Additive for photovoltaic electroplating process and electro-deposition copper electroplating solution

By using electrodeposition copper plating solution with additives such as 1,4-butynediol, 3-mercapto-1-propane sulfonate in the photovoltaic electroplating process, the high cost of silver electrodes of photovoltaic cell and the resistance of electroplating copper gate wires is solved. The problem has achieved cost reduction and efficiency improvement.

CN118996551APending Publication Date: 2024-11-22SUZHOU HAOSHEN INTELLIGENT TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411211564.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The high cost and width limitation of silver electrodes in the metallization process of existing photovoltaic cells hinder cost reduction and photoelectric conversion efficiency improvement, and the electroplated copper gate lines have problems such as excessive resistance and high resistivity.

Method used

Using an electrodeposition copper electroplating solution including additives such as 1,4-butyne glycol, sodium 3-mercapto-1-propane sulfonate, sodium polydisulfonate, sodium polydisulfonate, and so on, the plating layer is reduced by optimizing the copper ion deposition process. Internal stress improves the fine uniformity and conductivity of the copper layer.

Benefits of technology

It has achieved the reduction of the production cost of photovoltaic cells, improved power generation efficiency, solved the problem of excessive resistivity and resistance, and obtained a finer and even copper layer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996551A_ABST
    Figure CN118996551A_ABST
Patent Text Reader

Abstract

The invention discloses an additive for a photovoltaic electroplating process and an electro-deposition copper electroplating solution, the additive comprises a first additive, a second additive and a third additive, the first additive is selected from one or more of 1, 4-butynediol, 3-mercapto-1-sodium propane sulfonate and sodium 3, 4-dithiodipropane sulfonate, the second additive is selected from one or more of 1, 4-butynediol, 3-mercapto-1-sodium propane sulfonate and sodium 3, 4-dithiodipropane sulfonate, and the third additive is selected from one or more of sodium 3, 4-dithiodipropane sulfonate. The second additive is selected from one or more of polyethylene glycol, polypropylene glycol and propargyl alcohol, and the third additive is selected from 1-propynyl glyceryl ether and / or sodium edetate. The electrodeposition copper electroplating liquid prepared from the additive provided by the invention can optimize the photovoltaic cell electroplating process, so that an electrode shape beneficial to improving the power generation efficiency of a photovoltaic cell piece is obtained, and the additive has a wide application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of electroplating materials, and in particular to an additive for a photovoltaic electroplating process and an electrodeposited copper electroplating solution. Background Art

[0002] At present, photovoltaic cells are all made by screen printing silver paste and then sintering at high or low temperature to form silver electrodes to collect and transmit charges. This method is simple in process and is currently the most widely used photovoltaic cell metallization method. In recent years, the silver paste used in the metallization process is expensive, and the width and aspect ratio of the silver electrode in the metallization process are limited by the screen printing process, which not only leads to the continuous increase in the proportion of silver paste in the production cost of photovoltaic cells, but also the inability to further reduce the total production cost, and also hinders the further improvement of the photovoltaic cell photoelectric conversion efficiency. In order to further reduce the cost of photovoltaic cells and improve the photovoltaic cell photoelectric conversion efficiency, the demand for the use of electroplating to make photovoltaic cell metal electrodes is increasing. This method can use cheaper metals such as copper to replace silver, which can not only reduce costs, but also further reduce the width of the grid line through graphic transfer, reduce the shading area, and improve the power generation efficiency of photovoltaic cells.

[0003] Electroplated copper plays a key role in modern electronic industry applications due to its high reliability, productivity and low cost advantages, while meeting the transmission characteristics of electricity and heat. Additives are an important component of the electroplating solution and play an irreplaceable role in the electroplating process. Additives can effectively improve the current distribution during the electroplating process, improve the plating ability of the plating solution, affect the transportation and electrocrystallization process of copper ions from the solution body to the reaction interface, and thus change the electrochemical deposition rate of the micro-concave and micro-convex parts of the board surface. The existing electroplating technology is generally more traditional electroplating, and the electroplated copper grid lines have problems such as excessive resistance and high resistivity. Summary of the invention

[0004] In order to solve the above technical problems, the purpose of the present invention is to provide an additive for photovoltaic electroplating process.

[0005] A further object of the present invention is to provide an electrodeposition copper plating solution for photovoltaic electroplating process.

[0006] The third object of the present invention is to provide a photovoltaic copper electroplating process.

[0007] The above object of the present invention is achieved through the following technical solutions:

[0008] The first aspect of the present invention provides an additive for a photovoltaic electroplating process, wherein the additive comprises a first additive, a second additive and a third additive, wherein the first additive is selected from one or more of 1,4-butynediol (CAS No.: 110-65-6), sodium 3-mercapto-1-propane sulfonate (CAS No.: 17636-10-1) and sodium polydisulfide propane sulfonate (CAS No.: 27206-35-5), the second additive is selected from one or more of polyethylene glycol (CAS No.: 25322-68-3), polypropylene glycol (CAS No.: 25322-69-4) and propargyl alcohol (CAS No.: 107-19-7), and the third additive is selected from 1-propynyl glycerol ether (CAS No.: 80-38-6) and / or sodium edetate (CAS No.: 126-92-1).

[0009] The additive provided by the present invention has the functions of a leveling agent, an accelerator, an inhibitor, a stabilizer, etc. It is a mixed additive and does not need to be mixed with other reagents again in a certain proportion when used. It can be directly added and used to meet the requirements of photovoltaic cell electroplating, and has broad application prospects.

[0010] Furthermore, the mass ratio of the first additive, the second additive and the third additive is (5-15):(5-15):(1-3), preferably 5:5:(1-3).

[0011] The additive provided by the invention can be used to prepare an electroplating copper electroplating solution, and can ensure that the electroplating solution has good conductivity, while the deposited copper is relatively fine and uniform.

[0012] A second aspect of the present invention provides an electroplating copper solution for use in a photovoltaic electroplating process, wherein the electroplating copper solution comprises the additive described in the first aspect.

[0013] The electroplated copper plating solution provided by the present invention contains additives, which can be adsorbed on the copper surface to obtain the deposition of leveled copper ions, while significantly reducing the internal stress between the molecules of the plated layer, ultimately achieving the copper layer shape required by the photovoltaic cell sheet, and solving the problems of excessive resistance and high resistivity of the electroplated copper grid line.

[0014] Furthermore, the concentration of the additive in the electrodeposited copper plating solution is 100-400 g / L.

[0015] Furthermore, the electrodeposition copper plating solution also includes copper sulfate, sulfuric acid and chloride ions.

[0016] Furthermore, the concentration of copper sulfate in the electrodeposited copper plating solution is 200-220 g / L.

[0017] Furthermore, the concentration of sulfuric acid in the electrodeposited copper plating solution is 55-75 g / L.

[0018] Furthermore, the concentration of chloride ions in the electrodeposited copper plating solution is 55-65 ppm.

[0019] The third aspect of the present invention provides a photovoltaic copper electroplating process, comprising the following steps: placing a photovoltaic cell and a titanium mesh in the electrodeposition copper electroplating solution described in the second aspect, with the photovoltaic cell serving as a cathode and the titanium mesh serving as an anode, and applying power to the cathode and the anode for photovoltaic copper electroplating.

[0020] Furthermore, the surface of the titanium mesh is covered with an iridium oxide coating.

[0021] Beneficial effects of the present invention:

[0022] 1. The additive provided by the present invention is a mixed additive. When used, it does not need to be mixed with other reagents again in a certain ratio. It can be directly added and used to meet the requirements of photovoltaic cell electroplating, and has broad application prospects.

[0023] 2. The electroplating copper plating solution configured with additives provided by the present invention can optimize the electroplating process of photovoltaic cells, thereby obtaining an electrode shape that is beneficial to improving the power generation efficiency of photovoltaic cells, and has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is a metallographic image of a photovoltaic cell grid line cross section obtained by using the electrodeposited copper plating solution of Example 1 in a photovoltaic copper electroplating process.

[0025] Figure 2 This is a metallographic image of the grid lines of a photovoltaic cell obtained by using the electrodeposited copper plating solution of Example 2 in a photovoltaic copper electroplating process.

[0026] Figure 3 This is a metallographic image of the grid lines of a photovoltaic cell obtained by using the electrodeposited copper plating solution of Example 3 in a photovoltaic copper electroplating process.

[0027] Figure 4 This is a metallographic image of the grid lines of a photovoltaic cell obtained by using the electrodeposited copper plating solution of Comparative Example 1 in a photovoltaic copper electroplating process. DETAILED DESCRIPTION

[0028] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0029] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.

[0030] Unless otherwise specified, the experimental methods used in the following examples are all conventional methods, and the materials, reagents, etc. used are all available from commercial sources unless otherwise specified.

[0031] Example 1

[0032] An electrodeposited copper plating solution for photovoltaic electroplating process comprises additives (a first additive 1,4-butynediol, a second additive polyethylene glycol and a third additive 1-propynyl glycerol ether), copper sulfate pentahydrate, sulfuric acid and hydrochloric acid, and a preparation method comprises the following steps:

[0033] 220 g of copper sulfate pentahydrate was dissolved in 1 L of deionized water, 30.5 mL of sulfuric acid was slowly added, hydrochloric acid was added to make the chloride ion concentration 55 ppm, 110 g of additives (50 g of the first additive 1,4-butynediol, 50 g of the second additive polyethylene glycol and 10 g of the third additive 1-propynyl glycerol ether) were added, and mixed to obtain an electrodeposited copper plating solution.

[0034] The electroplating copper solution of Example 1 is used in a photovoltaic copper electroplating process, comprising the following steps:

[0035] (1) Cut the photovoltaic cell into slices (2×2cm 2 ) is immersed in ethanol for 5 minutes to remove pollutants from the slices, and then rinsed with deionized water to ensure that the pollutants are rinsed clean to obtain a pretreated photovoltaic cell slice.

[0036] (2) Immerse the pretreated photovoltaic cell in an electroplated copper plating solution for 30 seconds to fully wet the surface of the cell.

[0037] (3) Pour the electroplated copper plating solution into the plating tank, place the soaked pretreated photovoltaic cell in the electroplated copper plating solution as the cathode, place the titanium mesh covered with iridium oxide coating in the electroplated copper plating solution as the anode, stir the electroplated copper plating solution stably, the magnetic stirring speed is 400r / min, and direct current is passed to the cathode and anode for photovoltaic copper electroplating. First, 1ASD electroplating is performed for 120s to pre-plate a copper seed layer, followed by 5ASD electroplating for 300s, and then 10ASD electroplating is performed for 20min.

[0038] Example 2

[0039] An electrodeposited copper plating solution for photovoltaic electroplating process comprises additives (a first additive, sodium 3-mercapto-1-propane sulfonate, a second additive, polypropylene glycol, and a third additive, sodium edetate), copper sulfate pentahydrate, sulfuric acid, and hydrochloric acid. The preparation method comprises the following steps:

[0040] Dissolve 220 g of copper sulfate pentahydrate in 1 L of deionized water, slowly add 30.5 mL of sulfuric acid, add hydrochloric acid to make the chloride ion concentration 55 ppm, add 220 g of additives (100 g of the first additive 3-mercapto-1-propane sulfonate sodium, 100 g of the second additive polypropylene glycol and 20 g of the third additive sodium edetate), and mix to obtain an electrodeposited copper plating solution.

[0041] The electroplating copper solution of Example 2 is used in a photovoltaic copper electroplating process, comprising the following steps:

[0042] (1) Slice the photovoltaic cell (2×2cm 2 ) is immersed in ethanol for 5 minutes to remove pollutants from the slices, and then rinsed with deionized water to ensure that the pollutants are rinsed clean to obtain a pretreated photovoltaic cell slice.

[0043] (2) Immerse the pretreated photovoltaic cell in an electroplated copper plating solution for 30 seconds to fully wet the surface of the cell.

[0044] (3) Pour the electroplated copper plating solution into the plating tank, place the soaked pretreated photovoltaic cell in the electroplated copper plating solution as the cathode, place the titanium mesh covered with iridium oxide coating in the electroplated copper plating solution as the anode, stir the electroplated copper plating solution stably, the magnetic stirring speed is 400r / min, and direct current is passed to the cathode and anode for photovoltaic copper electroplating. First, 1ASD electroplating is performed for 120s to pre-plate a copper seed layer, followed by 5ASD electroplating for 300s, and then 10ASD electroplating is performed for 20min.

[0045] Example 3

[0046] An electrodeposited copper electroplating solution for photovoltaic electroplating process comprises additives (a first additive sodium polydipropane disulfide sulfonate, a second additive propargyl alcohol, and a third additive 1-propynyl glyceryl ether and sodium edetate), copper sulfate pentahydrate, sulfuric acid and hydrochloric acid, and a preparation method comprises the following steps:

[0047] 220 g of copper sulfate pentahydrate was dissolved in 1 L of deionized water, 30.5 mL of sulfuric acid was slowly added, hydrochloric acid was added to make the chloride ion concentration 55 ppm, 330 g of additives (150 g of the first additive sodium polydisulfide dipropane sulfonate, 150 g of the second additive propargyl alcohol, and 30 g of the third additive 1-propynyl glyceryl ether and sodium edetate) were added, and mixed to obtain an electrodeposited copper plating solution.

[0048] The electroplating copper solution of Example 3 is used in a photovoltaic copper electroplating process, comprising the following steps:

[0049] (1) Slice the photovoltaic cell (2×2cm 2 ) is immersed in ethanol for 5 minutes to remove pollutants from the slices, and then rinsed with deionized water to ensure that the pollutants are rinsed clean to obtain a pretreated photovoltaic cell slice.

[0050] (2) Immerse the pretreated photovoltaic cell in an electroplated copper plating solution for 30 seconds to fully wet the surface of the cell.

[0051] (3) Pour the electroplated copper plating solution into the plating tank, place the soaked pretreated photovoltaic cell in the electroplated copper plating solution as the cathode, place the titanium mesh covered with iridium oxide coating in the electroplated copper plating solution as the anode, stir the electroplated copper plating solution stably, the magnetic stirring speed is 400r / min, and direct current is passed to the cathode and anode for photovoltaic copper electroplating. First, 1ASD electroplating is performed for 120s to pre-plate a copper seed layer, followed by 5ASD electroplating for 300s, and then 10ASD electroplating is performed for 20min.

[0052] Example 4

[0053] An electrodeposited copper plating solution for photovoltaic electroplating process comprises additives (a first additive 1,4-butynediol, a second additive polyethylene glycol and a third additive 1-propynyl glycerol ether), copper sulfate pentahydrate, sulfuric acid and hydrochloric acid, and a preparation method comprises the following steps:

[0054] 220 g of copper sulfate pentahydrate was dissolved in 1 L of deionized water, 30.5 mL of sulfuric acid was slowly added, hydrochloric acid was added to make the chloride ion concentration 55 ppm, 310 g of additives (200 g of the first additive 1,4-butynediol, 100 g of the second additive polyethylene glycol and 10 g of the third additive 1-propynyl glycerol ether) were added, and mixed to obtain an electrodeposited copper plating solution.

[0055] The electroplating copper solution of Example 4 is used in a photovoltaic copper electroplating process, and the process is basically the same as that of Example 1.

[0056] Example 5

[0057] An electrodeposited copper plating solution for photovoltaic electroplating process comprises additives (a first additive 1,4-butynediol, a second additive polyethylene glycol and a third additive 1-propynyl glycerol ether), copper sulfate pentahydrate, sulfuric acid and hydrochloric acid, and a preparation method comprises the following steps:

[0058] 220 g of copper sulfate pentahydrate was dissolved in 1 L of deionized water, 30.5 mL of sulfuric acid was slowly added, hydrochloric acid was added to make the chloride ion concentration 55 ppm, 210 g of additives (30 g of the first additive 1,4-butynediol, 150 g of the second additive polyethylene glycol and 30 g of the third additive 1-propynyl glycerol ether) were added, and mixed to obtain an electrodeposited copper plating solution.

[0059] The electroplating copper solution of Example 5 is used in a photovoltaic copper electroplating process, and the process is basically the same as that of Example 1.

[0060] Example 6

[0061] An electrodeposited copper plating solution for photovoltaic electroplating process comprises additives (a first additive 1,4-butynediol, a second additive polyethylene glycol and a third additive 1-propynyl glycerol ether), copper sulfate pentahydrate, sulfuric acid and hydrochloric acid, and a preparation method comprises the following steps:

[0062] 220 g of copper sulfate pentahydrate was dissolved in 1 L of deionized water, 30.5 mL of sulfuric acid was slowly added, hydrochloric acid was added to make the chloride ion concentration 55 ppm, 88 g of additives (40 g of the first additive 1,4-butynediol, 40 g of the second additive polyethylene glycol and 8 g of the third additive 1-propynyl glycerol ether) were added, and mixed to obtain an electrodeposited copper plating solution.

[0063] The electroplating copper solution of Example 6 is used in a photovoltaic copper electroplating process, and the process is basically the same as that of Example 1.

[0064] Example 7

[0065] An electrodeposited copper plating solution for photovoltaic electroplating process comprises additives (a first additive 1,4-butynediol, a second additive polyethylene glycol and a third additive 1-propynyl glycerol ether), copper sulfate pentahydrate, sulfuric acid and hydrochloric acid, and a preparation method comprises the following steps:

[0066] 220 g of copper sulfate pentahydrate was dissolved in 1 L of deionized water, 30.5 mL of sulfuric acid was slowly added, hydrochloric acid was added to make the chloride ion concentration 55 ppm, 500 g of additives (200 g of the first additive 1,4-butynediol, 200 g of the second additive polyethylene glycol and 100 g of the third additive 1-propynyl glycerol ether) were added, and mixed to obtain an electrodeposited copper plating solution.

[0067] The electroplating copper solution of Example 7 is used in a photovoltaic copper electroplating process, and the process is basically the same as that of Example 1.

[0068] Comparative Example 1

[0069] An electroplating copper plating solution for photovoltaic electroplating process comprises additives (a first additive, sodium 3-mercapto-1-propane sulfonate, and a second additive, polypropylene glycol), copper sulfate pentahydrate, sulfuric acid and hydrochloric acid, and a preparation method comprises the following steps:

[0070] Dissolve 220 g of copper sulfate pentahydrate in 1 L of deionized water, slowly add 30.5 mL of sulfuric acid, add hydrochloric acid to make the chloride ion concentration 55 ppm, add 400 g of additives (200 g of the first additive 3-mercapto-1-propane sulfonate sodium and 200 g of the second additive polypropylene glycol), and mix to obtain an electrodeposited copper plating solution.

[0071] The electroplating copper solution of Comparative Example 1 is used in a photovoltaic copper electroplating process, comprising the following steps:

[0072] (1) Cut the photovoltaic cell into slices (2×2cm 2 ) is immersed in ethanol for 5 minutes to remove pollutants from the slices, and then rinsed with deionized water to ensure that the pollutants are rinsed clean to obtain a pretreated photovoltaic cell slice.

[0073] (2) Immerse the pretreated photovoltaic cell in an electroplated copper plating solution for 30 seconds to fully wet the surface of the cell.

[0074] (3) Pour the electroplated copper plating solution into the plating tank, place the soaked pretreated photovoltaic cell in the electroplated copper plating solution as the cathode, place the titanium mesh covered with iridium oxide coating in the electroplated copper plating solution as the anode, stir the electroplated copper plating solution stably, the magnetic stirring speed is 400r / min, and direct current is passed to the cathode and anode for photovoltaic copper electroplating. First, 1ASD electroplating is performed for 120s to pre-plate a copper seed layer, followed by 5ASD electroplating for 300s, and then 10ASD electroplating is performed for 20min.

[0075] Comparative Example 2

[0076] An electroplating copper plating solution for photovoltaic electroplating process comprises additives (a first additive sodium 3-mercapto-1-propane sulfonate and a third additive sodium edetate), copper sulfate pentahydrate, sulfuric acid and hydrochloric acid, and a preparation method comprises the following steps:

[0077] 220 g of copper sulfate pentahydrate was dissolved in 1 L of deionized water, 30.5 mL of sulfuric acid was slowly added, hydrochloric acid was added to make the chloride ion concentration 55 ppm, 240 g of additives (200 g of the first additive sodium 3-mercapto-1-propane sulfonate and 40 g of the third additive sodium edetate) were added, and mixed to obtain an electrodeposited copper plating solution.

[0078] The electrodeposited copper plating solution of Comparative Example 2 was used in a photovoltaic copper electroplating process, and the process was basically the same as that of Example 1.

[0079] Comparative Example 3

[0080] An electrodeposited copper electroplating solution for photovoltaic electroplating process comprises additives (a second additive polypropylene glycol and a third additive sodium edetate), copper sulfate pentahydrate, sulfuric acid and hydrochloric acid, and a preparation method comprises the following steps:

[0081] Dissolve 220 g of copper sulfate pentahydrate in 1 L of deionized water, slowly add 30.5 mL of sulfuric acid, add hydrochloric acid to make the chloride ion concentration 55 ppm, add 240 g of additives (200 g of the second additive polypropylene glycol and 40 g of the third additive sodium edetate), and mix to obtain an electrodeposited copper plating solution.

[0082] The electrodeposited copper plating solution of Comparative Example 3 was used in a photovoltaic copper electroplating process, and the process was basically the same as that of Example 1.

[0083] Figure 1 This is a metallographic image of the cross-section of the photovoltaic cell grid line obtained by using the electroplated copper plating solution of Example 1 in the photovoltaic copper electroplating process. Figure 1 It can be seen that the electroplating thickness of Example 1 is insufficient, and the side wall angle of the electroplated grid line is about 40° (the side wall angle is preferably 80°), indicating that the electroplating efficiency is poor under this condition. Figure 1 Similar, the main problems are: first, the thickness is insufficient; second, the side wall angle does not reach 80°; third, the electroplated copper structure is not fine enough and cannot meet the good resistivity requirements.

[0084] Figure 2 This is a metallographic image of the grid lines of a photovoltaic cell obtained by using the electroplated copper electroplating solution of Example 2 in a photovoltaic copper electroplating process. Figure 3 This is a metallographic image of the grid lines of a photovoltaic cell obtained by using the electroplated copper plating solution of Example 3 in a photovoltaic copper electroplating process. Figure 2 , Figure 3 It can be seen that by using the additives, electroplating solution and copper electroplating process provided by the present invention, the grid line shape required by the photovoltaic cell can be obtained.

[0085] Figure 4 This is a metallographic image of the grid lines of a photovoltaic cell obtained by using the electroplated copper plating solution of Comparative Example 1 in a photovoltaic copper electroplating process. Figure 4 It can be seen that the photovoltaic cell grid line electroplating effect of the test board electroplated in the electroplating solution lacking the third additive in Comparative Example 1 is not good, the surface is protruding and has defects. The metallographic images of the photovoltaic cell grid line obtained by using the electroplating copper plating solution of Comparative Examples 2 to 3 for the photovoltaic copper electroplating process are Figure 4 resemblance.

[0086] The grid lines of the cell were cut into a certain width, and the resistivity of the grid lines of the photovoltaic cell obtained by using the electroplating copper plating solutions of Examples 1 to 7 and Comparative Examples 1 to 3 in the photovoltaic copper electroplating process was tested using a contact resistivity tester (Meineng Photovoltaic TLM-STD). The test results are shown in Table 1:

[0087] Table 1

[0088]

[0089]

[0090] Obviously, the above embodiments of the present invention are only examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. Those skilled in the art should understand that other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.

Claims

1. An additive for photovoltaic electroplating process, characterized in that: The additives include a first additive, a second additive and a third additive, wherein the first additive is selected from one or more of 1,4-butynediol, sodium 3-mercapto-1-propane sulfonate and sodium polydisulfide propane sulfonate, the second additive is selected from one or more of polyethylene glycol, polypropylene glycol and propargyl alcohol, and the third additive is selected from 1-propynyl glyceryl ether and / or sodium edetate.

2. The additive according to claim 1, characterized in that The mass ratio of the first additive, the second additive and the third additive is (5-15):(5-15):(1-3).

3. An electrodeposition copper plating solution for photovoltaic electroplating process, characterized in that: The electrodeposition copper plating solution comprises the additive according to claim 1 or 2.

4. The copper electrodeposition plating solution according to claim 3, characterized in that: The concentration of the additive in the electrodeposition copper plating solution is 100-400 g / L.

5. The copper electrodeposition plating solution according to claim 3, characterized in that: The electrodeposition copper plating solution also includes copper sulfate, sulfuric acid and chloride ions.

6. The copper electrodeposition plating solution according to claim 5, characterized in that: The concentration of copper sulfate in the electrodeposited copper plating solution is 200-220 g / L.

7. The copper electrodeposition plating solution according to claim 5, characterized in that: The concentration of sulfuric acid in the electrodeposition copper plating solution is 55-75 g / L.

8. The copper electrodeposition plating solution according to claim 5, characterized in that: The concentration of chloride ions in the electrodeposition copper plating solution is 55-65 ppm.

9. A photovoltaic copper electroplating process, characterized in that: The method comprises the following steps: placing a photovoltaic cell and a titanium mesh in the electroplating copper electroplating solution described in any one of claims 3 to 8, using the photovoltaic cell as a cathode and the titanium mesh as an anode, and applying power to the cathode and the anode for photovoltaic copper electroplating.