Secondary battery and method for manufacturing same

By arranging the extension of the conductive and non-conductive areas on the separator of the lithium metal secondary battery, and using the separator design with alternate folding structure, the positional deviation of the positive electrode layer and the negative electrode layer during the charge and discharge process of the lithium metal secondary battery is solved. and short circuit problems, improving the energy efficiency and capacity stability of the battery.

CN118738510APending Publication Date: 2024-10-01HONDA MOTOR CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310321328.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

During the charging and discharging process of lithium metal secondary batteries, due to changes in the thickness of the negative electrode layer, the positions of the positive electrode layer and the negative electrode layer shift, short circuits may occur, and the density of the negative electrode active material decreases, affecting the energy efficiency of the battery.

Method used

An extension is provided on the positive terminal side of the separator, part of which is a conductive area and part of which is a non-conductive area, to ensure that the conductive layer is not easily in contact with the positive electrode layer and the positive electrode lead, preventing short circuits, and through the alternation of long insulating porous films The folded structure stabilizes the position of the conductive layer and the non-conductive area, and increases the contact area between the conductive layer and the negative electrode layer.

Benefits of technology

It effectively prevents the short circuit between the positive electrode layer and the negative electrode layer caused by charging and discharging, increases the density of active materials in the negative electrode layer, and improves the energy efficiency and capacity stability of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118738510A_ABST
    Figure CN118738510A_ABST
Patent Text Reader

Abstract

The problem to be solved by the present invention is to provide: a secondary battery in which, even if the thickness of a negative electrode layer changes greatly due to charging and discharging and the negative electrode layer side of a separator has a conductive layer, the conductive layer does not easily come into contact with a positive electrode layer and a positive electrode lead, and short-circuiting does not easily occur between the positive electrode layer and the negative electrode layer; this secondary battery is provided with: an electrode laminate having a positive electrode layer, a negative electrode layer, and a separator disposed between the positive electrode layer and the negative electrode layer; an electrolyte; an exterior body that accommodates the electrode laminate and the electrolyte solution; a positive electrode terminal and a negative electrode terminal provided in the exterior body; a positive electrode lead electrically connecting the positive electrode layer and the positive electrode terminal; and a negative electrode lead electrically connecting the negative electrode layer and the negative electrode terminal. The separator has an extending portion extending outward beyond an end portion of the positive electrode layer on a side connected to the positive electrode terminal. On the surface of the separator on the negative electrode layer side, at least a portion of a portion in contact with the negative electrode layer is a conductive region in which a conductive layer is provided, and at least a portion of an end portion of the extended portion on the positive electrode terminal side is a non-conductive region in which the conductive layer is not provided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a secondary battery and a method for manufacturing the same. Background Art

[0002] In recent years, in order to make it affordable and trustworthy for many people, and to ensure access to sustainable and advanced energy, research and development have been conducted on secondary batteries that help improve energy efficiency. In order to increase the energy density of secondary batteries, a secondary battery with a laminated structure in which multiple positive electrode layers and negative electrode layers are alternately overlapped has been studied. In the secondary battery with this laminated structure, in order to suppress the positional displacement of the positive electrode layer and the negative electrode layer, it has been studied to bend the long strip of separator into a zigzag shape, and to alternately overlap the positive electrode layer and the negative electrode layer in the folded portion (Patent Documents 1, 2).

[0003] [Prior art literature]

[0004] [Patent Document]

[0005] [Patent Document 1] International Publication No. 2020 / 003846

[0006] [Patent Document 2] International Publication No. 2020 / 003847 Summary of the invention

[0007] [Problems to be solved by the invention]

[0008] However, in the related technology of secondary batteries, the subject is high capacity. In order to achieve high capacity of secondary batteries, it is hoped that lithium metal secondary batteries using metallic lithium as negative electrode active materials can be put into practical use. However, the thickness of the negative electrode layer of lithium metal secondary batteries will change greatly due to charging and discharging. Therefore, in a lithium metal secondary battery with a laminated structure in which multiple positive electrode layers and negative electrode layers are alternately stacked, the positive electrode layer and the negative electrode layer may be easily misaligned due to the change in the thickness of the negative electrode layer caused by charging and discharging.

[0009] Moreover, in lithium metal secondary batteries, due to repeated charging and discharging, an SEI layer (solid electrolyte interphase) accumulates at the interface between the collector of the negative electrode layer and lithium, and lithium dendrites are easily generated during charging. Once lithium dendrites are generated, the lithium dendrites may penetrate the diaphragm and cause a short circuit between the positive electrode layer and the negative electrode layer. Moreover, once lithium dendrites are generated, the density of the metal lithium layer (negative electrode active material layer) precipitated on the negative electrode collector may be reduced, thereby causing the lithium secondary battery to expand excessively during charging.

[0010] According to the research of the inventors, sometimes, by using a laminated body with a conductive layer stacked on the surface of a porous film as a separator, and configuring the conductive layer in a manner that the conductive layer is on the negative electrode layer side, it is possible to suppress a short circuit caused by dendrites or a decrease in the active material layer density of the negative electrode layer in a charged state. However, in a secondary battery using a separator having a conductive layer on the surface of the negative electrode layer side, the conductive layer contacts the positive electrode layer or the positive electrode lead connecting the positive electrode layer to the positive terminal, and a short circuit may occur between the positive electrode layer and the negative electrode layer.

[0011] The present invention is completed in view of the above, and its purpose is to provide a secondary battery and a manufacturing method thereof, wherein even if the thickness of the negative electrode layer of the secondary battery changes greatly due to charging and discharging, and the negative electrode layer side of the separator has a conductive layer, the conductive layer is not easy to contact the positive electrode layer and the positive electrode lead, and the positive electrode layer and the negative electrode layer are not easy to short-circuit. Moreover, the present invention even helps to improve energy efficiency.

[0012] [Technical means to solve the problem]

[0013] The inventors have found that the above-mentioned problem can be effectively solved by providing an extension portion extending outward beyond the end of the positive electrode layer on the side connected to the positive electrode terminal in the separator, setting at least a portion of the portion in contact with the negative electrode layer as a conductive region provided with a conductive layer, and setting at least a portion of the end of the positive electrode terminal side of the extension portion as a non-conductive region not provided with a conductive layer, thereby completing the present invention. Therefore, the present invention provides the following technology.

[0014] (1) A secondary battery, comprising: an electrode stack having a positive electrode layer, a negative electrode layer, and a separator arranged between the positive electrode layer and the negative electrode layer; an electrolyte; an outer body accommodating the electrode stack and the electrolyte; a positive terminal and a negative terminal, which are arranged on the outer body; a positive electrode lead electrically connecting the positive electrode layer to the positive terminal; and a negative electrode lead electrically connecting the negative electrode layer to the negative terminal; the separator having an extension portion extending outward beyond the end of the positive electrode layer on the side connected to the positive terminal; on the surface of the separator on the negative electrode layer side, at least a portion of the portion in contact with the negative electrode layer is set as a conductive region provided with a conductive layer, and at least a portion of the end of the extension portion on the positive terminal side is set as a non-conductive region where the conductive layer is not provided.

[0015] According to the secondary battery of (1), since at least a portion of the extension portion of the separator extending outward beyond the end of the positive electrode layer on the side connected to the positive terminal is set as a non-conductive region, even if the thickness of the negative electrode layer changes significantly due to charge and discharge, the conductive layer provided in the portion of the separator in contact with the negative electrode layer is not easy to contact the positive electrode layer and the positive electrode lead. Therefore, a short circuit is not easy to occur between the positive electrode layer and the negative electrode layer.

[0016] (2) A secondary battery according to (1), wherein the separator is a long strip separator, comprising a long strip insulating porous membrane, and the conductive region and the non-conductive region provided on one surface of the long strip insulating porous membrane, wherein the conductive region extends along the length direction of the long strip insulating porous membrane, and the non-conductive region is arranged at least at one end in the width direction of the long strip insulating porous membrane, and the long strip separator is formed by alternatingly overlapping the first fold and the second fold, wherein the first fold has the surface of the long strip insulating porous membrane side as the inner side. The positive electrode layer is sandwiched in the first fold and is located at a position where the non-conductive region becomes the extension portion, and the negative electrode layer is sandwiched in the second fold and is located at a position in contact with the conductive region; the positive electrode terminal is electrically connected to an end of the positive electrode layer on the side where the non-conductive region is disposed; and the negative electrode terminal is electrically connected to an end of the negative electrode layer on the side opposite to the side where the non-conductive region is disposed.

[0017] According to the secondary battery of (2), the separator is a long strip separator, the positive electrode layer is located at the first fold formed alternately, and the negative electrode layer is located at the second fold, so that the positive electrode layer and the negative electrode layer are not easily offset. In addition, a strip-shaped conductive layer is formed along the length direction of the long strip separator, and the length of the conductive layer in the length direction is longer than the length of the negative electrode layer, so that the effect of the conductive layer can be effectively obtained. In addition, the non-conductive area of ​​the long strip separator becomes an extension portion, so that the conductive layer is not easily in contact with the positive electrode layer and the positive electrode lead.

[0018] (3) The secondary battery according to (1) or (2), wherein the end of the conductive region on the positive electrode terminal side is located the same as or inside the end of the negative electrode layer on the positive electrode terminal side.

[0019] According to the secondary battery of (3), the end of the extension portion is a non-conductive region, so the conductive layer is unlikely to come into contact with the positive electrode layer and the positive electrode lead.

[0020] (4) The secondary battery according to any one of (1) to (3), wherein the non-conductive region is disposed only at an end portion of the separator on the positive electrode terminal side.

[0021] According to the secondary battery of (4), the area other than the end of the extension portion is a conductive region, and the contact area between the conductive layer and the negative electrode layer is increased, thereby suppressing short circuits due to dendrites or a decrease in the density of the active material layer of the negative electrode layer in a charged state.

[0022] (5) The secondary battery according to any one of (1) to (4), wherein the negative electrode active material is metallic lithium.

[0023] According to the secondary battery of (5), since the negative electrode active material is metallic lithium, a high capacity can be achieved.

[0024] (6) A method for manufacturing a secondary battery, comprising the following steps: preparing a long strip separator, the long strip separator comprising a long strip insulating porous membrane, and a conductive region provided with a conductive layer and a non-conductive region not provided with a conductive layer arranged on one surface of the long strip insulating porous membrane, the conductive region extending along the length direction of the long strip insulating porous membrane, the non-conductive region causing a long strip laminated sheet arranged at at least one end in the width direction of the long strip insulating porous membrane to be in a meandering shape, and the long strip separator is formed by alternatingly overlapping a first fold and a second fold. , the first fold is bent in the length direction with the surface on the side of the long strip of insulating porous membrane as the inner side, and the second fold is bent in the length direction with the surface on the side where the conductive area and the non-conductive area are arranged as the inner side; the positive electrode layer and the first fold are arranged opposite to each other, and the negative electrode layer and the second fold are arranged opposite to each other; and the positive terminal is connected to the end of the positive electrode layer on the side where the non-conductive area is arranged via the positive lead, and the negative terminal is connected to the end of the negative electrode layer on the opposite side of the side connected to the positive terminal via the negative lead.

[0025] According to the manufacturing method of the secondary battery of (6), the positive terminal is connected to the end of the positive electrode layer on the side where the non-conductive area is arranged via the positive electrode lead, so it is beneficial to industrially manufacture a secondary battery in which an extension portion extends from the end of the positive electrode layer on the side connected to the positive terminal. In addition, the positive electrode layer is arranged at the first fold of the long strip separator, and the negative electrode layer is arranged at the second fold. Therefore, in the obtained secondary battery, the positive electrode layer and the negative electrode layer are not easily misaligned. In addition, a strip-shaped conductive layer is formed along the length direction of the long strip separator, and the length of the conductive layer in the length direction is longer than the length of the negative electrode layer. Therefore, the effect of the conductive layer can be effectively obtained in the obtained secondary battery.

[0026] [Effects of the invention]

[0027] According to the present invention, a secondary battery and a method for manufacturing the same can be provided. Even if the thickness of the negative electrode layer of the secondary battery changes significantly due to charge and discharge, and a separator having a conductive layer on the negative electrode layer side is used, the conductive layer is not likely to contact the positive electrode layer and the positive electrode lead, and a short circuit is not likely to occur between the positive electrode layer and the negative electrode layer. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 It is a perspective view of a secondary battery in one embodiment of the present invention.

[0029] Figure 2 yes Figure 1Sectional view along line II-II.

[0030] Figure 3 yes Figure 1 Cross-sectional view along line III-III.

[0031] Figure 4 This is a plan view of a separator that can be used in a secondary battery according to one embodiment of the present invention.

[0032] Figure 5 yes Figure 4 VV line cross-sectional view. DETAILED DESCRIPTION

[0033] Hereinafter, embodiments of the present invention will be described with reference to the drawings. However, the embodiments described below are merely illustrative of the present invention, and the present invention is not limited to the following contents.

[0034] Figure 1 It is a perspective view of the secondary battery in the first embodiment of the present invention. Figure 2 yes Figure 1 The II-II line cross-sectional view, Figure 3 yes Figure 1 Cross-sectional view along line III-III. Figure 4 This is a plan view of a separator that can be used in a secondary battery according to one embodiment of the present invention. Figure 5 yes Figure 4 VV line cross-sectional view.

[0035] The secondary battery 100 in this embodiment includes: an electrode stack 10 having a positive electrode layer 20, a negative electrode layer 30, and a long strip separator 40 disposed between the positive electrode layer 20 and the negative electrode layer 30; an electrolyte (not shown); and an outer body 50 that contains the electrode stack 10 and the electrolyte. The positive electrode layer 20 includes: a positive electrode collector 21, and a positive electrode active material layer 22 stacked on both sides of the positive electrode collector 21. The negative electrode layer 30 includes: a negative electrode collector 31, and a lithium foil 32 stacked on both sides of the negative electrode collector 31. The secondary battery 100 is set as a lithium metal secondary battery. In a lithium metal secondary battery, metallic lithium is used as a negative electrode active material. When charging, lithium is released from the positive electrode active material layer 22, and the lithium is precipitated on the surface of the lithium foil 32 to form a metallic lithium layer. Therefore, when charging, the thickness of the negative electrode layer 30 increases. On the other hand, during discharge, lithium is released from the metal lithium layer and is stored in the positive electrode active material layer 22. Therefore, during discharge, the thickness of the negative electrode layer 30 decreases. Therefore, the thickness of the negative electrode layer 30 changes greatly due to charge and discharge. Figure 1 to Figure 3 The secondary battery 100 shown is in a discharge state. The widths of the positive electrode layer 20, the negative electrode layer 30 and the long strip separator 40 are as shown in FIG. Figure 2 As shown, the strip-shaped separator 40 is the widest, the negative electrode layer 30 is the second widest, and the positive electrode layer 20 is the narrowest.

[0036] The secondary battery 100 also has: a positive terminal 24 and a negative terminal 34, which are provided on the outer body 50; a positive electrode lead 23, which electrically connects the positive electrode layer 20 (positive electrode collector 21) and the positive terminal 24; and a negative electrode lead 33, which electrically connects the negative electrode layer 30 (negative electrode collector 31) and the negative terminal 34. Parts of the positive terminal 24 and the negative terminal 34 are exposed to the outside. The positive terminal 24 is arranged along the width direction of the long strip separator 40 (a direction perpendicular to the length direction of the long strip separator 40), and the negative terminal 34 is arranged at a position opposite to each other with the electrode stack 10 sandwiched therebetween.

[0037] The long strip separator 40 has an extension portion 40a extending outward beyond the end of the positive electrode layer 20 connected to the positive electrode terminal 24. The extension length of the extension portion 40a also varies depending on the thickness of the positive electrode layer 20, the size of the positive electrode lead 23, the thickness of the conductive layer 42, etc., but is, for example, greater than the thickness of the positive electrode active material layer 22. When the width of the positive electrode layer 20 is greater than the width of the negative electrode layer 30, the extension portion 40a may also extend beyond the end of the negative electrode layer 30.

[0038] On the surface of the long strip separator 40 on the negative electrode layer 30 side, at least a portion of the portion in contact with the negative electrode layer 30 is set as a conductive region 401 provided with a conductive layer 42, and at least a portion of the end of the extension 40a on the positive terminal side is set as a non-conductive region 402 where the conductive layer 42 is not provided. The width of the conductive layer 42 (the length in the direction orthogonal to the length direction of the long strip separator 40) may be greater than the width of the positive electrode layer 20, or may be the same as or less than the width of the negative electrode layer 30. Regarding the width of the conductive layer 42, the end of the conductive layer 42 (conductive region 401) on the negative electrode terminal 34 side may extend beyond the negative electrode layer 30, or may be arranged to the end of the long strip separator 40. The end of the conductive layer 42 on the positive terminal 24 side may be located at the same side as or further inside than the end of the negative electrode layer 30 on the positive terminal 24 side. In the present embodiment, the end of the conductive layer 42 on the positive terminal 24 side is located inside the end of the negative electrode layer 30 on the positive terminal 24 side. The non-conductive region 402 may be disposed only at the end portion of the long separator 40 on the positive electrode terminal 24 side. The width of the non-conductive region is preferably greater than at least the thickness of the positive electrode active material layer 22 .

[0039] The long strip separator 40 includes a long strip insulating porous film 41, a conductive region 401 disposed on the surface of the long strip insulating porous film 41 on the negative electrode layer 30 side, and a non-conductive region 402 (see Figure 4). The conductive region 401 has a strip-shaped conductive layer 42 arranged along the length direction of the long strip insulating porous membrane 41. The non-conductive region 402 does not have a conductive layer 42. At least one end of the width direction of the long strip insulating porous membrane 41 is the non-conductive region 402. In the present embodiment, the non-conductive region 402 is arranged at one end of the width direction of the long strip insulating porous membrane 41. The long strip diaphragm 40 is formed by folding the first fold 43 and the second fold 44 alternately. The first fold 43 is a portion bent in the length direction in a manner that the surface on the side of the long strip insulating porous membrane 41 is the inner side. The first fold 43 has a folded front end 43a and an opening 43b located on the opposite side of the front end 43a. The second fold 44 is a portion bent in the length direction in a manner that the surface on the side where the conductive region 401 and the non-conductive region 402 are arranged is the inner side. The second folded portion 44 has a folded front end 44 a and an opening 44 b located on the opposite side of the front end 44 a .

[0040] The positive electrode layer 20 and the first fold 43 are arranged opposite to each other, and the negative electrode layer 30 and the second fold 44 are arranged opposite to each other. The positive electrode layer 20 is in contact with the long strip insulating porous film 41 of the long strip separator 40, and the negative electrode layer 30 is in contact with the conductive layer 42 of the long strip separator 40. The positive terminal 24 is connected to the end of the positive electrode layer 20 (positive electrode collector 21) on the side where the non-conductive region 402 is arranged. Thus, the non-conductive region 402 of the long strip separator 40 functions as an extension 40a. The negative terminal 34 is connected to the end of the negative electrode layer 30 (negative electrode collector 31) on the opposite side to the side connected to the positive terminal 24. The end of the positive electrode layer 20 on the opposite side to the side connected to the positive terminal 24 (the side where the negative electrode layer 30 is connected to the negative terminal 34) can also be located further inside than the end of the negative electrode layer 30.

[0041] The material of the positive electrode collector 21 is not particularly limited, and for example, aluminum can be used. The material of the positive electrode lead 23 may be the same as or different from the material of the positive electrode collector 21. The positive electrode lead 23 may also be integrally connected to the positive electrode collector 21. In the present embodiment, the positive electrode lead 23 is formed by extending the positive electrode collector 21, and is integrally connected to the positive electrode collector 21. The material of the positive terminal 24 may be the same as or different from the material of the positive electrode lead 23. The positive terminal 24 may also be integrally connected to the positive lead 23. In the present embodiment, the positive terminal 24 and the positive lead 23 are different components and are electrically connected to each other.

[0042] The positive electrode active material layer 22 contains a positive electrode active material. Examples of the positive electrode active material include lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), and LiNiO2. p Mn q Co rO2(p+q+r=1), LiNi p Al q Co r O2(p+q+r=1), lithium manganate (LiMn2O4), Li 1+x Mn 2-x-y M y O4 (x+y=2, M=at least one selected from Al, Mg, Co, Fe, Ni and Zn) represented by a heterogeneous element substituted Li-Mn spinel, lithium titanate (an oxide containing Li and Ti), lithium metal phosphate (LiMPO4, M=at least one selected from Fe, Mn, Co, and Ni), etc. The positive electrode active material layer 22 may also contain various additives such as a binder and a conductive aid used as a material of the positive electrode active material layer.

[0043] The material of the negative electrode collector 31 is not particularly limited, and for example, copper can be used. The material of the negative electrode lead 33 may be the same as that of the negative electrode collector 31, or different from that of the negative electrode collector 31. The negative electrode lead 33 may also be connected integrally with the negative electrode collector 31. In the present embodiment, the negative electrode lead 33 is formed by extending the negative electrode collector 31, and is connected integrally with the negative electrode collector 31. The material of the negative terminal 34 may be the same as that of the negative electrode lead 33, or different from that of the negative electrode lead 33. The negative terminal 34 may also be connected integrally with the negative electrode lead 33. In the present embodiment, the negative terminal 34 and the negative electrode lead 33 may be different components, and are electrically connected to each other.

[0044] The long strip of the long strip separator 40 can be used as an insulating porous membrane 41, and known types such as porous sheets and non-woven fabric sheets used as separators for secondary batteries can be used. Examples of materials for porous sheets include polyolefins such as polyethylene and polypropylene, aramid, polyimide, fluororesins, etc. Examples of materials for non-woven fabric sheets include glass fibers, cellulose fibers, etc. There is no particular restriction on the film thickness of the long strip insulating porous membrane 41, but it is preferably more than 10 μm from the viewpoint of blocking the dendrites of lithium metal, and preferably less than 15 μm from the viewpoint of reducing the resistance in the battery. The film thickness of the long strip insulating porous membrane 41 is more preferably in the range of 10 to 12 μm. Moreover, the air permeability of the long strip insulating porous membrane 41 is not particularly limited, but from the viewpoint of reducing the resistance in the battery, it is preferably less than 200 sec / 100 mL, and more preferably less than 150 sec / 100 mL. The porosity of the long insulating porous film 41 is not particularly limited, but is preferably within a range of 40 to 60% from the viewpoint of uniform diffusion of lithium in the long separator 40 and strength of the long separator 40 .

[0045] The conductive layer 42 of the long strip diaphragm 40 may not be stacked over the entire conductive region 401. Figure 5As shown in FIG. 1 , the conductive layer 42 may be laminated to cover a portion of the hole 41a of the long insulating porous film 41 located in the conductive region 401. The conductivity of the conductive layer 42 is not particularly limited and is within the range of 1.0×10 1 ~1.0×10 5 S / cm. Since the conductivity of the conductive layer 42 is 1.0×10 1 As a result, lithium can be deposited on the surface of the conductive layer 42, which can prevent lithium dendrites from growing toward the positive electrode layer 20 and causing a short circuit. 5 S / cm or less, lithium can be uniformly deposited on the surface of the conductive layer 42 .

[0046] The conductive layer 42 is in electrical contact with either the negative electrode layer 30 or the metallic lithium deposited in the negative electrode layer 30 in both the discharge state and the charge state. As a result, the potential of the conductive layer 42 is the same as the potential of the negative electrode collector 31, so that lithium can be deposited more uniformly between the conductive layer 42 of the long strip separator 40 and the lithium foil 32.

[0047] The conductivity of the conductive layer 42 is lower than that of the negative electrode collector 31, that is, the conductivity of the negative electrode collector 31 may be higher than that of the conductive layer 42. By making the conductivity of the negative electrode collector 31 higher than that of the conductive layer 42, the lithium on the long insulating porous film 41 side of the conductive layer 42 can be prevented from being concentratedly precipitated, and the damage such as the shape change of the conductive layer 42 caused by the concentrated precipitation of lithium can be suppressed. The conductivity of the conductive layer 42 may also be, for example, in the range of 1 / 10 to 1 / 100000 of the conductivity of the negative electrode collector 31.

[0048] The peel strength of the conductive layer 42 relative to the long strip insulating porous membrane 41 is not particularly limited, preferably 10 N / m or more, more preferably 30 N / m or more. When the peel strength of the conductive layer 42 is as high as the above value, the conductive layer 42 can function stably for a long time, so the charge and discharge cycle life becomes longer.

[0049] The surface resistivity of the conductive layer 42 may also be 200Ω / cm 2 the following.

[0050] The thickness of the conductive layer 42 may also be in the range of 0.01 to 5 μm. When the thickness of the conductive layer 42 is 0.01 μm or more, the effect of the conductive layer 42 can be obtained. When the thickness of the conductive layer 42 is 5 μm or less, the decrease in energy density caused by the conductive layer 42 can be reduced.

[0051] Conductive materials such as metals and carbon nanotubes (CNTs) can be used as the material of the conductive layer 42. Examples of metals include Cu, Zn, Ti, and Sn. These conductive materials can be used alone or in combination of two or more.

[0052] There is no particular limitation on the coating method for forming the conductive layer 42 on the long strip-shaped insulating porous film 41, and for example, a sputtering method and a coating method can be used. As the sputtering method, a DC (direct current) sputtering method and an RF (radio frequency) sputtering method can be used. In the coating method, a coating liquid in which the material of the conductive layer 42 is dispersed is applied to the surface of the long strip-shaped insulating porous film 41 and dried.

[0053] The electrolyte contains an organic solvent and an electrolyte. As an organic solvent, for example, cyclic carbonates, chain carbonates, cyclic ethers, chain ethers, hydrofluoroethers, aromatic ethers, sulfones, cyclic esters, chain carboxylates, and nitriles can be used. Examples of cyclic carbonates include ethylene carbonate, propylene carbonate, vinylene carbonate, and fluoroethylene carbonate. Examples of chain carbonates include dimethyl carbonate, diethyl carbonate, and ethyl methyl carbonate. Examples of cyclic ethers include tetrahydrofuran, 2-methyltetrahydrofuran, tetrahydropyran, 1,3-dioxolane, and 4-methyl 1,3-dioxolane. Examples of chain ethers include 1,2-dimethoxyethane, 1,2-diethoxyethane, ethoxymethoxyethane, and diethyl ether. Examples of hydrofluoroethers include 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether, 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether, bis(2,2,2-trifluoroethyl)ether, 1,2-bis(1,1,2,2-tetrafluoroethoxy)ethane, etc. Examples of aromatic ethers include anisole. Examples of sulfones include cyclopentane sulfone, methylcyclopentane sulfone, etc. Examples of cyclic esters include γ-butyrolactone, etc. Examples of chain carboxylates include acetate, butyrate, propionate, etc. Examples of nitriles include acetonitrile, propionitrile, etc. One organic solvent may be used alone, or two or more may be used in combination.

[0054] The electrolyte is a charge transfer medium, i.e., a source of lithium ions, and contains a lithium salt. Examples of lithium salts include LiPF6, LiBF4, LiClO4, LiAsF6, LiCF3sO3, LiC(CF3SO2)3, LiN(CF3SO2)2(LiTFSI), LiN(FSO2)2(LiFSI), and LiBC4O8. A lithium salt may be used alone or in combination of two or more. The concentration of the electrolyte is, for example, in the range of 1.5 to 4.0 mol / L.

[0055] The outer casing 50 can expand and contract as the thickness of the electrode stack 10 (especially the thickness of the negative electrode layer 30) changes due to charge and discharge. As a material for the outer casing 50, a laminated film can be used. As a laminated film, a laminated film having a three-layer structure in which an inner resin layer, a metal layer, and an outer resin layer are laminated in sequence from the inside can be used. As materials for the inner resin layer and the outer resin layer, for example, polyethylene terephthalate (PET), polyamide (nylon), and polypropylene (PP) can be used. As a material for the metal layer, for example, aluminum can be used.

[0056] The secondary battery 100 of the present embodiment can be manufactured by a method including, for example, a long separator manufacturing step, an electrode layer disposing step, a terminal connecting step, an outer body housing step, and a sealing step.

[0057] In the step of preparing the long strip diaphragm, a long strip diaphragm 40 formed by the first fold 43 and the second fold 44 described above being alternately overlapped is prepared. The long strip diaphragm 40 can be prepared by: comprising a long strip insulating porous membrane 41, and a conductive region 401 provided with a conductive layer 42 and arranged on one surface of the long strip insulating porous membrane 41, and a non-conductive region 402 not provided with a conductive layer 42, wherein the conductive region 401 extends along the length direction of the long strip insulating porous membrane 41, and the non-conductive region 402 makes the long strip laminated sheet arranged at at least one end in the width direction of the long strip insulating porous membrane 41 present a meandering shape.

[0058] In the electrode layer configuration step, the positive electrode layer 20 and the first fold 43 are configured to face each other, and the negative electrode layer 30 and the second fold 44 are configured to face each other. By using this step, the electrode laminate 10 is obtained. The positive electrode layer 20 can be configured by inserting the positive electrode layer 20 from the opening 43b of the first fold 43. The negative electrode layer 30 can be configured by inserting the negative electrode layer 30 from the opening 44b of the second fold 44. The long strip separator production step and the electrode layer configuration step can be implemented in parallel. The following operation can also be implemented, for example, after the positive electrode layer 20 is configured on the surface of the long strip insulating porous membrane 41 side of the long strip laminated sheet, the long strip laminated sheet is bent in the length direction in a manner that the surface of the long strip insulating porous membrane 41 side is the inner side, and then, after the negative electrode layer 30 is configured on the surface of the conductive layer 42 side, the long strip laminated sheet is bent in the length direction in a manner that the surface of the conductive layer 42 side is the inner side.

[0059] In the terminal connection step, the positive terminal 24 is connected to the end of the positive electrode layer 20 (positive electrode collector 21) of the electrode stack 10 via the positive electrode lead 23, and the negative terminal 34 is connected to the end of the negative electrode layer 30 (negative electrode collector 31) via the negative electrode lead 33. The positive terminal 24 is connected to the end of the positive electrode layer 20 on the side of the non-conductive region 402 where the long strip separator 40 is arranged. The negative terminal 34 is connected to the end of the negative electrode layer 30 in the direction opposite to the side where the positive terminal 24 is arranged.

[0060] In the outer casing housing step, the electrode laminate 10 connecting the positive electrode terminal 24 and the negative electrode terminal 34 and an electrolyte (not shown) are housed in the outer casing 50 so that a part of the positive electrode terminal 24 and the negative electrode terminal 34 are exposed to the outside.

[0061] In the sealing step, the outer casing 50 accommodating the electrode laminate 10 connecting the positive electrode terminal 24 and the negative electrode terminal 34 and the electrolyte is sealed.

[0062] According to the secondary battery 100 of the present embodiment constructed as described above, the elongated separator 40 has an extension portion 40a extending outward beyond the end of the positive electrode layer 20 on the side connected to the positive electrode terminal 24, so that even if the thickness of the negative electrode layer 30 changes greatly due to charging and discharging, the conductive layer 42 provided at the portion of the elongated separator 40 in contact with the negative electrode layer 30 is not easy to contact the positive electrode layer 20 and the positive electrode lead 23. Therefore, the positive electrode layer 20 and the negative electrode layer 30 are not easy to short-circuit.

[0063] According to the secondary battery 100 of the present embodiment, in the long strip separator 40, the first fold 43 and the second fold 44 are formed alternately and overlapped, the positive electrode layer 20 is located at the first fold 43, and the negative electrode layer 30 is located at the second fold 44, so the positions of the positive electrode layer 20 and the negative electrode layer 30 are not easily offset. In addition, the end of the conductive region 401 on the positive electrode terminal 24 side is closer to the inside than the end of the negative electrode layer 3020 on the positive electrode terminal 24 side, and the end of the extension 40a is the non-conductive region 402, so the conductive layer 42 is not easily in contact with the positive electrode layer 20 and the positive electrode lead 23. In addition, the non-conductive region 402 is only arranged at the end of the long strip separator 40 on the positive electrode terminal 24 side, and the portion other than the end of the extension 40a becomes the conductive region 401, and the contact area between the conductive layer 42 and the negative electrode layer 30 is increased, so that the short circuit caused by dendrites or the decrease in the density of the active material layer of the negative electrode layer in the charged state can be suppressed.

[0064] According to the secondary battery 100 of this embodiment, the end of the positive electrode layer 20 on the opposite side to the side connected to the positive terminal 24 (the side where the negative electrode layer 30 is connected to the negative terminal 34) is closer to the inside than the end of the long strip separator 40. Therefore, the end of the positive electrode layer 20 on the opposite side to the side connected to the positive terminal 24 is less likely to contact the conductive layer 42 of the long strip separator 40.

[0065] Furthermore, the method for manufacturing the secondary battery 100 according to the present embodiment is advantageous for industrially manufacturing the secondary battery 100 .

[0066] As mentioned above, although the preferred embodiment of the present invention has been described, the present invention is not limited to the above-described embodiment, and appropriate changes can be made.

[0067] In the secondary battery 100 of this embodiment, a long strip separator 40 is used, but the separator is not limited thereto. Separator sheets may be respectively interposed between the plurality of positive electrode layers 20 and the negative electrode layers 30. In this case, an extension portion extending outward beyond the end of the positive electrode layer on the side connected to the positive electrode terminal is provided for each separator sheet, and on the surface of the separator sheet on the negative electrode layer side, at least a portion of the portion in contact with the negative electrode layer is set as a conductive region provided with a conductive layer, and at least a portion of the end of the extension portion on the positive electrode terminal side is set as a non-conductive region without a conductive layer.

[0068] Moreover, in the secondary battery 100 of the present embodiment, the negative electrode layer 30 uses the metal lithium layer precipitated during charging as the negative electrode active material layer, but the negative electrode active material layer is not limited to this. As the negative electrode active material layer, a layer containing a negative electrode active material that absorbs lithium during charging and releases lithium during discharge can also be used. As the negative electrode active material, lithium transition metal oxides such as lithium titanate, transition metal oxides such as TiO2, Nb2O3 and WO3, SiO, metal sulfides, metal nitrides, and carbon materials such as artificial graphite, natural graphite, graphite, soft carbon and hard carbon can be used. Moreover, as the negative electrode active material, a metal that can form an alloy with lithium can be used. As examples of metals that can form an alloy with lithium, Mg, Si, Au, Ag, In, Ge, Sn, Pb, Al and Zn can be listed.

[0069] Furthermore, the long strip separator 40 may also have an extension portion extending in the length direction, and the extension portion is wound on the outer side of the electrode stack 10 in a manner such that the surface on the long strip insulating porous membrane 41 side is on the outer side. By winding the extension portion on the outer side of the electrode stack 10, the extension portion applies a restraining force to the electrode stack 10, and the positive electrode layer 20 and the negative electrode layer are less likely to be misaligned.

[0070] [Experimental example]

[0071] The effects of a secondary battery using a laminated body in which a conductive layer is laminated on the surface of an insulating porous membrane as a separator and the conductive layer is arranged on the negative electrode layer side will be described using an experimental example.

[0072] [Experimental Example 1]

[0073] (Production of Diaphragm)

[0074] An insulating porous film (film thickness: 20 μm, porosity: 58%, air permeability: 92 sec / 100 mL) was prepared. A copper conductive layer with a thickness of 0.08 μm was formed on one surface of the insulating porous film by RF sputtering. The insulating porous film with the copper conductive layer was punched into a size of 40 mm×50 mm to serve as a separator.

[0075] (Production of positive electrode layer)

[0076] Acetylene black (AB) as a conductive material, polyvinylidene fluoride (PVDF) as a binder (adhesive), and polyvinyl pyrrolidone (PVP) as a dispersant were pre-mixed in N-methyl-2-pyrrolidone (NMP) as a dispersing solvent, and wet mixed using a rotary mixer to obtain a pre-mixed slurry. Then, Li1Ni 0.8 Co 0.1 Mn 0.1 O2 (NCM811) and pre-doped materials are mixed with the obtained premixed slurry, and a planetary mixer is used for dispersion treatment to obtain a positive electrode active material paste. The median diameter of NCM811 is 12 μm. Next, the obtained positive electrode active material paste is applied to an aluminum positive electrode collector without a primer layer, dried, pressed by a roller press, and dried in a vacuum at 120°C to form a positive electrode plate with a positive electrode active material layer. The obtained positive electrode plate is punched into a size of 30 mm × 40 mm as a positive electrode layer.

[0077] (Production of negative electrode layer)

[0078] Prepare a copper foil with a thickness of 10 μm (conductivity: 6.5×10 6 The coating material was formed by bonding a lithium foil having a thickness of 20 μm to a lithium foil having a thickness of 20 μm. The coating material was punched out into a size of 34 mm×44 mm to serve as a negative electrode current collector.

[0079] (Electrolyte)

[0080] An electrolyte solution was prepared by dissolving LiFSI in 1,2-dimethoxyethane (DME) at a concentration of 4 mol / L.

[0081] (Manufacturing of lithium metal secondary batteries)

[0082] The copper conductive layer of the separator is overlapped on the surface of the lithium foil side of the negative electrode collector, and the positive electrode active material layer of the positive electrode layer is overlapped on the surface on the opposite side of the copper conductive layer side of the separator, so as to produce an electrode laminated body in which the negative electrode layer, the separator, and the positive electrode layer are laminated in sequence. Then, the positive terminal is mounted on the positive electrode collector of the obtained electrode laminated body via the positive electrode lead, and the negative terminal is mounted on the copper foil of the negative electrode collector via the negative electrode lead. The laminated body with the positive terminal and the negative terminal mounted is placed in a laminated film bag, and then an electrolyte is added, and then the laminated film bag is sealed to produce a lithium metal secondary battery.

[0083] [Experimental Example 2]

[0084] A lithium metal secondary battery was produced in the same manner as in Experimental Example 1 except that a 0.06 μm-thick zinc conductive layer was formed by RF sputtering instead of the copper conductive layer in the production of the separator.

[0085] [Experimental Example 3]

[0086] In the preparation of the diaphragm, a conductive layer made of carbon nanotubes (CNT) with a thickness of 2.1 μm was formed by a coating method instead of a conductive layer made of copper. A lithium metal secondary battery was prepared in the same manner as in Experimental Example 1. The carbon nanotube conductive layer was formed as follows. First, N-methyl-N-pyrrolidone (NMP) was used as a solvent, and carbon nanotubes were added in an amount of 4% by weight of a solid content concentration, and PVDF (#9300, manufactured by KUREHA Co., Ltd.) was added as a binder in an amount of 5 parts by weight relative to 95 parts by weight of carbon nanotubes. Next, a dispersion treatment was performed at 1000 rpm for 10 minutes using a rotation-revolution mixer to prepare a coating solution. Using a scraper, the obtained coating solution was applied to the surface of the insulating porous membrane and dried.

[0087] [Experimental Example 4]

[0088] A lithium metal secondary battery was produced in the same manner as in Experimental Example 1 except that a 0.06 μm-thick tin conductive layer was formed by RF sputtering instead of the copper conductive layer in the production of the separator.

[0089] [Comparative Experiment Example 1]

[0090] A lithium metal secondary battery was produced in the same manner as in Experimental Example 1 except that a copper conductive layer was not formed in the production of the separator.

[0091] [evaluate]

[0092] The conductivity, surface resistivity, and peel strength of the conductive layer of the separator produced in each experimental example were measured by the following method. The measurement results are shown in Table 1 together with the material, coating method, and thickness of the conductive layer of the separator.

[0093] The lithium metal secondary batteries prepared in each experimental example and comparative experimental example were measured for the presence or absence of short circuits and the rate of increase in lithium thickness using the following method. The measurement results are shown in Table 1.

[0094] (Conductivity and surface resistivity of conductive layer)

[0095] The conductivity and surface resistivity were measured using a high-precision, high-performance resistivity meter (Nitto Seiko Analytical Science Co., Ltd., Loresta GP TCP-600).

[0096] (Peel Strength)

[0097] A conductive layer of 5.0 cm in length and 2.5 cm in width was crimped onto a 2.5 cm wide adhesive tape, and the adhesive tape was crimped onto a fixed plate. Next, one end of the conductive layer was folded back 180 degrees, and an electric test bench (manufactured by IMADA Co., Ltd.) was used to pull the conductive layer at a speed of 300 mm / min to peel off the conductive layer from the insulating porous membrane. A digital dynamometer (manufactured by IMADA Co., Ltd.) was used to measure the load required from the beginning of the peeling of the conductive layer to the end of the peeling. The value obtained by dividing the average value of the obtained load by the width of the adhesive tape was used as the peel strength.

[0098] (Whether the lithium metal secondary battery has a short circuit)

[0099] The lithium metal secondary battery just produced was left to stand at a measurement temperature of 25° C. for 24 hours.

[0100] For the lithium metal secondary battery after standing, the following first charge and discharge cycle was performed 3 times, and then the following second charge and discharge cycle was performed 50 times to confirm whether the lithium metal secondary battery had a short circuit. When the charge capacity of the lithium metal secondary battery was more than 105% of the discharge capacity before charging, a short circuit was considered to have occurred and was regarded as having a short circuit.

[0101] (1st charge and discharge cycle)

[0102] The charging was performed under the following conditions: constant current charging was performed at a current value of 2.2 mA until the voltage reached 4.300 V, and then constant voltage charging was performed for 60 minutes at a voltage value of 4.300 V. The discharging was performed under the following conditions: constant current discharging was performed at a current value of 4 mA until the voltage reached 2.65 V. The battery was left to stand for 30 minutes between discharging and charging.

[0103] (2nd charge and discharge cycle)

[0104] The charging was performed under the following conditions: constant current charging at a current value of 74 mA to 3.823 V, constant current charging at a current value of 52 mA to 4.051 V, constant current charging at a current value of 46 mA to 4.173 V, constant current charging at a current value of 22 mA to 4.300 V, and then constant voltage charging at a voltage value of 4.300 V for 90 minutes. The discharging was performed under the following conditions: constant current discharge at a current value of 18 mA to 2.65 V. The battery was left to stand for 30 minutes between discharging and charging.

[0105] (Lithium thickness increase rate of lithium metal secondary battery)

[0106] The thickness T1 (μm) of the negative electrode layer during initial charging and the thickness T2 (μm) of the negative electrode layer during charging after 50 cycles (total thickness of the negative electrode collector and the metal lithium layer) were measured, and the lithium thickness increase rate T (μm / cycle) was calculated according to the following formula.

[0107] T (μm / cycle) = (T2-T1) / 50

[0108] The thickness T1 (μm) of the negative electrode layer at the time of initial charge was measured in the following manner.

[0109] The lithium metal secondary battery just produced was left to stand at a measurement temperature of 25° C. for 24 hours.

[0110] The lithium metal secondary battery after standing was subjected to the first charge and discharge cycle described above three times. Then, constant current charging was performed at a current value of 14.7 mA until 4.300 V, and then constant voltage charging was performed at a voltage value of 4.300 V for 60 minutes to charge the lithium metal secondary battery. The charged lithium metal secondary battery was allowed to stand for 30 minutes and then disassembled, the negative electrode layer was taken out, and its thickness was measured as the thickness T1 of the negative electrode layer.

[0111] The thickness T2 of the negative electrode layer during charging after 50 cycles was measured in the following manner.

[0112] The lithium metal secondary battery just produced was left to stand at a measurement temperature of 25° C. for 24 hours.

[0113] After the standing lithium metal secondary battery, the first charge and discharge cycle described above was performed 3 times, and then the second charge and discharge cycle described above was performed 50 times. Then, constant current charging was performed at a current value of 14.7 mA until 4.300 V, and then constant voltage charging was performed at a voltage value of 4.300 V for 60 minutes to charge the lithium metal secondary battery. The charged lithium metal secondary battery was disassembled after standing for 30 minutes, the negative electrode layer was taken out, and its thickness was measured as the thickness T2 of the negative electrode layer.

[0114] [Table 1]

[0115]

[0116] According to Table 1, for the lithium metal secondary batteries in Experimental Examples 1 to 4 having a separator with a conductive layer, short circuits are not likely to occur even if they are repeatedly charged and discharged, the lithium thickness increases at a low rate, and the metal lithium layer (negative electrode active material layer) generated by charging is dense and has a high density. In contrast, in the lithium metal secondary battery of Comparative Experimental Example 1 having a separator without a conductive layer, short circuits are likely to occur if charged and discharged repeatedly, and the lithium thickness increases at a high rate, so a loose negative electrode active material layer with low density is generated by charging.

[0117] Reference numerals

[0118] 10: Electrode laminate

[0119] 20: Positive electrode layer

[0120] 21: Positive electrode collector

[0121] 22: Positive electrode active material layer

[0122] 23: Positive lead

[0123] 24: Positive terminal

[0124] 30: Negative electrode layer

[0125] 31: Negative electrode collector

[0126] 33: Negative lead

[0127] 34: Negative terminal

[0128] 40: Long strip diaphragm

[0129] 40a: extension

[0130] 401: Conductive area

[0131] 402: Non-conductive area

[0132] 41: Long strip insulating porous film

[0133] 41a: hole

[0134] 42: Conductive layer

[0135] 43: The first turn

[0136] 43a: Front End

[0137] 43b: Opening

[0138] 44: The second turn

[0139] 44a: Front End

[0140] 54b: Opening

[0141] 60:Exterior body

[0142] 100: Secondary battery

Claims

1. A secondary battery comprising: An electrode stack having a positive electrode layer, a negative electrode layer, and a separator disposed between the positive electrode layer and the negative electrode layer; Electrolyte; An outer casing, housing the electrode stack and the electrolyte; A positive terminal and a negative terminal are arranged on the outer casing; a positive electrode lead, electrically connecting the positive electrode layer to the positive electrode terminal; and a negative electrode lead, electrically connecting the negative electrode layer to the negative electrode terminal; The separator has an extension portion extending outward beyond the end of the positive electrode layer on the side connected to the positive electrode terminal; On the surface of the separator on the negative electrode layer side, at least a portion of the portion in contact with the negative electrode layer is set as a conductive region provided with a conductive layer, and at least a portion of the end of the extended portion on the positive electrode terminal side is set as a non-conductive region without the conductive layer.

2. The secondary battery according to claim 1, wherein The diaphragm is a long strip diaphragm, comprising a long strip insulating porous membrane, and the conductive region and the non-conductive region arranged on one surface of the long strip insulating porous membrane, the conductive region extending along the length direction of the long strip insulating porous membrane, the non-conductive region arranged at least one end in the width direction of the long strip insulating porous membrane, and the long strip diaphragm is formed by alternating and overlapping a first fold and a second fold, the first fold is bent in the length direction in a manner that the surface on the side of the long strip insulating porous membrane is on the inner side, and the second fold is bent in the length direction in a manner that the surface on the side where the conductive region and the non-conductive region are arranged is on the inner side; The positive electrode layer is sandwiched in the first fold and is located at a position where the non-conductive region becomes the extension portion, and the negative electrode layer is sandwiched in the second fold and is located at a position in contact with the conductive region; The positive electrode terminal is electrically connected to the end of the positive electrode layer on the side where the non-conductive region is arranged; The negative electrode terminal is electrically connected to an end portion of the negative electrode layer on the side opposite to the side where the non-conductive region is arranged.

3. The secondary battery according to claim 1, wherein The end of the conductive region on the positive electrode terminal side is located at the same side as or inside the end of the negative electrode layer on the positive electrode terminal side. 4 . The secondary battery according to claim 1 , wherein the non-conductive region is disposed only at an end portion of the separator on the positive electrode terminal side. 5 . The secondary battery according to claim 1 , wherein the negative electrode active material is metallic lithium.

6. A method for manufacturing a secondary battery, comprising the following steps: A strip-shaped separator is prepared, wherein the strip-shaped separator comprises a strip-shaped insulating porous membrane, and a conductive region provided with a conductive layer and a non-conductive region not provided with a conductive layer, which are arranged on one surface of the strip-shaped insulating porous membrane, wherein the conductive region extends along the length direction of the strip-shaped insulating porous membrane, and the non-conductive region makes the strip-shaped laminated sheet arranged at least at one end in the width direction of the strip-shaped insulating porous membrane present a meandering shape, and the strip-shaped separator is formed by alternatingly overlapping a first fold and a second fold, wherein the first fold is bent in the length direction in a manner that the surface on the side of the strip-shaped insulating porous membrane is on the inner side, and the second fold is bent in the length direction in a manner that the surface on the side where the conductive region and the non-conductive region are arranged is on the inner side; The positive electrode layer and the first fold are arranged to face each other, and the negative electrode layer and the second fold are arranged to face each other; and A positive electrode terminal is connected to the end of the positive electrode layer on the side where the non-conductive region is arranged via a positive electrode lead, and a negative electrode terminal is connected to the end of the negative electrode layer on the opposite side to the side connected to the positive electrode terminal via a negative electrode lead.