Capacitive deionization electrode for treating low-concentration fluorine ion wastewater as well as preparation and application of capacitive deionization electrode

The capacitive deionization system that combines cerium-nitrogen co-modified turbine layered carbon-based materials and carboxyl activated carbon solves the problems of low efficiency and high cost of fluoride ion removal in the existing technology, and achieves efficient adsorption and removal of low-concentration fluorine wastewater. Cycling stability avoids secondary pollution.

CN118745028AActive Publication Date: 2024-10-08NANKAI UNIV

Patent Information

Application Number
CN202411064076.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-10-08
Estimated Expiration
2044-08-05

AI Technical Summary

Technical Problem

Existing water treatment technology has problems such as inconvenient operation, large area, high cost and easy to cause secondary pollution when removing fluoride ions from wastewater. Moreover, the application of carbon-based electrodes in fluoride removal is limited by the lack of active sites in the structure. Dots and carbons have weak physical interactions with fluoride ions.

Method used

The cerium-nitrogen co-modified turbine layered carbon-based material formed by pyrolysis of supramolecular precursor is used as the anode, combined with carboxyl activated carbon as the cathode, to construct an asymmetric capacitive deionization system, and uses the valence control method to increase the unsaturated sites of the material. To improve the adsorption capacity of fluoride ions.

Benefits of technology

It achieves efficient and rapid adsorption of low-concentration fluoride wastewater, shows good fluoride ion selectivity and cycle stability, avoids secondary pollution, and reduces operating costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118745028A_ABST
    Figure CN118745028A_ABST
Patent Text Reader

Abstract

The invention discloses preparation and application of a capacitive deionization electrode for treating low-concentration fluorine ion wastewater, and belongs to the technical field of capacitive deionization. A cerium-nitrogen co-modified turbine layered carbon-based material which is prepared by taking supramolecules as a precursor, forming a carbon skeleton through pyrolysis and then carrying out metal modification control is taken as an anode, carboxyl activated carbon is taken as a cathode, and the cathode and the anode jointly form a capacitive deionization system. The cerium-nitrogen co-modified turbine layered carbon-based material electrode has a layered, loose and controllable mesoporous structure, active sites brought by a large number of unsaturated coordination vacancies and an excellent electric double-layer capacitance behavior. The cerium-nitrogen co-modified turbine layered carbon-based material electrode shows excellent fluorine ion adsorption capacity in low-concentration fluorine-containing wastewater, specifically, the adsorption rate is high, the adsorption capacity is large, and the effluent concentration can reach the relevant standard or below. The capacitive deionization electrode material has a good engineering application prospect in actual sewage treatment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of water treatment and resource utilization technology - the field of capacitive deionization technology, and specifically relates to a capacitive deionization device using a turbine layered carbon-based material loaded with trivalent cerium with abundant unsaturated sites as an anode for efficient adsorption of fluoride ions in wastewater and a preparation method thereof. Background Art

[0002] Fluoride ion (F - ) are widely present in the natural environment, especially in the global water cycle, posing a potential threat to humans and other organisms. They are beneficial to human health at low levels, but can be harmful at high levels. Ingestion of fluoride ions at excessive concentrations by the human body can lead to bone and tooth fluorosis, and in severe cases, even complete loss of bone function, which is extremely harmful to health. According to the World Health Organization (WHO) drinking water quality guidelines, the concentration of fluoride ions in drinking water should be strictly controlled below 1.5 mg / L. With the intensification of industrial wastewater and domestic sewage discharge activities, the fluoride content in the global water cycle is getting higher and higher, and new technologies for wastewater defluoridation are gradually receiving attention and development. At present, ion exchange, electrolysis, adsorption and precipitation methods have been developed and are widely used to remove fluoride ions from wastewater. Adsorption is a commonly used water treatment method that has always attracted the attention of many scholars. It is also one of the most effective and reliable methods for defluoridation. Among them, adsorption materials with excellent adsorption properties are the key factors for efficient defluoridation. Adsorbents have a strong effect on F - The adsorption process of F usually includes three basic steps: (1) - Diffusion or transport from the solution to the outer surface of the adsorbed particle through the boundary layer around the adsorbed particle is called molecular diffusion; (2) F - Adsorbed on the surface of adsorbent particles; (3) F on the surface of adsorbent - The exchange with the substances in the adsorbed particles, or the transfer to the inner surface of the adsorbed particles, is called intraparticle diffusion. The reason why the adsorbent has good adsorption characteristics is mainly because it has a dense pore structure and a huge specific surface area or has groups that can form chemical bonds with the adsorbate. The chemical precipitation method is to add soluble chemicals to the fluoride-containing wastewater, so that it reacts with ionic inorganic pollutants to form fluoride precipitates that are insoluble or difficult to dissolve in water, thereby achieving the purpose of reducing the fluoride content in the water. Coagulation precipitation and chemical precipitation are two commonly used precipitation methods, and are also the most commonly used fluoride removal methods. The principle of the ion exchange method is to use ion exchange resins to selectively remove pollutants from wastewater. While removing the target ions, equivalent ions are also released into the solution to maintain the electrical neutrality of the solution. The ion exchange method for fluoride removal is to react the anions in the ion exchange resin with the F in the water. - Exchange, thereby reducing the F -The membrane treatment method for fluorine removal uses many tiny holes on a special membrane to selectively pass F in the liquid according to the size of the mixture particles. - Membrane treatment mainly includes reverse osmosis, electrodialysis, ultrafiltration and nanofiltration, which is a relatively friendly separation technology. However, these methods all have problems such as inconvenient operation, large footprint, high cost, and easy to cause secondary pollution, which also means that these methods have great defects and obstacles in practical application.

[0003] As an electrosorption method, capacitive deionization has made excellent progress in ion removal applications due to its advantages such as low cost and no secondary pollution. In a typical capacitive deionization process, in a working system, a low energy consumption voltage is applied to two parallel electrodes, and the charged ions are quickly captured by the electrodes carrying the opposite charge, and are enriched through electrode regeneration and wait for further treatment, thereby achieving the separation and removal of ions from the solution. At present, there are few studies on the application of capacitive deionization in fluoride removal, and it may be a potential excellent fluoride removal technology. The performance of the capacitive deionization system is inseparable from the performance of the electrode material. Carbon-based materials have long been concerned and continuously explored and developed due to their rich and diverse morphologies, stable structural properties and excellent conductivity. Capacitive deionization electrodes have achieved remarkable results in seawater desalination. However, the lack of active sites in the structure and the weak double-layer capacitance (EDLC) of the original carbon-based electrode expand the limitations of its ion removal ability, and the carbon and F - The physical interaction between them is also weak. To overcome the known limitations, metal-doped site-modified electrode materials were created and considered an effective strategy to stimulate deionization performance, and various composite electrode technologies were derived, such as Faraday effect metal oxide loading, metal / nitrogen co-doping and bimetallic sensing, which have achieved pioneering achievements in deionization and fluoride removal. There are multiple additional synergistic effects in each of these mechanisms to improve the target performance. Summary of the invention

[0004] In order to solve the above problems, the present invention provides a preparation and application of a capacitive deionization electrode for treating low-concentration fluoride ion wastewater. The capacitive deionization electrode exhibits a large number of unsaturated coordination vacancies, exhibits large capacity and fast rate adsorption of fluoride ions in low-concentration fluoride wastewater, and achieves good fluoride ion selectivity.

[0005] The present invention also provides a preparation method of the electrode material and its application effect in treating fluorine wastewater.

[0006] Preparation of capacitive deionization electrode for treating low-concentration fluoride ion wastewater, using supramolecule as precursor, cerium-nitrogen co-modified turbo-layered carbon-based material prepared by pyrolysis to form a carbon skeleton and then metal modification control as anode, carboxyl activated carbon as cathode, cathode and anode together constitute a capacitive deionization system;

[0007] The preparation method of the cerium-nitrogen co-modified turbine layered carbon-based material of the capacitor deionization anode material is as follows:

[0008] 1) at 25° C., dissolving 2-2.5 g of 1,2,4,5-benzenetetracarboxylic acid and 1-2 g of melamine in 80-120 ml of distilled water, stirring for 8-12 hours, semi-sealing the resulting solution in a 100-120° C. forced air drying oven for 22-26 hours, then raising the drying oven temperature by 8-12° C. for 6-10 hours, and finally completely drying the resulting semi-solid to obtain a precursor;

[0009] 2) The precursor is sent into a tube furnace and heated at 1-10°C min in a nitrogen environment. -1 After heating to 800-1100°C at a heating rate of 1-3 hours, the carbon-based skeleton is washed with deionized water and dried to obtain a carbon-based skeleton; the carbon-based skeleton (0.1-0.3 g) is dispersed in distilled water (10-50 ml), and then cerium nitrate hexahydrate (0.8-1.2 g) is added, followed by immediate stirring for 0.5-2 hours, and then ultrasonic treatment for 10-50 minutes. The pH value of the resulting mixture is adjusted to 11-13 with potassium hydroxide, and then stirred for another 1-3 hours, and then the sample is washed three times with distilled water and dried. The resulting solid is sent to a muffle furnace at 1-10°C min -1 After heating to 800-1100°C at a heating rate of 1-5 hours, washing with deionized water and drying, the obtained product is a cerium-nitrogen co-modified turbine layered carbon-based material.

[0010] The preparation method of the electrode is as follows:

[0011] 1) For the anode, cerium-nitrogen co-modified turbo-layered carbon-based material, conductive carbon black and polytetrafluoroethylene were ground and mixed at 80%, 10% and 10% by mass, respectively, and ultrasonicated for 8-12 minutes to obtain a slurry. The slurry was evenly dripped and coated on graphite paper, then dried at 60-100°C for 2-8 hours, and finally made into an electrode. At the same time, carboxyl activated carbon was selected as the cathode material, and the cathode was prepared using the same steps;

[0012] 2) The obtained slurry is evenly pressed on graphite paper by a rolling method, and then dried at 60-100° C. for 2-8 hours to finally form an electrode;

[0013] 3) Selecting carboxyl activated carbon as the cathode material, the cathode was prepared using the same steps;

[0014] The construction method of the capacitive deionization device is as follows:

[0015] 1) Our CDI system uses an asymmetric electrode, using cerium-nitrogen co-modified turbo-layered carbon-based materials as the anode to capture fluoride ions, and carboxyl activated carbon as the cathode for adsorption and desorption experiments;

[0016] 2) In the adsorption experiment, sodium fluoride solution was added to the CDI reactor, and a voltage of 1.0-1.4V was applied to the two electrodes of the battery. The adsorption time of each group of experiments was 100-140min, and samples were collected every 10-20 minutes, with 0.5mL of solution taken each time;

[0017] 3) After the adsorption is completed, the applied voltage is changed to -1.0-1.4V, the desorption time is about 100-140min, and the desorbed electrode is immersed in deionized water for standby use.

[0018] The present invention uses a self-assembly method to achieve the synthesis of a structurally ordered turbine layered carbon-based material, and uses a valence state control method to load the carbon-based material with a large amount of trivalent cerium having abundant unsaturated sites, thereby preparing a cerium-nitrogen co-modified turbine layered carbon-based material with loose and porous mesoporous channels that are conducive to rapid ion diffusion.

[0019] The advantages and effects of the present invention are:

[0020] The supermolecule synthesized from pyrophthalic acid and melamine is used as a precursor, the precursor is pyrolyzed to obtain a turbine layered carbon-based material, and the loading of trivalent cerium on the carbon base is controlled to prepare a cerium-nitrogen co-modified turbine layered carbon-based material. The prepared cerium-nitrogen co-modified turbine layered carbon-based material is a carbon-based material with uniform particle size and regular laminar fluid shape, showing good diffusivity and dispersibility. Controlling the valence state of the loaded cerium improves the overall adsorption potential of the material, and there are a large number of active oxygen vacancies. In addition, when the present invention is used as the anode of the CDI electrode, the double electric layer effect is obvious, the specific capacitance is good, it has a strong electrical adsorption performance, and it can be used for low-concentration fluoride wastewater.

[0021] In 10 mg / L sodium fluoride solution, at a voltage of 1.2 V, the CDI system using cerium-nitrogen co-modified turbolayered carbon-based materials as the electrode anode exhibited an excellent fluoride ion adsorption capacity of 1.23 mmol / g.

[0022] In order to verify the above-mentioned unique structural engineering design, the electrode material of the present invention was characterized by XPS and SEM, and the feasibility of the structure, the effectiveness of the synthesis and the real existence of the chemical composition were proved from the aspects of component content and microstructure. In addition, in the control experiments with different reaction conditions, the electrosorption behavior was affected by factors such as pH and interfering ions. The conditional experiments provided a large amount of data for analyzing the ability of the electrode to remove fluoride ions, and the adsorption kinetics simulation provided a theoretical basis for analyzing the solute distribution and mass transfer process, so as to further explore the electrosorption mechanism of the turbine layered carbon-based material. In addition, the cyclic stability of the invented electrode material was also studied and proved to have good cyclic stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is a schematic diagram of the valence state controlled method for synthesizing materials.

[0024] Figure 2 This is a scanning electron microscope image of a cerium-nitrogen co-modified turbine layered carbon-based material electrode.

[0025] Figure 3 It is a cyclic voltammetry test curve that represents the capacitance contribution ratio during the operation of the material electrode.

[0026] Figure 4 This is an analysis chart showing the abundance of oxygen vacancies in the material as proven by X-ray photoelectron spectroscopy experiments.

[0027] Figure 5 This is the adsorption capacity diagram of cerium-nitrogen co-modified turbine layered carbon-based materials for different interfering ions, different initial pH, different initial voltage, and different test concentrations.

[0028] Figure 6 This is a graph showing the fitting results of the material electrode adsorption experiment using pseudo-first-order, pseudo-second-order adsorption kinetics and adsorption isotherm models.

[0029] Figure 7 This is the cycle stability diagram showing that 75% of the initial adsorption capacity is still maintained after 20 cycle experiments. DETAILED DESCRIPTION

[0030] The following non-limiting embodiments may enable a person skilled in the art to more fully understand the present invention, but are not intended to limit the present invention in any way.

[0031] Example 1

[0032] Preparation of Ce-N co-modified turbo-layered carbon-based materials:

[0033] At 25°C, 2.287 g of 1,2,4,5-benzenetetracarboxylic acid and 1.513 g of melamine were dissolved in 100 ml of distilled water and stirred for 10 hours. The resulting solution was semi-sealed in a 110°C forced air drying oven for 24 hours, and then the drying oven temperature was increased by 10°C for 8 hours. Finally, the resulting semi-solid was completely dried to obtain a precursor. The precursor was sent to a tube furnace and heated at 5°C min in a nitrogen environment. -1 After heating to 900°C at a heating rate of 2 hours, the carbon-based skeleton was washed with deionized water and dried to obtain a carbon-based skeleton. The carbon-based skeleton (0.2 g) was dispersed in distilled water (30 ml), and then cerium nitrate hexahydrate (1.0 g) was added, followed by immediate stirring for 1 hour and then ultrasonic treatment for 30 minutes. The pH value of the resulting mixture was adjusted to 12 with potassium hydroxide, and then stirred for another 2 hours, then washed three times with distilled water and dried. The resulting solid was sent to a muffle furnace and heated at 5°C min -1 After being heated to 900°C at a heating rate of 300°C for 3 hours, the product is washed with deionized water and dried, and the obtained product is a cerium-nitrogen co-modified turbine layered carbon-based material.

[0034] Electrode preparation and device construction:

[0035] For the anode, cerium-nitrogen co-modified turbo-layered carbon-based material, conductive carbon black and polytetrafluoroethylene were ground and mixed at 80%, 10% and 10% respectively, and ultrasonicated for 10 minutes to obtain a slurry. The obtained slurry was rolled on graphite paper by rolling method, and then dried at 80 ° C for 4 hours to finally make an electrode. At the same time, activated carbon activated by carboxyl group was selected as the cathode material, and the cathode was prepared using the same steps.

[0036] Our CDI system uses an asymmetric electrode, using cerium-nitrogen co-modified turbo-layered carbon-based materials as the anode to capture fluoride ions, and carboxyl activated carbon as the cathode for adsorption and desorption experiments. In the adsorption experiment, sodium fluoride solution was added to the CDI reactor, and a voltage of 1.2V was applied to the two electrodes of the battery. The adsorption time for each group of experiments was 120 minutes, and samples were collected every 15 minutes, with 0.5mL of solution taken each time. After the adsorption was completed, the applied voltage was changed to -1.2V, the desorption time was about 120 minutes, and the electrode after desorption was soaked in deionized water for use.

[0037] Example 2

[0038] Electrosorption performance test:

[0039] The electrosorption experiment was carried out in a 10 mg / L sodium fluoride solution. All condition experiments used cerium-nitrogen co-modified turbo-layered carbon-based materials as the anode and carboxyl activated carbon as the cathode. When sampling, 0.5 mL of solution was taken each time, and the fluoride ion content was detected by ion chromatography.

[0040] In order to analyze the influence of common interfering ions in water bodies on the adsorption of fluoride ions by cerium-nitrogen co-modified turbine layered carbon-based materials, chloride ions, nitrate ions, sulfate ions and bicarbonate ions at the same concentration were added to 10 mg / L sodium nitrate solution, so as to have a deeper understanding of the selectivity of cerium-nitrogen co-modified turbine layered carbon-based materials for fluoride ions.

[0041] The fluoride ion electrosorption capacity of the fabricated electrode was calculated as follows:

[0042]

[0043] Where Qe (mg / g) refers to the fluoride ion electrical adsorption capacity within a certain period of time, C0 (mg / L) and Ce (mg / L) represent the fluoride ion concentrations at the initial time and time t, respectively, m (g) is the weight of the electrode material, and V (mL) represents the volume of the solution at that time.

[0044] The calculation method of fluoride ion electrosorption rate is as follows:

[0045]

[0046] Where Vt (mg / g / min) refers to the nitrate electrical adsorption rate, Qe (mg / g) refers to the fluoride ion electrical adsorption capacity within a certain period of time, and t (min) is the reaction time.

[0047] Example 3

[0048] Adsorption kinetics simulation

[0049] The pseudo first-order, pseudo second-order adsorption kinetics and adsorption isotherm models were used to numerically fit the material electrode adsorption experiment to explore the dominant factors and adsorption patterns of the adsorption process and to analyze the adsorption process more deeply. The adsorption isotherm models used were the Langmuir adsorption isotherm model and the Friedrich adsorption isotherm model.

[0050] The present invention has been described in detail above in conjunction with the embodiments, but the present invention is not limited to the above embodiments, and various changes can be made within the knowledge scope of ordinary technicians in the relevant technical field without departing from the purpose of the present invention.

Claims

1. A preparation of a capacitive deionization electrode for treating low-concentration fluoride ion wastewater, using supramolecules as precursors, cerium-nitrogen co-modified turbo-layered carbon-based materials prepared by pyrolysis to form a carbon skeleton and then metal modification control as the anode, carboxyl activated carbon as the cathode, and the cathode and anode together constitute a capacitive deionization system; The preparation method of the cerium-nitrogen co-modified turbine layered carbon-based material of the capacitor deionization anode material is as follows: 1) at 25° C., dissolving 2-2.5 g of 1,2,4,5-benzenetetracarboxylic acid and 1-2 g of melamine in 80-120 ml of distilled water, stirring for 8-12 hours, semi-sealing the resulting solution in a 100-120° C. forced air drying oven for 22-26 hours, then raising the drying oven temperature by 8-12° C. for 6-10 hours, and finally completely drying the resulting semi-solid to obtain a precursor; 2) The precursor is sent into a tube furnace and heated at 1-10°C min in a nitrogen environment. -1 After heating to 800-1100°C at a heating rate of 1-3 hours, washing with deionized water and drying can obtain a carbon-based skeleton; 0.1-0.3 g of the carbon-based skeleton is dispersed in 10-50 ml of distilled water, and then 0.8-1.2 g of cerium nitrate hexahydrate is added, followed by immediate stirring for 0.5-2 hours, and then ultrasonic treatment for 10-50 minutes; the pH value of the resulting mixture is adjusted to 11-13 with potassium hydroxide, and then stirred for another 1-3 hours, and then washed with distilled water three times and dried; the resulting solid is sent to a muffle furnace and heated at 1-10°C min -1 After heating to 800-1100°C at a heating rate of 1-5 hours, washing with deionized water and drying, the obtained product is a cerium-nitrogen co-modified turbine layered carbon-based material; The preparation method of the electrode is as follows: 1) For the anode, cerium-nitrogen co-modified turbo-layered carbon-based material, conductive carbon black and polytetrafluoroethylene were ground and mixed at 80%, 10% and 10% by mass, respectively, and ultrasonicated for 8-12 minutes to obtain a slurry. The slurry was evenly dripped and coated on graphite paper, and then dried at 60-100°C for 2-8 hours to finally make an electrode; at the same time, carboxyl activated carbon was selected as the cathode material, and the cathode was prepared using the same steps; 2) The obtained slurry is evenly pressed on graphite paper by a rolling method, and then dried at 60-100° C. for 2-8 hours to finally form an electrode; 3) Selecting carboxyl activated carbon as the cathode material, the cathode was prepared using the same steps; The construction method of the capacitive deionization device is as follows: 1) Our CDI system uses an asymmetric electrode, using cerium-nitrogen co-modified turbo-layered carbon-based materials as the anode to capture fluoride ions, and carboxyl activated carbon as the cathode for adsorption and desorption experiments; 2) In the adsorption experiment, sodium fluoride solution was added to the CDI reactor, and a voltage of 1.0-1.4V was applied to the two electrodes of the battery. The adsorption time of each group of experiments was 100-140min, and samples were collected every 10-20 minutes, with 0.5mL of solution taken each time; 3) After the adsorption is completed, the applied voltage is changed to -1.0-1.4V, the desorption time is about 100-140min, and the desorbed electrode is immersed in deionized water for standby use.

2. A capacitive deionization electrode for treating low-concentration fluoride ion wastewater, characterized in that: The electrode is prepared by the method according to claim 1.

3. An application of a capacitive deionization electrode prepared by the method according to claim 2 for treating low-concentration fluoride ion wastewater, characterized in that: Capacitors used to treat low concentration fluoride ion wastewater.

Citation Information

Patent Citations

  • Electrochemistry fluoride removing device

    CN208054987U

  • Porous carbon materials comprising a carbon additive

    WO2024073165A1

  • Cerium oxide sulfur-doped carbon aerogel microsphere, preparation method therefor and application thereof

    WO2024108743A1

  • KR20200121100A

Cited By

  • Mesoporous electro-adsorption defluorination positive electrode material rich in defects after vulcanization reconstruction

    CN119409294A