Positive electrode material and preparation method thereof, secondary battery and terminal equipment

By optimizing the particle size distribution and sintering process of the cathode material, a nickel-cobalt-manganese ternary cathode material with high voltage resistance and high crystallinity is formed, which solves the problem that the cathode material of the lithium-ion battery is prone to cracking under high pressure and improves the energy of the battery. Density and security.

CN118738378APending Publication Date: 2024-10-01HUAWEI TECH CO LTD +1
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202310541316.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2023-05-12
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing lithium-ion battery cathode materials are prone to cracks and crushing under high compaction densities, leading to increased side reactions with the electrolyte and affecting cycle performance and safety.

Method used

By limiting the area relationship of the particle size distribution diagram of the cathode material before and after pressure, the pressure resistance performance of the particles is optimized. A nickel-cobalt-manganese ternary cathode material with high crystallinity and uniform particle size dispersion is used, and through segmented sintering The process forms single crystal or single crystal-like particles.

Benefits of technology

It improves the voltage resistance and compaction density of the cathode material, reduces side reactions with the electrolyte, and improves the cycle performance and safety performance of lithium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118738378A_ABST
    Figure CN118738378A_ABST
Patent Text Reader

Abstract

The invention provides a positive electrode material and a preparation method thereof, a secondary battery and terminal equipment. The area of a first particle size distribution diagram of the positive electrode material before being pressed is S0, the area of a second particle size distribution diagram of the positive electrode material after being pressed by 4t is S (4t), the area of an overlapped area of the first particle size distribution diagram and the second particle size distribution diagram is S (4t), and the area of the second particle size distribution diagram of the positive electrode material after being pressed by 8t is S (8t). The area of the overlapped region of the first particle size distribution diagram and the second particle size distribution diagram is S (8t); s1 (4t) is equal to S (4t)-S (4t), and S2 (4t) is equal to S0-S (4t); s1 (8t) is equal to S (8t)-S (8t), and S2 (8t) is equal to S0-S (8t); wherein S1 (8t) / S1 (4t) is less than or equal to 1.2, and S2 (8t) / S2 (4t) is less than or equal to 1.3.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims the priority of the Chinese patent application filed with the China Patent Office on March 30, 2023, with application number 202310361930.9 and application name “Positive electrode material and preparation method thereof, secondary battery and terminal device”, the entire contents of which are incorporated by reference in this application. Technical Field

[0003] The present application relates to the field of batteries, and in particular to a positive electrode material and a preparation method thereof, a secondary battery and a terminal device. Background Art

[0004] With the rapid growth of mobile terminal devices and electric vehicle applications, the requirements for the energy density, charge and discharge rate, and safety performance of lithium-ion batteries are increasing. In order to improve the energy density of lithium-ion batteries, it is usually necessary to increase the compaction density of the positive electrode material to increase the filling amount of the positive electrode material per unit volume. Since the existing positive electrode material particles have poor pressure resistance, when a high compaction force is applied to the positive electrode material, the particles of the positive electrode material will inevitably crack or even crush. The fractured positive electrode material is more likely to produce side reactions with the electrolyte during the charge and discharge process, thereby affecting the cycle performance and safety of the lithium-ion battery. Summary of the invention

[0005] The present application provides a positive electrode material and a preparation method thereof, a secondary battery and a terminal device. The positive electrode material particles of the present application have high pressure resistance to improve the cycle performance and safety performance of the lithium-ion battery.

[0006] In a first aspect, the present application provides a positive electrode material, wherein the area of ​​a first particle size distribution diagram of the positive electrode material before being pressed is S0, and the area of ​​a second particle size distribution diagram of the positive electrode material after being subjected to 4 tons of pressure is S (4t) , the area of ​​the overlap between the first particle size distribution diagram and the second particle size distribution diagram is ΔS (4t ), the area of ​​the third particle size distribution diagram of the positive electrode material after being subjected to 8 tons of pressure is S (8t) The area of ​​the overlap between the first particle size distribution diagram and the third particle size distribution diagram is ΔS (8t) ;

[0007] S 1(4t) =S (4t) -△S (4t) , S 2(4t) =S0-△S (4t) ; S 1(8t) =S (8t) -△S (8t) , S 2(8t)=S0-△S (8t) ;

[0008] Among them, S 1(8t) / S 1(4t) ≤1.2, S 2(8t) / S 2(4t) ≤1.3.

[0009] The positive electrode material of the present application can obtain a positive electrode material with better pressure resistance by limiting the relationship between the area of ​​the particle size distribution diagram of the positive electrode material before being compressed, after being compressed by 4 tons of pressure (abbreviated as 4t) and after being compressed by 8 tons of pressure (abbreviated as 8t). Among them, after the particles of the positive electrode material are ruptured by pressure, the particle size distribution diagram will shift in the direction of smaller particle size. 1(4t) It can be used to represent the area change value of the non-overlapping area of ​​the particle size distribution diagram of the positive electrode material particles before and after being subjected to 4t pressure, S 1(8t) It can be used to represent the area change value of the non-overlapping area of ​​the particle size distribution diagram of the positive electrode material particles before and after being subjected to pressure, S 1(8t) / S 1(4t) It can be used to characterize the relationship between the second particle size distribution of the positive electrode material particles relative to the 4t pressure and the non-overlapping area of ​​the second particle size distribution and the third particle size distribution after 8t pressure. The smaller the ratio, the better the pressure resistance of the positive electrode particles. After being subjected to 8t pressure, there is no obvious difference between the curve after being subjected to 4t pressure. Similarly, S 2(4t) It can be used to represent the area change value of the non-overlapping area of ​​the particle size distribution diagram of the positive electrode material particles before and after being subjected to 4t pressure, S 2(8t) It can be used to represent the area change value of the non-overlapping area of ​​the particle size distribution diagram of the positive electrode material particles before and after being subjected to pressure, S 2(8t) / S 2(4t) It can be used to characterize the ratio of the non-overlapping area between the first particle size distribution diagram before the positive electrode material particles are subjected to pressure, the second particle size distribution diagram after 4t pressure, and the third particle size distribution diagram after 8t pressure and the first particle size distribution diagram. The smaller the ratio, the better the pressure resistance of the positive electrode particles. After being subjected to 4t pressure and 8t pressure respectively, the smaller the change of the second particle size distribution diagram and the third particle size distribution diagram relative to the first particle size distribution diagram, the higher the particle stability of the positive electrode material. When a secondary battery is prepared with a positive electrode material having this performance, since the positive electrode material of the present application has a higher pressure resistance, the compaction density of the positive electrode material can be increased, and the energy density of the secondary battery can be increased. The positive electrode material of the present application, due to its better pressure resistance, can keep the particles of the positive electrode material at a higher integrity when subjected to higher pressure strength, thereby reducing the side reactions between the positive electrode material and the electrolyte, thereby improving the cycle performance and safety performance of the secondary battery.

[0010] In an optional implementation, S 1(8t) / S 1(4t) ≤1.1, S 2(8t) / S 2(4t) ≤1.2. When S 1(8t) / S 1(4t) ≤1.1, S 2(8t) / S 2(4t) When ≤1.2, it means that the particle size distribution of the positive electrode material particles changes less before and after compression. The particle size distribution diagram after compression has a higher degree of overlap than the particle size distribution diagram before compression, indicating that the particles of the positive electrode material are almost not damaged before and after compression, and a positive electrode material with higher pressure resistance can be further obtained.

[0011] In an optional implementation, the specific surface area of ​​the positive electrode material before being pressed is B0, and the specific surface area of ​​the positive electrode material after being pressed by 4 tons is B (4t) The specific surface area of ​​the positive electrode material after being subjected to 8 tons of pressure is B (8t) Among them, B (8t) / B (4t) ≤1.26, B (8t) / B0≤1.56; preferably, B (8t) / B (4t) ≤1.23, B (8t) / B0≤1.51. If the particles of the positive electrode material rupture during compression, the total specific surface area of ​​the particles of the positive electrode material will increase after compression. (8t) / B (4t) ≤1.26, B (8t) / B0≤1.56; preferably, B (8t) / B (4t) ≤1.23, B (8t) When / B0≤1.51, it means that the particles of the positive electrode material are not damaged much after being compressed, and the specific surface area hardly increases, which proves that the positive electrode material has better pressure resistance. By limiting the ratio between the specific surface area of ​​the positive electrode material before being compressed, the specific surface area after being subjected to 4 tons of pressure and 8 tons of pressure, a positive electrode material with higher pressure resistance can be further obtained.

[0012] In an optional implementation, the particle crystallinity of the positive electrode material is 78% to 95%. The positive electrode material particles with such crystallinity have high resistance to compression fracturing, and when used in secondary batteries, can effectively maintain the integrity of the particles, reduce the occurrence of side reactions, and improve the cycle stability and safety performance of the secondary battery.

[0013] In a second aspect, the present application provides a positive electrode material, wherein the particle crystallinity of the positive electrode material is 78% to 95%, and the particle size dispersion coefficient K of the positive electrode material satisfies 1.050≤K≤1.150, wherein:

[0014] K=K 90 (V) / K 90 (N);

[0015] K 90 (V)=[D 90 (V)-D 10 (V)] / D 50 (V);

[0016] K 90 (N)=[D 90 (N)-D 10 (N)] / D 50 (N);

[0017] K 90 (V) value range 0.800≤K 90 (V)≤1.600, preferably, 1.000≤K 90 (V)≤1.400.

[0018] D 90 (V) is the particle size corresponding to when the cumulative particle size volume distribution of the positive electrode material particles reaches 90%;

[0019] D 10 (V) is the particle size corresponding to the cumulative particle size volume distribution of the positive electrode material particles reaching 10%;

[0020] D 50 (V) is the particle size corresponding to when the cumulative particle size volume distribution of the positive electrode material particles reaches 50%;

[0021] D 90 (N) is the particle size corresponding to when the cumulative particle size distribution of the positive electrode material particles reaches 90%;

[0022] D 10 (N) is the particle size corresponding to when the cumulative particle size distribution of the positive electrode material particles reaches 10%;

[0023] D 50 (N) is the particle size corresponding to when the cumulative particle size number distribution of the positive electrode material particles reaches 50%.

[0024] The positive electrode material of the present application has a high crystallinity. And the particle size dispersion coefficient K of the positive electrode material, i.e. K 90 (V) / K 90(N) satisfies 1.050≤K≤1.150, indicating that the particle size volume distribution of the positive electrode material is relatively close to the particle size number distribution, and the particle size number distribution is narrower, indicating that the particle size dispersion of the positive electrode material is good and the particle size is more uniform. Therefore, the positive electrode material of the present application has uniform particles and high grain integrity, and can obtain good pressure resistance performance.

[0025] In a third aspect, the present application provides a method for preparing the positive electrode material of the present application, the preparation method comprising:

[0026] A mixture of a nickel-cobalt-manganese precursor, a lithium source and an oxide having a doping element is sintered, and the positive electrode material is obtained after cooling; wherein the sintering process comprises:

[0027] S1. Heat from room temperature to T0 within t0 at a heating rate of 1.0-3.0℃ / min; t0≤2.8h, 455℃≤T0≤465℃;

[0028] S2, heating from T0 to T1 at a heating rate of 1.0-3.0℃ / min at time t1, and keeping warm for t2; t1≤2.33h, 465℃≤T1≤500℃ and T1>T0, t2≤4h;

[0029] S3, heating from T1 to T2 at a heating rate of 1.0-3.0℃ / min at time t3, and keeping warm for t4; t3≤3h, 500℃≤T2≤800℃ and T2>T1, t4≤10h;

[0030] S4. Raise the temperature from T2 to T3 at a heating rate of 1.0-3.0°C / min at time t5, and keep warm for t6; t5≤3h, 700°C≤T3≤1000°C and T3>T2, 6h≤t6≤16h.

[0031] The above-mentioned sintering process is a crystallization nucleation process in which solid and liquid phases coexist. During the sintering process, the lithium source material decomposes and melts, and the melted lithium source material reacts on the surface of the oxide particles and inside the oxide particles to form a plurality of tiny primary particles, and then at each different temperature stage, a plurality of tiny primary particles can form secondary particles and fuse and grow inside the secondary particles, and the secondary particles can fuse and grow to form single crystal particles; then at a specific temperature, as the reaction time continues to increase, the single crystal particles can gradually grow to form single crystals. In the sintering process of the present application, the heating rate and the sintering temperature and holding time at different stages are controlled in sections to obtain a positive electrode material with uniform size and single crystal morphology. The positive electrode material obtained by this method can have higher voltage resistance.

[0032] In an optional implementation, the T1 satisfies: 470°C ≤ T1 ≤ 490°C. In an optional implementation, the T2 and the T3 satisfy: T3-T2 ≥ 50°C, 650°C ≤ T2 ≤ 800°C, 750°C ≤ T3 ≤ 900°C. In an optional implementation, the t1 satisfies 1.5h ≤ t1 ≤ 3.5h, the t2 satisfies 4h ≤ t2 ≤ 8h, and the t3 satisfies 7h ≤ t3 ≤ 14h. In an optional implementation, the molar ratio of the lithium source to the nickel-cobalt-manganese precursor is 1.0 to 1.1:1. By optimizing the process parameters at different stages of the sintering process, the voltage resistance of the positive electrode material can be further improved.

[0033] In a fourth aspect, the present application provides a secondary battery, which comprises a positive electrode sheet, a separator, an electrolyte and a negative electrode sheet, wherein the positive electrode sheet comprises the positive electrode material of the present application.

[0034] In a fifth aspect, the present application provides a terminal device, which includes the secondary battery of the present application.

[0035] In addition to secondary batteries, terminal devices may also include power-consuming components or power supply components. Among them, terminal devices include but are not limited to mobile phones, watches, computers, electric vehicles, energy storage devices, etc. Taking mobile phones as an example, terminal devices may include power-consuming components such as chips and display screens in addition to secondary batteries. Taking energy storage devices as an example, terminal devices may include power supply components such as grid connection components or solar cells in addition to secondary batteries.

[0036] Among them, the data in the above-mentioned possible implementation methods of the present application, such as the ratio of the integrated areas of each particle size distribution diagram, the sintering temperature at each stage of the sintering process, the insulation time and other data, when measured, the values ​​within the engineering measurement error range should be understood to be within the range specified in the present application.

[0037] The technical effects that can be achieved in the fourth and fifth aspects mentioned above can be described with reference to the corresponding effects in the first aspect mentioned above, and will not be repeated here. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 A schematic diagram of the temperature rise process of the sintering process of an embodiment;

[0039] Figure 2 This is the SEM electron microscope photo of Example 1;

[0040] Figure 3 The particle size distribution diagram of the sample in Example 1 after the original particle size and the 4t and 8t pressure resistance tests;

[0041] Figure 4 This is the SEM electron microscope photo of Comparative Example 1;

[0042] Figure 5 The particle size distribution diagram of the sample of comparative example 1 after the original particle size and the 4t and 8t pressure resistance tests;

[0043] Figure 6 The following are the cycle comparison data of the sample batteries corresponding to Comparative Example 1 and Example 1. DETAILED DESCRIPTION

[0044] In order to make the objectives, technical solutions and advantages of the present application clearer, the present application will be further described in detail below in conjunction with the accompanying drawings.

[0045] The terms used in the following embodiments are only for the purpose of describing specific embodiments and are not intended to be limiting of the present application. As used in the specification and appended claims of the present application, the singular expressions "a", "an", "above", "the" and "this" are intended to also include expressions such as "one or more", unless there is a clear contrary indication in the context.

[0046] References to "one embodiment" or "some embodiments" etc. described in this specification mean that a particular feature, structure or characteristic described in conjunction with the embodiment is included in one or more embodiments of the present application. Thus, the phrases "in one embodiment", "in some embodiments", "in some other embodiments", "in some other embodiments", etc. that appear at different places in this specification do not necessarily refer to the same embodiment, but mean "one or more but not all embodiments", unless otherwise specifically emphasized in other ways. The terms "including", "comprising", "having" and their variations all mean "including but not limited to", unless otherwise specifically emphasized in other ways.

[0047] The positive electrode material of secondary batteries plays a decisive role in the performance of secondary batteries. The positive electrode materials of lithium-ion batteries include lithium iron phosphate, lithium iron manganese, lithium cobalt oxide, nickel-cobalt-manganese ternary materials, etc. Among them, nickel-cobalt-manganese ternary materials have the advantage of high specific capacity, and as the nickel content in the ternary materials increases, the battery energy density increases, but the stability and cycle performance also decrease accordingly. Through research, it is found that the existing ternary high-nickel materials have poor pressure bearing performance and often have the problem of fracturing under high compaction density. Therefore, how to improve the anti-fracture performance of ternary high-nickel materials to improve their stability and cycle performance has attracted widespread attention.

[0048] An embodiment of the present application provides a positive electrode material. The positive electrode material may be a high-nickel ternary positive electrode material. The particle size distribution diagram of the positive electrode material before being compressed is a first particle size distribution diagram. After the positive electrode material is subjected to a pressure of 4 tons (abbreviated as 4t), its particle size distribution diagram is a second particle size distribution diagram. After the positive electrode material is subjected to a pressure of 8 tons (abbreviated as 8t), its particle size distribution diagram is a third particle size distribution diagram. Integrate the various particle size distribution diagrams of the positive electrode material before and after being compressed to obtain the areas of different particle size distribution diagrams. Among them, the area obtained by integrating the first particle size distribution diagram is recorded as S0. The area obtained by integrating the second particle size distribution diagram is recorded as S (4t) The area obtained by integrating the third particle size distribution graph is recorded as S (8t) The area obtained by integrating the overlapping area of ​​the first particle size distribution graph and the second particle size distribution graph is recorded as △S (4t) The area obtained by integrating the overlapping area of ​​the first particle size distribution graph and the third particle size distribution graph is recorded as △S (8t) Among them, S1 (4t) =S (4t) -△S (4t) , S 2(4t) =S0-△S (4t) , S 1(8t) =S (8t) -△S (8t) , S 2(8t) =S0-△S (8t) ; S 1(4t) / S 1(8t) ≤1.2, S 2(4t) / S 2(8t) ≤1.3. Preferably, S 1(4t) / S 1(8t) ≤1.1, S 2(4t) / S 2(8t) ≤1.2.

[0049] When the positive electrode material satisfies the above relationship after being subjected to 4t and 8t pressure, it can have higher pressure resistance. When the positive electrode material that satisfies the above characteristics is used in a secondary battery, the secondary battery can have higher compaction density, cycle life and safety performance.

[0050] As an example, S 1(4t) / S 1(8t) The value of may be 1.2, 1.15, 1.10, 1.05, 1.0, 0.95, 0.90, 0.85, 0.80 or a lower value, or other values ​​within the range of any two of the above values, which shall be understood to be within the scope defined in the present application. 2(4t) / S 2(8t)The value of may be 1.30, 1.25, 1.2, 1.15, 1.10, 1.05, 1.0, 0.95, 0.90, 0.85, 0.80 or a lower value, or other values ​​within the range of any two of the above values, all of which should be understood to be within the range defined in the present application.

[0051] Among them, as an embodiment, the positive electrode material that meets the above characteristics can be a single crystal material, and its crystallinity can be 78% to 95%. Unlike the secondary granular agglomerate positive electrode material formed by the aggregation of a large number of primary particles, the positive electrode material of the present application has a higher crystallinity of particles and can form a positive electrode material similar to a single crystal or a quasi-single crystal. The positive electrode material with this crystallinity has higher particle stability, can withstand higher pressure in the process of making the electrode, can achieve a higher compaction density, and helps to improve the battery energy density.

[0052] In further research, it was found that the reasonable design of the change in the specific surface area of ​​the positive electrode material before and after compression can help further improve the pressure resistance of the positive electrode material. Among them, the specific surface area of ​​the positive electrode material before compression is B0, and the specific surface area of ​​the positive electrode material after 4t pressure is B0. (4t) The specific surface area of ​​the positive electrode material after being subjected to 8t pressure is B (8t) B0, B (4t) and B (8t) Can meet: B (8t) / B (4t) ≤1.26, B (8t) / B (0) ≤1.56. Preferably, B (8t) / B (4t) ≤1.23, B (8t) / B (0) ≤1.51.

[0053] As an example, B (8t) / B (4t) The value of may be 1.26, 1.25, 1.24, 1.23, 1.21, 1.20 or a lower value, or other values ​​within the range of any two of the above values, which shall be understood to be within the range defined in the present application. (8t) / B (0) The value of may be 1.56, 1.54, 1.53, 1.52, 1.51, 1.50, 1.49, 1.48, 1.47, 1.46 or a lower value, or other values ​​within the range of any two of the above values, all of which should be understood to be within the range defined in the present application.

[0054] As an exemplary illustration, the cathode material of the embodiment of the present application may be a high-nickel ternary cathode material, and its chemical formula may be Li 1+a Ni x Co yMn z M m M′ n O2, wherein -0.5≤a≤0.4, 0.8≤x<1, 0≤y<1, 0≤z<1, 0≤m≤0.1, 0≤n≤0.1, 0.05≤m+n≤0.1, m and n are not 0 at the same time, x+y+z+m+n=1; M and M′ are respectively selected from at least one element of Al, Y, Ti, Zr, V, Nb, Ta, Cr, Mo, W, La, Ce, Er, Mg, Sr, Ba and B. The high nickel ternary positive electrode material may include one doping element, two doping elements, or three or more doping elements.

[0055] The molar ratio of the lithium source to the nickel-cobalt-manganese precursor is 1.0 to 1.1:1, preferably 1.02 to 1.06:1. An appropriate excess of lithium helps to reduce the mixing of lithium and nickel, and helps to form a positive electrode material with a low mixing degree and a good layered structure. However, if the lithium is too much, it is easy to cause the residual alkali in the positive electrode material to be high, which reduces the electrical performance of the positive electrode material.

[0056] In addition, the positive electrode material of the present application has a particle crystallinity of 78% to 95%, and the particle size dispersion coefficient K of the positive electrode material satisfies 1.050≤K≤1.150.

[0057] K=K 90 (V) / K 90 (N);

[0058] K 90 (V)=[D 90 (V)-D 10 (V)] / D 50 (V);

[0059] K 90 (N)=[D 90 (N)-D 10 (N)] / D 50 (N);

[0060] K 90 (V) value range 0.800≤K 90 (V)≤1.600, preferably, 1.000≤K 90 (V)≤1.400;

[0061] D 90 (V) is the particle size corresponding to when the cumulative particle size volume distribution of the positive electrode material particles reaches 90%;

[0062] D 10 (V) is the particle size corresponding to the cumulative particle size volume distribution of the positive electrode material particles reaching 10%;

[0063] D 50 (V) is the particle size corresponding to when the cumulative particle size volume distribution of the positive electrode material particles reaches 50%;

[0064] D 90 (N) is the particle size corresponding to when the cumulative particle size distribution of the positive electrode material particles reaches 90%;

[0065] D 10 (N) is the particle size corresponding to when the cumulative particle size distribution of the positive electrode material particles reaches 10%;

[0066] D 50 (N) is the particle size corresponding to when the cumulative particle size number distribution of the positive electrode material particles reaches 50%.

[0067] The positive electrode material of the embodiment of the present application has a high crystallinity. And the particle size dispersion coefficient K of the positive electrode material, that is, K 90 (V) / K 90 (N) satisfies 1.050≤K≤1.150, wherein K is typically but not limited to 1.050, 1.055, 1.060, 1.070, 1.080, 1.090, 1.100, 1.110, 1.120, 1.130, 1.140 or 1.150 or a value between any two of the above values.

[0068] When the particle size dispersion coefficient K is taken from the above range, it means that the particle size volume distribution of the positive electrode material is relatively close to the particle size number distribution, and the particle size number distribution is narrower, which means that the particle size dispersion of the positive electrode material is good and the particle size is more uniform. Therefore, the positive electrode material of the present application has uniform particles and high grain integrity, and can obtain good pressure resistance performance.

[0069] The method for preparing a high-nickel ternary positive electrode material may include the following steps: sintering a mixture of a nickel-cobalt-manganese precursor, a lithium source and an oxide containing a doping element, and cooling to obtain the positive electrode material. The nickel-cobalt-manganese precursor may include some doping elements.

[0070] As an exemplary illustration, in an optional embodiment, the preparation method of the nickel-cobalt-manganese precursor includes: dissolving nickel, cobalt, manganese and a salt solution of a doping element to obtain a 1-3 mol / L mixed salt solution; dissolving sodium hydroxide into an alkaline solution with a concentration of 4-10 mol / L; dissolving ammonia water into a complexing agent solution with a concentration of 2-10 mol / L. The mixed salt solution, alkaline solution and complexing agent solution are added to the reactor in parallel to react, and stirring is maintained during the process. At the same time, the pH value and reaction temperature of the solution are controlled during the reaction. After solid-liquid separation, washing, drying and screening of the obtained positive electrode precursor slurry, a spherical nickel-cobalt-manganese hydroxide Ni containing doping elements is obtained.x Co y Mn z M m M′ n (OH)2 precursor. Wherein, m and n can be zero at the same time. When m and n are both zero, a nickel-cobalt-manganese precursor without any doping element can be obtained. When m and n are not zero at the same time, a nickel-cobalt-manganese precursor with at least one doping element can be obtained.

[0071] The lithium source may be hydrated lithium hydroxide, or a mixed lithium source of hydrated lithium hydroxide and a lithium salt such as lithium nitrate or lithium carbonate. In one embodiment of the present application, hydrated lithium hydroxide is selected as the lithium source material.

[0072] The oxide containing the doping element may be, for example, an oxide containing M, an oxide containing M', or an oxide containing both M and M'. When the precursor and the oxide contain both M and M', the ratio of the total content of M and M' to Li, Ni, Co, and Mn must satisfy the chemical formula: Li 1+a Ni x Co y Mn z M m M′ n O2.

[0073] The nickel-cobalt-manganese precursor, the lithium source and the oxide containing the doping element are uniformly mixed and then sintered in an oxygen atmosphere. Figure 1 FIG. 1 is a schematic diagram of the heating process of the sintering process of an embodiment. Figure 1 As shown, the sintering process may include the following steps:

[0074] S11, heating from room temperature to T0 within t0 at a heating rate of 1.0-3.0°C / min; t0≤2.8h, 455°C≤T0≤465°C;

[0075] S12, heating from T0 to T1 at a heating rate of 1.0-3.0°C / min at time t1, and keeping warm for t2; t1≤2.33h, 465°C≤T1≤500°C and T1>T0, t2≤4h;

[0076] S13, heating from T1 to T2 at a heating rate of 1.0-3.0°C / min at time t3, and keeping warm for t4; t3≤3h, 500°C≤T2≤800°C and T2>T1, t4≤10h;

[0077] S14, heating from T2 to T3 at time t5 at a heating rate of 1.0-3.0°C / min, and keeping warm for t6; t5≤3h, 700°C≤T3≤1000°C and T3>T2, 6h≤t6≤16h.

[0078] Among them, the hydrated lithium hydroxide and the nickel-cobalt-manganese precursor as lithium sources can undergo a dehydration reaction in step S11, and the dehydration reaction of the hydrated lithium hydroxide can be: LiOH·H2O(s)→LiOH(s)+H2O(g), and the dehydration reaction of the nickel-cobalt-manganese precursor can be: Me(OH)2(s)→MeO2(s)+H2O(g). The nickel-cobalt-manganese precursor particles can form oxide particles after dehydration. In steps S11 and S12, the lithium hydroxide can be melted to form liquid lithium hydroxide. The reaction process in steps S12 to S14 is essentially a crystallization nucleation process in which solid and liquid phases coexist. In this process, the melted lithium hydroxide can nucleate on the surface and inside of the oxide to form tiny primary particles. Multiple tiny particles can agglomerate to form secondary particles. Since there is always liquid lithium hydroxide during the sintering process, the liquid lithium hydroxide will promote the fusion growth between the primary particles inside the secondary particles and between the secondary particles, thereby forming single crystals or single crystal-like particles with high crystallinity. During the sintering process, the positive electrode material can be transformed from an amorphous state to a regular and ordered structure. Therefore, by optimizing the sintering process of the positive electrode material, the morphology and size of the particles of the positive electrode material can be controlled, and then a positive electrode material with higher crystallinity and more uniform particle size can be obtained, thereby improving the pressure resistance of the positive electrode material.

[0079] In a preferred embodiment, the value range of T1 may be 470°C to 490°C. The temperature difference between T2 and T3 may be ≥50°C. Among them, the value range of T2 may be 650°C to 800°C. The value range of T3 may be 750°C to 900°C.

[0080] In a preferred embodiment, the value range of t1 may be 1.5 to 3.5 hours, the value range of t2 may be 4 to 8 hours, and the value range of t3 may be 7 to 14 hours.

[0081] As an exemplary illustration, in step S11, the value of t0 may be 2.8h, 2.7h, 2.5h, 2.45h, 2.4h, 2.35h, 2.3h, 2.25h, 2.2h, 2.15h, 2.1h or a lower value, or other values ​​within the range of any two of the above values, which shall be understood to be within the scope defined in the present application. The value of T0 may be 455°C, 458°C, 460°C, 462°C or 465°C, or other values ​​within the range of any two of the above values, which shall be understood to be within the scope defined in the present application.

[0082] In step S12, the value of t1 may be 2.33h, 2.30h, 2.25h, 2.20h, 2.15h, 2.10h, 2.05h, 2.0h or a lower value, or other values ​​within the range of any two values ​​above, which shall be understood as being within the scope defined in the present application. The value of t2 may be 4h, 3.9h, 3.8h, 3.7h, 3.6h, 3.5h, 3.3h, 3.2h or a lower value, or other values ​​within the range of any two values ​​above, which shall be understood as being within the scope defined in the present application. The value of T1 may be 465°C, 470°C, 475°C, 480°C, 485°C, 490°C, 495°C or 500°C, or other values ​​within the range of any two values ​​above, which shall be understood as being within the scope defined in the present application.

[0083] In step S13, the value of t3 may be 3h, 2.9h, 2.8h, 2.7h, 2.6h, 2.5h, 2.4h, 2.3h, 2.2h, 2.1h, 2.0h or a lower value, or other values ​​within the range of any two values ​​above, which shall be understood to be within the scope defined in the present application. The value of t4 may be 10h, 9.5h, 9.2h, 9h, 8.8h, 8.5h, 8.2h, 8h, 7.5h, 7.2h, 7h or a lower value, or other values ​​within the range of any two values ​​above, which shall be understood to be within the scope defined in the present application. The value of T2 may be 500°C, 520°C, 550°C, 580°C, 600°C, 620°C, 650°C, 680°C, 700°C, 720°C, 750°C, 780°C, 800°C or other values ​​within the range of any two of the above numerical values, which should be understood to be within the range defined in this application.

[0084] In step S14, the value of t5 may be 3h, 2.9h, 2.8h, 2.7h, 2.6h, 2.5h, 2.4h, 2.3h, 2.2h, 2.1h, 2.0h or a lower value, or other values ​​within any two numerical ranges, all of which shall be understood to be within the scope defined in the present application. The value of t6 may be 6h, 6.5h, 7h, 7.5h, 8h, 8.5h, 9h, 9.5h, 10h, 10.5h, 11h, 11.5h, 12h, 12.5h, 13h, 13.5h, 14h, 14.5h, 15h, 15.5h, 16h or other values ​​within any two numerical ranges, all of which shall be understood to be within the scope defined in the present application. The value of T3 may be 700°C, 720°C, 750°C, 780°C, 800°C, 820°C, 850°C, 880°C, 900°C, 920°C, 950°C, 980°C, 1000°C or other values ​​within the range of any two of the above numerical values, which should be understood to be within the range defined in this application.

[0085] The positive electrode material obtained by the preparation method of the present application is subjected to XRD diffraction analysis, and the crystallite grain size of the (003) crystal plane is a, the crystallite grain size of the (104) crystal plane is b, and the structure coefficient L=b / a, wherein the structure coefficient L≥1.05. Since the lithium ion transmission ability on the (104) crystal plane is much better than that on the (003) crystal plane, the larger the structure coefficient L, the larger the crystallite size of the (104) crystal plane relative to the (003) crystal plane, and the more conducive to the lithium ion transmission during the charge and discharge process.

[0086] Based on the same technical concept, an embodiment of the present application provides a secondary battery. The secondary battery may include a positive electrode sheet, a negative electrode sheet, an electrolyte and a separator. Among them, the positive electrode sheet and the negative electrode sheet are relatively stacked, the electrolyte and the separator are arranged between the positive electrode sheet and the negative electrode sheet, and the electrolyte infiltrates the separator. The positive electrode sheet may include a positive electrode collector and a positive electrode layer containing the positive electrode material of the embodiment of the present application arranged on at least one side surface of the positive electrode collector. The negative electrode sheet includes a negative electrode collector and a negative electrode layer containing the negative electrode material arranged on at least one side surface of the negative electrode collector. The secondary battery of the present application may be a lithium-ion battery, illustratively, it may be a nickel-cobalt-manganese ternary lithium-ion battery.

[0087] Based on the same technical concept, the embodiment of the present application provides a terminal device, which includes but is not limited to mobile phones, watches, computers, electric vehicles, energy storage devices, etc.

[0088] The present application will be further described in detail below in conjunction with specific examples. It should be understood that the following examples are only used to illustrate the present application and are not used to limit the scope of the present application.

[0089] Example 1

[0090] This embodiment is a positive electrode material, and the specific preparation process includes the following steps:

[0091] S11. Using nickel sulfate, cobalt sulfate and manganese sulfate as raw materials, dissolve the three salts in water at a molar ratio of Ni:Co:Mn=90:5:5 to prepare a 2.0 mol / L uniform mixed salt solution, prepare an alkaline solution with a sodium hydroxide concentration of 6.0 mol / L, and prepare a complexing agent solution with an ammonia concentration of 6 mol / L. Under a nitrogen atmosphere, add the mixed salt solution, alkaline solution and complexing agent solution to the reactor in parallel for reaction, set the stirring speed to 150 rpm, control the pH to about 12.0, and the reaction temperature to 60°C. After the reaction is completed, the obtained nickel cobalt manganese hydroxide slurry is filtered and washed, and the obtained filter cake is dried at 120°C for 6 hours to obtain a spherical nickel cobalt manganese hydroxide precursor Ni 0.90 Co 0.05 Mn 0.05 (OH)2.

[0092] S12, the precursor Ni obtained in step S11 0.90 Co 0.05 Mn 0.05 (OH)2, lithium hydroxide and strontium hydroxide are mixed in a high-speed mixer according to the molar ratio of Li:(Ni+Co+Mn):Sr=1.04:1:0.005.

[0093] S13, the obtained mixture is sintered in an oxygen atmosphere, and the heating and sintering process adopted is:

[0094] ① Heating from room temperature to 460℃ at a heating rate of 3℃ / min, the required time is 2.45h,

[0095] ②Heat from 460℃ to 480℃ at a heating rate of 2℃ / min, the required time is 0.17h, keep warm for 3h,

[0096] ③Heat from 480℃ to 750℃ at a heating rate of 2℃ / min, the required time is 2.25h, keep warm for 6h,

[0097] ④Heat from 750℃ to 850℃ at a heating rate of 2℃ / min, the required time is 0.83h, keep warm for 10h,

[0098] ⑤Then cool naturally to room temperature.

[0099] The sintered samples were crushed and sieved to obtain the positive electrode material Li for lithium-ion batteries. 1.04 Ni 0.9 Co 0.05 Mn 0.05 Sr 0.005 O2.

[0100] The microscopic morphology of the sample of this embodiment was observed using an electron microscope. Figure 2 It is the SEM electron microscope photo of Example 1. Figure 2 As shown, the high nickel ternary material prepared in this embodiment exhibits a single crystal morphology with a high degree of single crystallization and has good pressure resistance. The crystallinity is 83%.

[0101] The crystallinity test method is: the SEM electron microscope image of the sample is manually marked using Nano measure software, and the SEM electron microscope image at 5k magnification is counted, where the total number of all primary particles is recorded as N total On the other hand, the sum of the primary particle data contained in the "quasi-single crystal" particles formed by 5 or more primary particles in the SEM electron microscope image is recorded as N0, and the calculation method of crystallinity J is defined as J = (N total -N0) / N total ×100%.

[0102] The particle size distribution diagram of the original particles of the sample of this embodiment was tested. After applying 4t pressure and 8t pressure to the sample respectively, the particle size distribution diagram of the sample after being pressed was tested. Figure 3 This is the particle size distribution diagram of the sample in Example 1 after the original particle size and the 4t and 8t pressure resistance tests. Figure 3 The particle size distribution diagrams shown are all normalized particle size distribution diagrams. According to the particle size distribution results of the positive electrode material obtained from the test, the volume distribution K is calculated. 90 (V) and the number distribution K 90 (N), where K 90 (V)=[D 90 (V)-D 10 (V)] / D 50 (V); K 90 (N)=[D 90 (N)-D 10 (N)] / D 50 (N).

[0103] The particle size distribution of the positive electrode material is tested by using a Malvern 3000 laser particle size analyzer to test the particle size distribution. Specifically, the solvent used for the test using Malvern 3000 is 700 ml of pure water, to which 20 ml of 5% sodium pyrophosphate is added, and then the sample is added until the shading reaches 14%-16%, and then the measurement is performed, and the ultrasonic internal ultra-high test is performed, and the average result of three tests is taken as the sample particle size test data.

[0104] Example 2

[0105] This embodiment is a positive electrode material, which is different from the embodiment 1 in that the heating and sintering process is different. The other steps are the same as the embodiment 1.

[0106] The heating and sintering process in this embodiment specifically includes the following processes:

[0107] ① Heating from room temperature to 460℃ at a heating rate of 3℃ / min, the required time is 2.45h;

[0108] ②Heat from 460℃ to 480℃ at a heating rate of 2℃ / min, the required time is 0.17h, and keep warm for 3h;

[0109] ③Heat from 480℃ to 750℃ at a heating rate of 2℃ / min, the required time is 2.25h, and keep warm for 6h;

[0110] ④ Heating from 750℃ to 850℃ at a heating rate of 2℃ / min, the required time is 0.83h, and the temperature is kept for 16h;

[0111] ⑤Then cool naturally to room temperature.

[0112] The sintered samples were crushed and sieved to obtain the positive electrode material Li for lithium-ion batteries. 1.04 Ni 0.9 Co 0.05 Mn 0.05 Sr 0.005 The high-nickel ternary positive electrode material prepared in this comparative example exhibits a single crystal morphology with a high degree of single crystallization and has good pressure resistance.

[0113] Example 3

[0114] This embodiment is a positive electrode material, which is different from the embodiment 1 in that the heating and sintering process is different. The other steps are the same as the embodiment 1.

[0115] The heating and sintering process in this embodiment specifically includes the following processes:

[0116] ① Heating from room temperature to 460℃ at a heating rate of 3℃ / min, the required time is 2.45h;

[0117] ②Heat from 460℃ to 480℃ at a heating rate of 2℃ / min, the required time is 0.17h, and keep warm for 1h;

[0118] ③Heat from 480℃ to 750℃ at a heating rate of 2℃ / min, the required time is 2.25h, and keep warm for 6h;

[0119] ④Heat from 750℃ to 850℃ at a heating rate of 2℃ / min, the required time is 0.83h, and keep warm for 10h;

[0120] ⑤Then cool naturally to room temperature.

[0121] The sintered samples were crushed and sieved to obtain the positive electrode material Li for lithium-ion batteries. 1.04 Ni 0.9 Co 0.05 Mn 0.05 Sr 0.005 The high-nickel ternary positive electrode material prepared in this embodiment exhibits a single crystal morphology with a high degree of single crystallization and has good pressure resistance.

[0122] Comparative Example 1

[0123] This comparative example is a positive electrode material, which is different from Example 1 in that the heating and sintering process is different. The other steps are the same as Example 1.

[0124] The heating and sintering process in this comparative example specifically includes the following processes:

[0125] ① Heating from room temperature to 460℃ at a heating rate of 3℃ / min, the required time is 2.45h;

[0126] ②Heat from 460℃ to 850℃ at a heating rate of 2℃ / min for 3.25h, and keep warm for 14h;

[0127] ③ Cool naturally to room temperature.

[0128] The sintered samples were crushed and sieved to obtain the positive electrode material Li for lithium-ion batteries. 1.04 Ni 0.9 Co0.05Mn 0.05 Sr 0.005 O2.

[0129] The microscopic morphology of the sample of this embodiment was observed using an electron microscope. Figure 4 This is the SEM electron microscope photo of Comparative Example 1. Figure 4 As shown, the high-nickel ternary positive electrode material prepared in this comparative example exhibits a single-crystal morphology with a large number of agglomerated particles, and its pressure resistance is poor.

[0130] The particle size distribution diagram of the original particles of the sample of this embodiment was tested. After applying 4t pressure and 8t pressure to the sample respectively, the particle size distribution diagram of the sample after being pressed was tested. Figure 5 This is the particle size distribution diagram of the sample in comparative example 1 after the original particle size and the 4t and 8t pressure resistance tests. Figure 5 The particle size distribution diagrams shown are all normalized particle size distribution diagrams.

[0131] Comparative Example 2

[0132] This comparative example is a positive electrode material, which is different from Example 1 in that the heating and sintering process is different. The other steps are the same as Example 1.

[0133] The heating and sintering process in this comparative example specifically includes the following processes:

[0134] ① Heating from room temperature to 460℃ at a heating rate of 3℃ / min, the required time is 2.45h;

[0135] ②Heat from 460℃ to 750℃ at a heating rate of 2℃ / min, the required time is 2.42h, and keep warm for 6h;

[0136] ③ Heating from 750℃ to 850℃ at a heating rate of 2℃ / min, the required time is 0.83h, and the temperature is kept for 10h;

[0137] ④ Cool naturally to room temperature.

[0138] The sintered samples were crushed and sieved to obtain the positive electrode material Li for lithium-ion batteries. 1.04 Ni 0.9 Co0.05Mn 0.05 Sr 0.005The high-nickel ternary positive electrode material prepared in this comparative example exhibits a single-crystal morphology with a large number of agglomerated particles, and its pressure resistance is relatively poor.

[0139] Comparative Example 3

[0140] This comparative example is a positive electrode material, which is different from Example 1 in that the heating and sintering process is different. The other steps are the same as Example 1.

[0141] The heating and sintering process in this comparative example specifically includes the following processes:

[0142] ① Heating from room temperature to 460℃ at a heating rate of 3℃ / min, the required time is 2.45h;

[0143] ②Heat from 460℃ to 480℃ at a heating rate of 2℃ / min, the required time is 0.17h, and keep warm for 9h;

[0144] ③Heat from 480℃ to 850℃ at a heating rate of 2℃ / min, the required time is 3.05h, and keep warm for 10h;

[0145] ④ Cool naturally to room temperature.

[0146] The sintered samples were crushed and sieved to obtain the positive electrode material Li for lithium-ion batteries. 1.04 Ni 0.9 Co0.05Mn 0.05 Sr 0.005 The high-nickel ternary positive electrode material prepared in this comparative example exhibits a single-crystal morphology with a large number of agglomerated particles, and its pressure resistance is relatively poor.

[0147] Comparative Example 4

[0148] This comparative example is a positive electrode material, which is different from Example 1 in that the heating and sintering process is different. The other steps are the same as Example 1.

[0149] The heating and sintering process in this comparative example specifically includes the following processes:

[0150] ① Heating from room temperature to 460℃ at a heating rate of 3℃ / min, the required time is 2.45h;

[0151] ②Heat from 460℃ to 480℃ at a heating rate of 2℃ / min, the required time is 0.17h, and keep warm for 1h;

[0152] ③Heat from 480℃ to 750℃ at a heating rate of 2℃ / min for 2.25h, and keep warm for 1h;

[0153] ④Heat from 750℃ to 850℃ at a heating rate of 2℃ / min, the required time is 0.83h, and keep warm for 10h;

[0154] ⑤ Cool naturally to room temperature.

[0155] The sintered samples were crushed and sieved to obtain the positive electrode material Li for lithium-ion batteries. 1.04 Ni 0.9 Co0.05Mn 0.05 Sr 0.005 The high-nickel ternary positive electrode material prepared in this comparative example exhibits a single-crystal morphology with a large number of agglomerated particles, and its pressure resistance is relatively poor.

[0156] The area parameters and specific surface area values ​​obtained by integrating the particle size distribution diagrams of the original particles and the compressed particles of the above embodiments and comparative examples are listed in Table 1. The specific surface area test was carried out using a Tri-star 3020 specific surface meter, and the sample pretreatment conditions were heating to 300°C and degassing for 60 minutes, and then the test value was obtained by reading it from the software using a static test method.

[0157] Table 1

[0158]

[0159]

[0160] The high nickel ternary positive electrode materials of each embodiment and comparative example were used to assemble lithium ion battery button half-cells. After assembly, the 0.1C discharge specific capacity, the first coulomb efficiency and the cycle retention rate after 80 charge and discharge cycles of each sample battery were tested. The test voltage was 3.0 to 4.3 V, and the test results are listed in Table 2. Figure 6 The following are the cycle comparison data of the sample batteries corresponding to Comparative Example 1 and Example 1. Figure 6 In the corresponding 80 cycle tests, the charge and discharge voltage was 4.3V, the charge and discharge current was 1C, and the test temperature was 45°C.

[0161] Table 2

[0162]

[0163] Combining Table 1 with Table 2 and Figure 6 , the cycle retention rate of Examples 1-3 of the present application is significantly better than that of Comparative Examples 1-4. 90(V) and the particle size distribution coefficient K are all within the range defined in the present application. It shows that the particle size distribution of the positive electrode particles obtained in Examples 1-3 is more uniform. In addition, compared with Comparative Examples 1-4, the structural coefficient L of the positive electrode material of Examples 1-3 is also higher, indicating that the positive electrode material of the present application embodiment is more conducive to the transmission of lithium ions.

[0164] For Example 1, its characteristic is that the sintering process adopts a multi-stage programmed temperature increase, directly increases the temperature from room temperature to 460°C, then reduces the heating rate and increases the temperature to 480°C and maintains it for a period of time, so that the lithium salt can fully contact the precursor particles. This process can make the crystal nucleation process more uniform and orderly. Then continue to heat up to 750°C to form highly uniform and orderly morphological secondary particles. Then continue to heat up to 850°C and keep it warm for a certain period of time to grow single crystal particles with a high degree of single crystallization and uniform morphology.

[0165] In Example 2, the holding time at 850° C. is prolonged to obtain larger single crystal particles. However, too long a holding time may cause excessive sintering of the single crystal material, which may have a certain impact on the capacity.

[0166] In Example 3, the reaction time of the lithium hydroxide solution and the precursor is shortened, and the voltage resistance of the final positive electrode material is improved to a certain extent, but it is not as good as the positive electrode material prepared under the preferred conditions, but its voltage resistance and cycle performance are still better than the comparative example.

[0167] For Comparative Example 1, during the sintering heating process, the temperature was first directly raised from room temperature to 460° C., and then directly raised to 850° C. In this process, since the liquid lithium hydroxide and the decomposition products of the precursor reacted directly during the heating process, the wetting and contact effect between the liquid lithium salt and the precursor was poor, so multiple crystal nuclei were formed during the heating reaction and grew randomly, resulting in poor particle uniformity and a single crystal morphology in which multiple primary particles were aggregated together, poor pressure resistance, and poor electrical properties.

[0168] Compared with Comparative Example 1, the advantage of Comparative Example 2 is that after reaching 460°C, the temperature is first raised to 750°C, which is the corresponding temperature for the formation of secondary particles. At this temperature, the lithium salt will form secondary particles composed of small primary particles aggregated with the precursor. Maintaining this temperature for a period of time can limit the uneven growth of crystal particles to a certain extent. After keeping at 750°C for a period of time, the temperature is raised to 850°C again. After the Austenite ripening process, the particles are able to grow and grow, thereby obtaining a material with a relatively better morphology. However, similarly, due to the relatively fast overall temperature rise in the sintering process, the precursor and the lithium salt cannot be in uniform contact, and the pressure resistance of the obtained Comparative Example 2 material is improved compared with that of Comparative Example 1, but it is still poor.

[0169] In Comparative Example 3, the temperature was maintained at 480°C for a long time, so that the lithium salt could fully contact with the precursor particles, and the crystal nucleation process was more uniform and orderly. The temperature was then directly raised to a higher temperature of 880°C and kept for a longer time. The single crystal morphology obtained finally had a high degree of single crystalization but the particles were over-sintered. The formed single crystal particles were larger and had obvious edges and corners, which was not conducive to the overall compaction performance and had an adverse effect on the capacity and cycle.

[0170] In Comparative Example 4, the holding time at 750°C, the temperature at which the secondary particles are formed, is relatively short, and then the temperature is continued to be raised to 850°C for single crystal growth. Due to the short holding time at 750°C, the secondary particles cannot be fully grown, and only a large number of crystal nuclei can be formed. On this basis, raising the temperature to 850°C will cause single crystal particles to grow in large quantities on the basis of more crystal nuclei and cannot grow up fully. Therefore, the method of Comparative Example 4 can only obtain particles with a single-crystal-like morphology that are still multiple primary particles gathered together. At the same time, compared with the single-crystal-like particles and the primary particles inside a single-crystal-like particle, the particles have a relatively uniform size but a smaller size. Compared with Comparative Example 2, the overall reaction time of Comparative Example 4 is the same, but the single crystal growth time at 850°C is short. Therefore, the obtained single crystal has low crystallinity and poor voltage resistance. Although the capacity is high, the cycle performance is poor.

[0171] The above experiments show that in the present embodiment, by controlling S 1(4t) / S 1(8t) Ratio and S 2(4t) / S 2(8t) The ratio of can obtain a positive electrode material with better pressure resistance. At the same time, the positive electrode material of the embodiment of the present application also introduces a high content of nickel into the nickel-cobalt-manganese ternary material to increase the capacity of the positive electrode material. When the positive electrode material having the above characteristics is applied to a secondary battery, the cycle performance of the secondary battery can be effectively improved. In addition, the preparation method provided in the embodiment of the present application forms high-nickel single crystal ternary positive electrode material particles with good single crystallization by continuously setting different temperatures and reaction times during the sintering process. The preparation method of the embodiment of the present application is simple and convenient to operate, can be applied to various kiln equipment, and is suitable for large-scale production.

[0172] The above are only specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any technician familiar with the technical field can easily think of changes or substitutions within the technical scope disclosed in the present application, which should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.

Claims

1. A positive electrode material, characterized in that: The area of ​​the first particle size distribution diagram of the positive electrode material before being pressed is S0, and the area of ​​the second particle size distribution diagram of the positive electrode material after being subjected to 4 tons of pressure is S (4t) The area of ​​the overlap between the first particle size distribution diagram and the second particle size distribution diagram is ΔS (4t) The area of ​​the third particle size distribution diagram of the positive electrode material after being subjected to 8 tons of pressure is S (8t) The area of ​​the overlap between the first particle size distribution diagram and the third particle size distribution diagram is ΔS (8t) ; S 1(4t) =S (4t) -△S (4t) ,S 2(4t) =S0-△S (4t) ; S 1(8t) =S (8t) -△S (8t) ,S 2(8t) =S0-△S (8t) ; Among them, S 1(8t) / S 1(4t) ≤1.2, S 2(8t) / S 2(4t) ≤1.

3.

2. The positive electrode material according to claim 1, characterized in that S 1(8t) / S 1(4t) ≤1.1,S 2(8t) / S 2(4t) ≤1.2。 3. The positive electrode material according to claim 1 or 2, characterized in that The specific surface area of ​​the positive electrode material before being pressed is B0, and the specific surface area of ​​the positive electrode material after being pressed by 4 tons is B (4t) The specific surface area of ​​the positive electrode material after being subjected to 8 tons of pressure is B (8t) ; in, B (8t) / B (4t) ≤1.26,B (8t) / B0≤1.56。 4. The positive electrode material according to claim 3, characterized in that B (8t) / B (4t) ≤1.23,B (8t) / B0≤1.51。 5. The positive electrode material according to any one of claims 1 to 4, characterized in that The particle crystallinity of the positive electrode material is 78% to 95%.

6. A positive electrode material, characterized in that: The particle crystallinity of the positive electrode material is 78% to 95%, and the particle size dispersion coefficient K of the positive electrode material satisfies 1.050≤K≤1.150, wherein: K=K 90 (V) / K 90 (N); K 90 (V)=[D 90 (V)-D 10 (V)] / D 50 (V); K 90 (N)=[D 90 (N)-D 10 (N)] / D 50 (N); K 90 (V) value range 0.800≤K 90 (V)≤1.600; D 90 (V) is the particle size corresponding to when the cumulative particle size volume distribution of the positive electrode material particles reaches 90%; D 10 (V) is the particle size corresponding to when the cumulative particle size volume distribution of the positive electrode material particles reaches 10%; D 50 (V) is the particle size corresponding to when the cumulative particle size volume distribution of the positive electrode material particles reaches 50%; D 90 (N) is the particle size corresponding to when the cumulative particle size distribution of the positive electrode material particles reaches 90%; D 10 (N) is the particle size corresponding to when the cumulative particle size distribution of the positive electrode material particles reaches 10%; D 50 (N) is the particle size corresponding to when the cumulative particle size number distribution of the positive electrode material particles reaches 50%.

7. The method for preparing the positive electrode material according to any one of claims 1 to 6, characterized in that: include: A mixture of a nickel-cobalt-manganese precursor, a lithium source and an oxide containing a doping element is sintered, and the positive electrode material is obtained after cooling; wherein the sintering process comprises: Heating from room temperature to T0 within t0 at a heating rate of 1.0-3.0°C / min; t0≤2.8h, 455°C≤T0≤465°C; Heating from T0 to T1 at a heating rate of 1.0-3.0°C / min at time t1, and keeping warm for t2; t1≤2.33h, 465°C≤T1≤500°C and T1>T0, t2≤4h; Heating from T1 to T2 at a heating rate of 1.0-3.0°C / min at time t3, and keeping warm for t4; t3≤3h, 500°C≤T2≤800°C and T2>T1, t4≤10h; The temperature is increased from T2 to T3 at a heating rate of 1.0-3.0°C / min at time t5, and kept at a temperature of t6; t5≤3h, 700°C≤T3≤1000°C and T3>T2, 6h≤t6≤16h.

8. The preparation method according to claim 7, characterized in that: The T1 satisfies: 470°C ≤ T1 ≤ 490°C.

9. The preparation method according to claim 7 or 8, characterized in that: The T2 and the T3 satisfy: T3-T2≥50°C, 650°C≤T2≤800°C, 750°C≤T3≤900°C.

10. The preparation method according to any one of claims 7 to 9, characterized in that: The t1 satisfies 1.5h≤t1≤3.5h, the t2 satisfies 4h≤t2≤8h, and the t3 satisfies 7h≤t3≤14h.

11. The preparation method according to any one of claims 7 to 10, characterized in that: The molar ratio of the lithium source to the nickel-cobalt-manganese precursor is 1.0 to 1.1:

1.

12. A secondary battery, characterized in that: It comprises a positive electrode plate, a separator and a negative electrode plate, wherein the positive electrode plate comprises the positive electrode material as claimed in any one of claims 1 to 6.

13. A terminal device, characterized in that: Comprising the secondary battery as claimed in claim 12.

Citation Information

Cited By

  • Method for rapidly evaluating performance of silicon-carbon negative electrode material of lithium ion battery

    CN119618907A

  • Positive electrode active material and preparation method therefor, positive electrode sheet, battery, and electric device

    WO2026208032A1

  • Positive electrode active material, positive electrode, lithium-ion secondary battery, and lithium-ion secondary battery module

    WO2026211590A1