Lithium-rich manganese-based composite positive electrode material, preparation method thereof and battery
By forming a vanadium-phosphorus composite film on the surface of the lithium-rich manganese-based cathode material, the problem of structural instability and surface residual alkali under high voltage conditions is solved, the cycle performance and electrochemical performance are significantly improved, the battery life is extended and the battery life is reduced. voltage attenuation and internal resistance.
Patent Information
- Application Number
- CN202410896892.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-10-01
AI Technical Summary
The irreversible release of oxygen and the transformation of the layered structure to a spinel structure of lithium-rich manganese-based cathode materials under high voltage conditions lead to voltage decay, poor cycle performance, high surface residual alkali and increased process costs, limiting their commercial application. .
It adopts a vanadium-phosphorus composite film coating layer composed of a core and a vanadium compound and a phosphorus compound. Through the synergistic effect of the vanadium compound and the phosphorus compound, it enhances structural stability, isolates the electrolyte, reduces side reactions, and forms lithium vanadate to improve conductivity and Thermal stability, and reducing surface residual alkali through acidic phosphorus compounds, improving lattice stability and cycle performance.
It significantly improves the cycle performance and electrochemical performance of lithium-rich manganese-based cathode materials, extends battery life, reduces voltage attenuation and internal resistance, and improves capacity retention and electrochemical performance.
Smart Images

Figure CN118738339A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of lithium-ion batteries, and in particular relates to a lithium-rich manganese-based composite positive electrode material and a preparation method thereof, and a battery. Background Art
[0002] With the continuous development of the new energy industry, the demand for energy storage is also growing rapidly. Whether it is new energy power generation, 5G base station construction or the development of electric vehicles, higher demands are being placed on energy storage materials.
[0003] Compared with the currently commercialized lithium iron phosphate materials and various ternary cathode materials, lithium-rich manganese-based cathode materials have attracted much attention due to their high theoretical specific capacity and low price. They have a wide voltage window of 2 to 4.8 V, and their theoretical capacity can reach up to 300 mAh g -1 , which is the highest in current positive electrode materials; in addition, the increase of manganese element can also reduce the use of expensive and scarce nickel and cobalt, and the cost of raw materials is lower.
[0004] However, its irreversible release of oxygen under high voltage and the transformation of layered structure to spinel structure caused by oxygen release limit its commercialization process. Therefore, a lot of current research work is centered around these problems of lithium-rich manganese-based materials.
[0005] At present, there are problems with lithium-rich manganese-based positive electrode materials: First, the button cell or full battery assembled with the material has a serious voltage drop during the cycle. Second, due to the precipitation of lattice oxygen, the first cycle coulomb efficiency is low, the first efficiency is ≤85%, and the material cycle performance is poor. Third, affected by the synthesis route and the properties of the lithium-rich manganese-based material itself, the residual alkali on the surface of the material is high, which may cause the slurry to gel into a jelly-like state during the full battery homogenization process, increasing the process cost and process difficulty.
[0006] In order to solve the problems of lithium-rich manganese-based positive electrode materials mentioned above, commonly used modification strategies include surface coating, doping, surface pretreatment, etc. However, because the structure of lithium-rich manganese-based positive electrode materials is still unclear, the synthesis and modification of lithium-rich manganese-based positive electrode materials are still in a development stage, and there is still a lot of room for improvement in the performance of lithium-rich manganese-based positive electrode materials. Therefore, providing a new preparation method of lithium-rich manganese-based composite positive electrode material to further improve the current problems of lithium-rich manganese-based positive electrode materials is of great significance for the application of lithium-rich manganese-based positive electrode materials in lithium-ion batteries. Summary of the invention
[0007] In order to solve the problems and shortcomings in the prior art, the present invention provides a lithium-rich manganese-based composite positive electrode material and a preparation method and a battery. The lithium-rich manganese-based composite positive electrode material has a high first efficiency and first-cycle discharge capacity, and the composite positive electrode material still has a high capacity retention rate after multiple cycles. It is a lithium-rich manganese-based composite positive electrode material with excellent performance, which is of great significance for its application in lithium batteries.
[0008] According to a first aspect of the present invention, a lithium-rich manganese-based composite positive electrode material is provided, comprising a core and a coating layer coated on the surface of the core, wherein the core comprises a lithium-rich manganese-based positive electrode material having a chemical structural formula of xLi2MnO3·(1-x)LiNi 0.5 Mn 0.5 O2, x has a value of 0.1 to 0.95; the coating layer includes a vanadium compound and a phosphorus compound; the vanadium compound includes at least one of vanadium pentoxide and lithium vanadate; the phosphorus compound includes at least one of phosphorus pentoxide, iron phosphate and iron pyrophosphate.
[0009] A coating layer including vanadium compounds and phosphorus compounds (referred to as vanadium-phosphorus composite film) is formed on the surface of the lithium-rich manganese-based positive electrode material whose core is a lithium-rich manganese-based positive electrode material. First, the vanadium-phosphorus composite film effectively protects the lithium-rich manganese-based positive electrode material, isolates the electrolyte from direct contact with the lithium-rich manganese-based positive electrode material, and thus reduces the occurrence of side reactions. Second, the vanadium-phosphorus composite film can further enhance the structural stability of the lithium-rich manganese-based positive electrode material, making it less likely to collapse and break due to cyclic stress during the charge and discharge cycle, improve its cycle performance, slow down its voltage decay rate, and improve the gram capacity and capacity retention rate. Third, the structural formula of the vanadium compound contains oxygen elements, so the vanadium compound can form lithium vanadate (LiVO3) with the lithium salt in the electrolyte. Lithium vanadate has good thermal stability and chemical stability, as well as high specific capacity and high electrical conductivity. Therefore, it can further improve the capacity and cycle retention rate of the positive electrode material, and reduce the voltage decay of the battery with the lithium-rich manganese-based material as the positive electrode, effectively improving the electrochemical performance of the battery. Fourth, phosphorus compounds are acidic, which can reduce the residual alkali on the surface of lithium-rich manganese-based positive electrode materials, improve battery cycle stability, reduce internal resistance, and increase battery life. This is because, first, the presence of surface residual alkali will change the charge distribution on the surface of the positive electrode material, resulting in accelerated capacity decay during the cycle, thereby reducing the cycle stability of the battery. Second, the surface residual alkali will form an insulating layer on the surface of the electrode, hindering the transmission of electrons and ions, thereby increasing the internal resistance of the battery. This will lead to a decrease in the rate performance of the battery, and the temperature rise phenomenon during the charging and discharging process will be more obvious. Third, due to the negative impact of surface residual alkali on battery performance, the life of the battery will be greatly affected. In a high temperature and high humidity environment, the surface residual alkali will also react with oxygen in the air, further shortening the life of the battery. Fifth, vanadium compounds contain oxygen, acidic phosphorus compounds generally contain oxygen, and lithium-rich manganese-based positive electrode materials also contain oxygen. Therefore, vanadium compounds and phosphorus compounds can form a surface with a compatible lattice structure, inhibiting the lapse of lattice oxygen in lithium-rich manganese-based positive electrode materials, further improving the lattice stability of lithium-rich manganese-based positive electrode materials, and improving their electrochemical properties such as cycle performance.
[0010] It should be noted here that in xLi2MnO3·(1-x)LiNi 0.5 Mn 0.5 In O2, the x value changes with the change of the Li ratio, Ni and Mn sum. Different x values will affect the electrochemical properties such as the discharge capacity of the positive electrode material. Usually, R&D personnel can adjust the x value according to different design requirements.
[0011] Preferably, the chemical structure of the lithium-rich manganese-based positive electrode material is 0.4Li2MnO3·0.6LiNi 0.5 Mn 0.5 O2.
[0012] Preferably, the total content of V and P in the lithium-rich manganese-based composite positive electrode material is 500-1000ppm. If the content of vanadium compounds and phosphorus compounds is too low, the coating thickness is low, and the protection effect on the lithium-rich manganese-based positive electrode material is poor. In addition, the amount of lithium vanadate formed by the vanadium compound and the lithium salt in the subsequent battery cycle is also small, which is not conducive to fully improving the electrochemical properties of the material. If the content of vanadium compounds and phosphorus compounds is too high and the coating film formed is too thick, the transmission efficiency of lithium ions will be reduced, which is not conducive to the cycle performance of the material.
[0013] Preferably, in the coating layer, the molar ratio of V to P is 0.1-0.9:0.1-0.9.
[0014] Preferably, in the coating layer, the vanadium compound is vanadium pentoxide and the phosphorus compound is phosphorus pentoxide. The vanadium-phosphorus composite film composed of these two compounds has the best improvement effect on the lithium-rich manganese-based positive electrode material, which may be due to the fact that these two substances have a certain synergistic effect on the lithium-rich manganese-based positive electrode material, and thus can further improve the electrochemical performance of the lithium-rich manganese-based positive electrode material. It should be noted here that because the lithium-rich manganese-based material originally has a high lithium content, there can be excess lithium fed back to vanadium pentoxide, so a certain amount of lithium vanadate can be formed to improve the cycle performance of the material. If the vanadium compound uses lithium vanadate from the beginning, on the one hand, the cost of lithium vanadate is higher, and on the other hand, in practical applications, the coating effect of lithium vanadate is worse than that of vanadium pentoxide. For example, the cycle performance of the positive electrode material coated with vanadium pentoxide is better, because lithium vanadate reacts slowly at the beginning during the battery cycle, which may be due to the relatively slow lithium ion deintercalation speed at the beginning, which leads to the battery prepared from the positive electrode particles coated with lithium vanadate at the beginning. The charge and discharge speed is relatively slow in the initial stage. Preferably, the D50 of the lithium-rich manganese-based positive electrode material is 1 to 10 μm. The particle size distribution of the positive electrode material will affect the electrochemical performance of the battery. Generally speaking, the smaller the particle size of the positive electrode material, the larger its specific surface area, and the better the capacity and rate performance of the battery. However, too small a particle size will also increase the internal resistance of the battery, thereby affecting the cycle life of the battery. And too large a particle size will also increase the internal resistance of the battery, thereby affecting the safety performance of the battery. Therefore, the particle size distribution of the positive electrode material needs to be optimized within a certain range to achieve the best electrochemical performance. Controlling the D50 of the lithium-rich manganese-based positive electrode material within the above range is conducive to controlling the final composite positive electrode material to have a more suitable particle size distribution, so that its electrochemical performance is optimized.
[0015] According to a second aspect of the present invention, a method for preparing the above-mentioned lithium-rich manganese-based composite positive electrode material is provided, comprising the following steps: S1. A nickel source solution and a manganese source solution are mixed to obtain a mixed solution, and under a protective atmosphere, a pH regulator and a precipitant solution are added to the mixed solution in a co-liquid manner to carry out a co-precipitation reaction for 40 to 60 hours. During the co-precipitation reaction, the pH of the reaction system is controlled to be 10 to 12 and the temperature is 40 to 70° C.; then the heating is turned off, and aging is continued for 10 to 20 hours, and then filtered, washed, and dried to obtain a lithium-rich manganese-based material precursor; pH The regulator includes at least one of ammonia water and ammonium bicarbonate; the precipitant solution is an alkaline solution; S2. The lithium-rich manganese-based material precursor is mixed and ground with the lithium source, and in an oxidizing atmosphere, the temperature is first raised to 100-500°C and calcined for 1-8 hours, and then the temperature is continued to be raised to 700-1000°C and calcined for 7-20 hours to obtain a lithium-rich manganese-based positive electrode material; S3. After mixing the lithium-rich manganese-based positive electrode material, vanadium source and phosphorus source, the temperature is first raised to 100-300°C and calcined for 1-5 hours, and then the temperature is continued to be raised to 400-700°C and calcined for 1-5 hours to obtain a lithium-rich manganese-based composite positive electrode material.
[0016] In the preparation method provided by the present invention, the lithium-rich manganese-based composite positive electrode material is prepared by first coprecipitation reaction to prepare a lithium-rich manganese-based material precursor, then calcined to prepare a lithium-rich manganese-based positive electrode material, and then added a vanadium source and a phosphorus source for further calcination to obtain it.
[0017] Specifically, first, in the preparation of the lithium-rich manganese-based material precursor in S1, the pH regulator and the precipitant solution together regulate the pH of the reaction system and carry out a coprecipitation reaction. At a specific pH and temperature, the crystals are initially grown, and under further aging, the solution will further react, so that the reaction is relatively complete, which is conducive to the further growth of small-particle crystals, and the already grown crystals can also be ground off the corners by the pH regulators such as ammonia water and ammonium bicarbonate in the solution, making the crystals round and smooth. At the same time, pH regulators such as ammonia water and ammonium bicarbonate can play the role of complexing cations Ni and Mn, which can further promote the integrity of crystal formation and improve the performance of crystal materials. It should also be noted here that after the coprecipitation reaction, it is very necessary to carry out aging for a certain period of time. Since the reaction always tends to proceed in the direction of low energy, after aging for a certain period of time, the Ni(OH)2 precipitation product will be rearranged according to its inherent lattice structure law, showing good crystallization performance, which is conducive to improving the structural stability of the crystal, and then it is conducive to the lithium-rich manganese-based positive electrode material with this as a precursor to show higher electrochemical performance.
[0018] Secondly, in S2, the lithium-rich manganese-based material precursor and the lithium source are calcined through a specific two-stage sintering procedure to form a lithium-rich manganese-based positive electrode material with good crystallinity and high structural stability. First, the first stage of sintering is the process of lithium melting and full fusion with the precursor, and the second stage of sintering is the process of material crystallization. Sintering at low temperature first ensures the full fusion of lithium and the precursor, promotes the overall uniformity of the various elements of the material before subsequent high-temperature sintering, is conducive to high-temperature rapid crystallization and promotes crystal integrity, improves the stability of the particle structure, and optimizes the electrochemical performance of the particles.
[0019] Finally, in S3, the lithium-rich manganese-based positive electrode material is mixed with a vanadium source and a phosphorus source, and then sintered in two stages, first at low temperature and then at high temperature. The low-temperature sintering is to volatilize the moisture in the material to prevent the moisture from increasing the difficulty of calcination and affecting the calcination efficiency. Specifically, moisture will increase the calcination temperature and heat transfer, thereby increasing the difficulty of calcination. Secondly, during the calcination process, the evaporation of moisture in the material will occupy part of the calcination energy, thereby slowing down the calcination rate. Therefore, if the moisture content in the material is too high, direct high-temperature calcination will reduce the calcination efficiency. The subsequent high-temperature sintering is to melt the vanadium source and the phosphorus source to adhere to the surface of the lithium-rich manganese-based positive electrode material, and form a dense, uniform and stable vanadium-phosphorus composite film on the surface of the lithium-rich manganese-based positive electrode material, which is beneficial to improve the overall electrochemical properties of the lithium-rich manganese-based material.
[0020] Preferably, in S1, the concentration of ammonia in the reaction system is controlled to be 0.5-5 mol / L by using ammonia. Controlling the concentration of ammonia within a certain range is conducive to maintaining the pH stability of the reaction system, thereby stabilizing the entire coprecipitation reaction process and obtaining particles with uniform particle size and high lattice stability.
[0021] Preferably, in S1, the nickel source and the manganese source are calculated in the following manner: the molar ratio of Ni / Mn is 0.1 to 1. Generally speaking, when the nickel ratio increases, the capacity of the battery will increase, but the cycle life may decrease; when the manganese ratio increases, the capacity of the battery will decrease and the cycle life will increase. Therefore, a high manganese and low nickel material formula is generally used in the positive electrode of a lithium-rich manganese-based lithium battery to balance the relationship between capacity and cycle life.
[0022] Preferably, in S1, during the coprecipitation reaction, the stirring rate is 300 to 800 rpm; during the aging process, the stirring rate is 100 to 200 rpm. During the coprecipitation reaction, a higher stirring rate is used to facilitate the full mixing of the materials and the full reaction. During the aging process, a lower stirring rate is used to facilitate the further growth of small particle crystals, avoiding excessive stirring rate affecting the further growth of grains, and affecting the crystal stability and electrochemical performance of the positive electrode particles.
[0023] Preferably, in S1, the nickel source includes at least one of nickel sulfate, nickel nitrate and nickel chloride; the manganese source includes at least one of manganese nitrate, manganese sulfate and manganese oxalate; and in the precipitant solution, the precipitant includes at least one of sodium hydroxide and sodium carbonate.
[0024] Preferably, in S1, the protective atmosphere includes at least one of nitrogen and argon.
[0025] Preferably, in S1, the pH of the reaction system is controlled to be 11 and the temperature is controlled to be 60° C. At this pH and temperature, the precipitated product has a single morphology, good sphericity, narrow particle size distribution, and high tap density, which is beneficial to improving the electrochemical performance of the positive electrode material.
[0026] Preferably, in S2, the amount of lithium source is calculated as follows: the molar ratio of Li / (Ni+Mn) is 1.01 to 1.90; the lithium source includes at least one of lithium hydroxide, lithium carbonate, and lithium chloride. As the Li / (Ni+Mn) ratio increases, the tap density of the material decreases, and the discharge gram capacity increases. As the Li / (Ni+Mn) ratio decreases, the tap density of the material increases, and the discharge gram capacity decreases. Therefore, it is necessary to control the Li / (Ni+Mn) ratio within a certain range to take into account the tap density and discharge gram capacity of the material and optimize the overall electrochemical properties of the material.
[0027] Preferably, in S2, the oxidizing atmosphere is at least one of oxygen and air.
[0028] Preferably, in S3, the vanadium source includes at least one of ammonium vanadate, lithium vanadate and vanadium pentoxide; the phosphorus source includes at least one of diammonium phosphate, monoammonium phosphate, iron phosphate and iron pyrophosphate.
[0029] Preferably, in S3, the vanadium source is vanadium pentoxide; and the phosphorus source is ammonium dihydrogen phosphate.
[0030] Preferably, in S3, the feeding amounts of vanadium source and phosphorus source are calculated as follows: the molar ratio of V to P is 0.1-0.9:0.1-0.9, and the total content of V and P in the lithium-rich manganese-based composite positive electrode material is 500-1000 ppm.
[0031] Preferably, in S3, during mixing and grinding, the mixing speed is 1000-5000 r / min, and the mixing time is 30-300 s.
[0032] According to a third aspect of the present invention, a battery is provided, comprising the composite positive electrode material. The battery prepared using the composite positive electrode material has a high first efficiency and first cycle discharge gram capacity, and still has a high capacity retention rate after multiple cycles. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1This is a SEM image of the composite positive electrode material prepared in Example 1 of the present invention, with a magnification of 10kx.
[0034] Figure 2 This is a SEM image of the composite positive electrode material prepared in Example 1 of the present invention, with a magnification of 50kx. DETAILED DESCRIPTION
[0035] In order to enable those skilled in the art to better understand the solutions of the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only embodiments of a part of the present invention, rather than all embodiments.
[0036] Example 1
[0037] 1. Preparation of composite cathode materials
[0038] The composite positive electrode material in this embodiment is prepared according to the following steps:
[0039] S1. Mix nickel sulfate solution and manganese oxalate solution to obtain a mixed solution. Under a nitrogen protective atmosphere, add ammonia water and sodium hydroxide solution to the mixed solution in a co-liquid manner to carry out a coprecipitation reaction for 50 hours. During the coprecipitation reaction, the pH of the reaction system is controlled to be 11±0.2 and the temperature is 60°C. At the same time, the concentration of ammonia water is controlled to be 2 mol / L, and the stirring rate during the coprecipitation reaction is 400 rpm; then turn off the heating, continue aging for 15 hours, and the stirring rate during the aging process is 150 rpm, then filter, wash, and dry to obtain a lithium-rich manganese-based material precursor; wherein, the amount of nickel sulfate and manganese oxalate is calculated based on a Ni / Mn molar ratio of 0.429;
[0040] S2. The lithium-rich manganese-based material precursor was mixed and ground with lithium hydroxide at a mixing speed of 3000 r / min and a mixing time of 150 s. In an oxygen atmosphere, the temperature was first raised to 300°C and calcined for 4 h, and then continued to be raised to 850°C and calcined for 14 h to obtain a lithium-rich manganese-based positive electrode material, which was crushed to a D50 of 5.5 μm; wherein the amount of lithium hydroxide was calculated based on a molar ratio of Li / (Ni+Mn) of 1.4; the chemical formula of the lithium-rich manganese-based positive electrode material is 0.4Li2MnO3·0.6LiNi 0.5 Mn 0.5 O2;
[0041] S3. After mixing the lithium-rich manganese-based positive electrode material, vanadium pentoxide and ammonium dihydrogen phosphate, the temperature is first raised to 200°C and calcined for 3 hours, and then the temperature is continued to be raised to 550°C and calcined for 3 hours to obtain a lithium-rich manganese-based composite positive electrode material, and the vanadium compound in the coating film on the surface of the final lithium-rich manganese-based positive electrode material is lithium vanadate, and the phosphorus compound is phosphorus pentoxide; wherein, the total content of V and P in the lithium-rich manganese-based composite positive electrode material is 800ppm, and the feeding amount of vanadium pentoxide and ammonium dihydrogen phosphate is calculated, and the molar ratio of V to P in vanadium pentoxide and ammonium dihydrogen phosphate is 0.4:0.6.
[0042] like Figure 1 and Figure 2 , are all electron microscope images of the composite positive electrode material prepared in Example 1, where Figure 1 The electron microscope magnification is 10kx. Figure 2 The magnification of the electron microscope in the image is 50kx.
[0043] 2. Preparation of batteries
[0044] The battery of this embodiment is prepared according to the following steps:
[0045] a. Weigh the materials according to the mass ratio of the composite positive electrode material: conductive carbon black (Super P): binder (PVDF) of 93:3:4, use N-methylpyrrolidone (NMP) as solvent, and centrifuge the mixture for 10 minutes to obtain a positive electrode slurry;
[0046] b. The positive electrode slurry was coated on the aluminum foil with a thickness of 160 μm by using a coating machine, dried at 120°C for 3 h, and then rolled once on a double-roll roller with a gap of 0.1 mm. The rolled aluminum foil was then transferred to a vacuum drying oven and dried at 120°C for 12 h to completely remove NMP and residual moisture.
[0047] c. Cut the dried electrode into discs with a diameter of 12 mm as the positive working electrode;
[0048] d. Assembling button cells: Using lithium sheets as negative electrodes, polypropylene diaphragms as diaphragms, and purchased custom electrolytes, assemble CR2032 button cells in a glove box filled with dry argon gas.
[0049] Example 2
[0050] 1. Preparation of composite cathode materials
[0051] When preparing the composite positive electrode material of this embodiment, the difference from that of embodiment 1 is that in S3, the total content of V and P in the lithium-rich manganese-based composite positive electrode material is 350 ppm. The rest is the same as that of embodiment 1.
[0052] 2. Preparation of batteries
[0053] The preparation of the battery of this example is consistent with that of Example 1.
[0054] Example 3
[0055] 1. Preparation of composite cathode materials
[0056] When preparing the composite positive electrode material of this embodiment, the difference from that of embodiment 1 is that in S3, the total content of V and P in the lithium-rich manganese-based composite positive electrode material is 1300 ppm. The rest is the same as that of embodiment 1.
[0057] 2. Preparation of batteries
[0058] The preparation of the battery of this example is consistent with that of Example 1.
[0059] Example 4
[0060] 1. Preparation of composite cathode materials
[0061] When preparing the composite positive electrode material of this embodiment, the difference from that of embodiment 1 is that in S3, the molar ratio of V to P in vanadium pentoxide and ammonium dihydrogen phosphate is 0.1:0.9. The rest is the same as that of embodiment 1.
[0062] 2. Preparation of batteries
[0063] The preparation of the battery of this example is consistent with that of Example 1.
[0064] Example 5
[0065] 1. Preparation of composite cathode materials
[0066] When preparing the composite positive electrode material of this embodiment, the difference from that of embodiment 1 is that in S3, the molar ratio of V to P in vanadium pentoxide and ammonium dihydrogen phosphate is 0.9:0.1. The rest is the same as that of embodiment 1.
[0067] 2. Preparation of batteries
[0068] The preparation of the battery of this example is consistent with that of Example 1.
[0069] Example 6
[0070] 1. Preparation of composite cathode materials
[0071] When preparing the composite positive electrode material of this embodiment, the difference from that of embodiment 1 is that in S3, the vanadium source is lithium vanadate, so that the vanadium compound in the coating film on the surface of the lithium-rich manganese-based positive electrode material is lithium vanadate. The rest is the same as embodiment 1.
[0072] 2. Preparation of batteries
[0073] The preparation of the battery of this example is consistent with that of Example 1.
[0074] Example 7
[0075] 1. Preparation of composite cathode materials
[0076] When preparing the composite positive electrode material of this embodiment, the difference from that of embodiment 1 is that in S3, the phosphorus source is iron phosphate, so that the phosphorus compound in the coating film on the surface of the lithium-rich manganese-based positive electrode material is iron phosphate. The rest is the same as embodiment 1.
[0077] 2. Preparation of batteries
[0078] The preparation of the battery of this example is consistent with that of Example 1.
[0079] Example 8
[0080] 1. Preparation of composite cathode materials
[0081] When preparing the composite positive electrode material of this embodiment, the difference from that of embodiment 1 is that in S3, the phosphorus source is a mixture of pyrophosphate iron, so that the phosphorus compound in the coating film on the surface of the lithium-rich manganese-based positive electrode material is pyrophosphate iron. The rest is the same as embodiment 1.
[0082] 2. Preparation of batteries
[0083] The preparation of the battery of this example is consistent with that of Example 1.
[0084] Example 9
[0085] 1. Preparation of composite cathode materials
[0086] When preparing the composite positive electrode material of this embodiment, the difference from that of embodiment 1 is that in S2, the lithium-rich manganese-based positive electrode material is crushed to a D50 of 1 μm. The rest is the same as that of embodiment 1.
[0087] 2. Preparation of batteries
[0088] The preparation of the battery of this example is consistent with that of Example 1.
[0089] Example 10
[0090] 1. Preparation of composite cathode materials
[0091] When preparing the composite positive electrode material of this embodiment, the difference from that of embodiment 1 is that in S2, the lithium-rich manganese-based positive electrode material is crushed to a D50 of 3.5 μm. The rest is the same as that of embodiment 1.
[0092] 2. Preparation of batteries
[0093] The preparation of the battery of this example is consistent with that of Example 1.
[0094] Embodiment 11
[0095] 1. Preparation of composite cathode materials
[0096] When preparing the composite positive electrode material of this embodiment, the difference from that of embodiment 1 is that in S2, the lithium-rich manganese-based positive electrode material is crushed to a D50 of 10 μm. The rest is the same as that of embodiment 1.
[0097] 2. Preparation of batteries
[0098] The preparation of the battery of this example is consistent with that of Example 1.
[0099] Example 12
[0100] 1. Preparation of composite cathode materials
[0101] When preparing the composite positive electrode material of this embodiment, the difference from that of embodiment 1 is that in S3, the calcination temperature of the first stage is 100° C. The rest is the same as that of embodiment 1.
[0102] 2. Preparation of batteries
[0103] The preparation of the battery of this example is consistent with that of Example 1.
[0104] Comparative Example 1
[0105] 1. Preparation of composite cathode materials
[0106] When preparing the composite positive electrode material of this comparative example, the difference from Example 1 is that only a vanadium source, that is, only 800 ppm of vanadium pentoxide is added to S3, and no diammonium phosphate is added, so that the coating film on the surface of the lithium-rich manganese-based positive electrode material contains only vanadium pentoxide. The rest is the same as Example 1.
[0107] 2. Preparation of batteries
[0108] The preparation of the battery of this comparative example is consistent with that of Example 1.
[0109] Comparative Example 2
[0110] 1. Preparation of composite cathode materials
[0111] When preparing the composite positive electrode material of this comparative example, the difference from Example 1 is that in S3, only a phosphorus source, that is, only 800 ppm of ammonium dihydrogen phosphate is added, and no vanadium pentoxide is added, so that the coating film on the surface of the lithium-rich manganese-based positive electrode material contains only phosphorus pentoxide. The rest is the same as Example 1.
[0112] 2. Preparation of batteries
[0113] The preparation of the battery of this comparative example is consistent with that of Example 1.
[0114] Comparative Example 3
[0115] 1. Preparation of composite cathode materials
[0116] When preparing the composite positive electrode material of this comparative example, the difference from Example 1 is that in S3, vanadium pentoxide is replaced with magnesium oxide, so that the coating film on the surface of the lithium-rich manganese-based positive electrode material is composed of magnesium oxide and phosphorus pentoxide. The rest is the same as Example 1.
[0117] 2. Preparation of batteries
[0118] The preparation of the battery of this comparative example is consistent with that of Example 1.
[0119] Comparative Example 4
[0120] 1. Preparation of composite cathode materials
[0121] When preparing the composite positive electrode material of this comparative example, the difference from Example 1 is that in S3, calcination is performed in one step, that is, calcination is performed directly to 550° C. without calcination in stages. The rest is the same as Example 1.
[0122] 2. Preparation of batteries
[0123] The preparation of the battery of this comparative example is consistent with that of Example 1.
[0124] Test Case
[0125] 1. Experimental Construction Method
[0126] The composite positive electrode materials or batteries prepared in all the above embodiments and comparative examples were subjected to the following performance tests:
[0127] (1) First-effect test:
[0128] After the prepared battery was left to stand for 3 hours, the charge / discharge test was performed on the LAND battery test system, with a voltage range of 2.0 to 4.8 V. The battery's 0.1C charge / discharge specific capacity was recorded, with the first efficiency = discharge specific capacity / charge specific capacity*100%.
[0129] (2) Discharge specific capacity and cycle capacity retention rate test
[0130] After the prepared battery was left to stand for 3 hours, the charge / discharge test was performed on the LAND battery test system with a voltage range of 2.0 to 4.8 V. The discharge specific capacity of the battery at a current of 1C was recorded, and the capacity retention rate of the battery after 50 cycles at a current of 1C was calculated and recorded. The capacity retention rate was calculated as: discharge capacity at the 50th cycle / discharge capacity at the first cycle.
[0131] (3) Determination of battery internal resistance
[0132] Resistance determination: Take the battery before and after the cycle, discharge it to 50% SOC, and measure it on a VMP3 resistance tester with an amplitude of 5mV to 10mV and a frequency of 100mHz-100KHz to obtain the Rct value.
[0133] 2. Experimental results
[0134] The test results of the above-mentioned related properties of the composite positive electrode materials or batteries prepared in all the above-mentioned embodiments and comparative examples are shown in Table 1.
[0135] Table 1 Test results of composite positive electrode materials or battery related performances prepared in the examples and comparative examples
[0136]
[0137]
[0138] As can be seen from Table 1, the lithium-rich manganese-based composite positive electrode material prepared by the present invention is applied to lithium batteries, so that the lithium batteries have higher first efficiency, first-cycle discharge specific capacity and capacity retention rate. At the same time, the internal resistance growth of the lithium battery is relatively low after a certain number of cycles. Please refer to Examples 1 to 12 for details. Therefore, the lithium-rich manganese-based composite positive electrode material of the present invention can effectively improve the electrochemical performance of lithium-rich manganese-based lithium batteries. This is because the present invention coats a layer of vanadium-phosphorus composite film on the surface of the particles of the lithium-rich manganese-based matrix material. The vanadium-phosphorus composite film can effectively protect the lithium-rich manganese-based core and improve the structural stability and conductivity of the positive electrode particles, thereby effectively improving the electrochemical performance of the lithium battery prepared thereby.
[0139] In comparative example 1, only a vanadium source is added to S3, that is, only a vanadium compound (vanadium pentoxide) is contained in the vanadium-phosphorus composite film. This will result in a higher residual alkali content on the surface of the material, increased internal resistance, and reduced cycle stability. Therefore, the first efficiency, first-cycle discharge capacity, and capacity retention rate of the battery are significantly reduced. At the same time, the internal resistance of the battery before and after the cycle is relatively large.
[0140] In Comparative Example 2, only a phosphorus source is added to S3, that is, only a phosphorus compound (phosphorus pentoxide) is contained in the vanadium-phosphorus composite film. The absence of a vanadium compound causes serious mixing of Li and Ni in the positive electrode material after several charge and discharge cycles of lithium ions and deintercalation, and the material cycle performance deteriorates. This also leads to a significant decrease in the first efficiency, first-cycle discharge specific capacity, and capacity retention rate of the battery. At the same time, the internal resistance of the battery before and after the cycle is relatively large.
[0141] In Comparative Example 3, vanadium pentoxide is replaced with magnesium oxide in S3, which makes the material's cycle performance also deteriorate, resulting in a decrease in various battery performances. This is because the coatings formed by different materials have different modification effects. Compared with the vanadium-phosphorus composite film coating, the coating formed by magnesium oxide and phosphorus pentoxide has no obvious effect on reducing lithium-nickel mixing and improving the stability of lithium-rich manganese-based materials, which leads to a deterioration in the electrochemical performance of the material, and then leads to a decrease in various electrochemical performances of the battery.
[0142] Comparative Example 4 directly calcined in one step in S3, that is, directly calcined to 550°C without calcining in stages, so the performance of the obtained material will also decline, resulting in a decline in various performances of the battery. This is because direct one-step calcination will cause the moisture in the material to not evaporate in time, and side reactions will occur when the temperature rises, resulting in a low Li content in the material and a decline in electrical properties, which will affect the performance of the material. At the same time, it will also cause water molecules to escape from the material when the temperature rises, leaving gaps and not dense, and the overall energy density of the material will decrease. In addition, direct high-temperature calcination is also likely to cause cracking of the material, which is not conducive to improving the stability of the material, and finally leads to a decline in various performances of the battery.
[0143] Further comparing Example 1 with Examples 2-3, the total content of V and P in the lithium-rich manganese-based composite positive electrode material in Examples 2 and 3 is too much and too little respectively. If the total content of V and P is too little, the residual alkali on the surface of the material will increase and the internal resistance will increase during the cycle; and if the total content of V and P is too much, the coating layer will be too thick, affecting the lithium ion transmission and resulting in a decrease in the discharge capacity. Because of these factors, the initial efficiency and capacity retention rate of the battery are ultimately reduced compared to Example 1.
[0144] Comparing Example 1 with Examples 4 and 5, compared with Example 1, the proportion of V in the vanadium-phosphorus composite film in Example 4 is relatively small, and the proportion of P in the vanadium-phosphorus composite film in Example 4 is relatively small in Example 5, which leads to that the various performance indicators of the battery are worse than those of the examples. This is because if V is less, the mixed cycle performance of Li and Ni becomes worse; if P is less, the overall residual alkali of the material is high, resulting in increased internal resistance and decreased cycle performance. Therefore, it is mainly necessary to control V and P within a specific range to ensure that the performance of the material is better, which is more conducive to the various performances of the battery.
[0145] Comparing Example 1 with Examples 6 to 8, it can be found that when the type of vanadium source or phosphorus source is changed, the performance of the battery will also be affected. This is because there is a certain interaction between different materials, and certain changes will occur during the high-temperature calcination process. At the same time, different materials have different modification effects on the lithium-rich manganese-based core, so the final performance of the battery is also different. And from the above-mentioned embodiments, it can be seen that when the vanadium source is vanadium pentoxide and the phosphorus source is diammonium phosphate, it is more conducive to the optimization of the performance of the lithium-rich manganese-based material, and the performance of the battery is further optimized.
[0146] By comparing Example 1 with Examples 9 to 11, it can be found that the particle size of the lithium-rich manganese-based positive electrode material (kernel) will also affect the material properties and thus the performance of the battery. For example, compared with Example 1, the D50 of the lithium-rich manganese-based positive electrode material (kernel) in Example 9 is smaller, so the D50 of the composite positive electrode material is also smaller, and it is easy to mix and agglomerate, resulting in a decrease in discharge capacity. The D50 of the lithium-rich manganese-based positive electrode material (kernel) in Example 11 is larger, so the D50 of the composite positive electrode material is also larger, but the specific surface area is smaller, and the contact area between particles is reduced, resulting in a decrease in the efficiency of electron and ion transmission, thereby resulting in a decrease in battery capacity and a decrease in cycle life. Therefore, the smaller or larger the particle size of the lithium-rich manganese-based positive electrode material (kernel), the performance effect of optimizing the material will decrease, resulting in a relatively poor modification effect on the battery.
[0147] Comparing Example 1 and Example 12, in Example 12, the calcination temperature of the first stage in S3 is relatively low, so there will be residual moisture in the material like in Comparative Example 2, but the moisture will be less than that in Comparative Example 2. In this case, the residual moisture will also cause side reactions when the temperature rises, resulting in a decrease in the Li content of the material, a decrease in electrical performance, and a decrease in the overall energy density of the material, which ultimately leads to a decrease in battery performance.
[0148] The above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit the protection scope of the present invention. Although the present invention is described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that the technical solutions of the present invention can be modified or equivalently replaced, but these modifications or replacements are all within the protection scope of the present invention.
Claims
1. A lithium-rich manganese-based composite positive electrode material, characterized in that: The invention comprises a core and a coating layer coated on the surface of the core, wherein the core comprises a lithium-rich manganese-based positive electrode material with a chemical structural formula of xLi2MnO3·(1-x)LiNi 0.5 Mn 0.5 O2, the value of x is 0.1 to 0.95; The coating layer includes a vanadium compound and a phosphorus compound; The vanadium compound includes at least one of vanadium pentoxide and lithium vanadate; The phosphorus compound includes at least one of phosphorus pentoxide, iron phosphate and iron pyrophosphate.
2. The lithium-rich manganese-based composite positive electrode material according to claim 1, characterized in that: The total content of V and P in the lithium-rich manganese-based composite positive electrode material is 500-1000 ppm.
3. The lithium-rich manganese-based composite positive electrode material according to claim 2, characterized in that: In the coating layer, the molar ratio of V to P is 0.1-0.9:0.1-0.
9.
4. The lithium-rich manganese-based composite positive electrode material according to claim 1, characterized in that: In the coating layer, the vanadium compound is vanadium pentoxide, and the phosphorus compound is phosphorus pentoxide.
5. The lithium-rich manganese-based composite positive electrode material according to claim 1, characterized in that: The D50 of the lithium-rich manganese-based positive electrode material is 1 to 10 μm.
6. A method for preparing the lithium-rich manganese-based composite positive electrode material according to any one of claims 1 to 5, characterized in that: The steps include: S1. Mixing a nickel source solution and a manganese source solution to obtain a mixed solution, adding a pH regulator and a precipitant solution to the mixed solution in a co-liquid manner under a protective atmosphere for a co-precipitation reaction for 40 to 60 hours, wherein during the co-precipitation reaction, the pH of the reaction system is controlled to be 10 to 12 and the temperature is controlled to be 40 to 70° C.; then turning off the heating, continuing aging for 10 to 20 hours, and then filtering, washing, and drying to obtain a lithium-rich manganese-based material precursor; the pH regulator comprises at least one of ammonia water and ammonium bicarbonate; the precipitant solution is an alkaline solution; S2. The lithium-rich manganese-based material precursor is mixed with a lithium source and ground, and the mixture is first heated to 100 to 500 ° C and calcined for 1 to 8 hours in an oxidizing atmosphere, and then further heated to 700 to 1000 ° C and calcined for 7 to 20 hours to obtain the lithium-rich manganese-based positive electrode material; S3. After mixing the lithium-rich manganese-based positive electrode material, vanadium source and phosphorus source, first heat it to 100-300° C. and calcine it for 1-5 hours, and then continue to heat it to 400-700° C. and calcine it for 1-5 hours to obtain the lithium-rich manganese-based composite positive electrode material.
7. The method for preparing the lithium-rich manganese-based composite positive electrode material according to claim 6, characterized in that: In S1, the ammonia water is also used to control the ammonia water concentration in the reaction system to be 0.5-5 mol / L.
8. The method for preparing the lithium-rich manganese-based composite positive electrode material according to claim 6, characterized in that: In S1, the feeding amounts of the nickel source and the manganese source are calculated as follows: the molar ratio of Ni / Mn is 0.1 to 1; In S2, the amount of the lithium source is calculated as follows: the molar ratio of Li / (Ni+Mn) is 1.01 to 1.
90.
9. The method for preparing the lithium-rich manganese-based composite positive electrode material according to claim 6, characterized in that: The vanadium source includes at least one of ammonium vanadate, lithium vanadate and vanadium pentoxide; The phosphorus source includes at least one of diammonium phosphate, monoammonium phosphate, iron phosphate, and iron pyrophosphate.
10. A battery, characterized in that: It comprises the lithium-rich manganese-based composite positive electrode material as claimed in any one of claims 1 to 5.
Citation Information
Cited By
Composite lithium supplement agent and preparation method and application thereof
CN119921006A