusting the scallop shape of the shell pattern, it can be more conducive to the deposition of the PVD seed layer, thereby improving the adhesion of the electroplating layer and effectively reducing the void phenomenon in the electroplating process.

[0035] The present invention Figure 5 The 100nm "water drop-shaped" shell pattern has Y1 of 100nm and Y2 of 150nm. The specific etching process is: 320 loops of Bosch process, etching depth of 120um, TSV etching angle of 90°. PVD and electroplating process are: TiW / Au=50nm / 200nm.

[0036] It should be noted that in the description of the present application, the drawings and the description of the embodiments are illustrative rather than restrictive, and the same drawings throughout the embodiments of the specification mark the same structure. In addition, for the sake of understanding and ease of description, the drawings may exaggerate the thickness of some layers, films, panels, regions, etc. In addition, the terms "upper", "lower", "top", "bottom", "inner", "outer", etc. indicate the orientation or position relationship based on the orientation or position relationship shown in the drawings, which is only for the convenience of describing the present application and simplifying the description, and does not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present application.

[0037] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A TSV through-hole morphology, It is characterized in that The TSV through hole includes n "water drop-shaped" shell patterns arranged in a cycle, n≥1; In each "water drop-shaped" shell pattern, the maximum etching length in the horizontal direction is X, and the etching depth in the vertical direction is Y. X divides the etching depth Y in the vertical direction into two parts, namely Y1 and Y2, where Y1≤X<Y2; Wherein, the horizontal direction is a direction perpendicular to the axial direction of the through hole.

2. The TSV through hole morphology according to claim 1, It is characterized in that The etching length X in the horizontal direction is 100 nm, and the etching depth Y in the vertical direction is 250 nm.

3. The TSV through hole morphology according to claim 1, It is characterized in that The etching length X in the horizontal direction is 100 nm, the etching depth Y in the vertical direction is 250 nm, Y1 is 100 nm, and Y2 is 150 nm.

4. The TSV through hole morphology according to claim 1, It is characterized in that The "teardrop-shaped" shell pattern is a structure that is wide at the top and narrow at the bottom, or narrow at the top and wide at the bottom.

5. The TSV through-hole etching method according to any one of claims 1 to 4, It is characterized in that This is achieved by adjusting the etching parameters in the Bosch process.

6. The method for depositing a TSV through hole electroplating layer as claimed in any one of claims 1 to 4, It is characterized in that The deposition process is a PVD process.

7. The method according to claim 6, It is characterized in that When the "water drop-shaped" shell pattern is a structure that is narrow at the top and wide at the bottom, a PVD machine with an enhanced negative bias at the bottom is used for deposition.

8. The method according to claim 6, It is characterized in that When the "water drop-shaped" shell pattern is a structure that is wide at the top and narrow at the bottom, a PVD machine without an enhanced negative bias at the bottom is used for deposition.