Crown ether compound, rechargeable battery electrolyte and rechargeable battery

By using crown ether-based compounds as electrolyte additives in lithium metal batteries, the problems of dendrites and side reactions are solved, the cycle stability and kinetic performance of the battery are improved, the electrolyte consumption is reduced, and the battery is realized under high voltage conditions. long cycle stability.

CN118745164AActive Publication Date: 2024-10-08HAIKOU QIANMU CONSULTING SERVICE CO LTD

Patent Information

Application Number
CN202410727620.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-06
Publication Date
2024-10-08
Estimated Expiration
2044-06-06

AI Technical Summary

Technical Problem

Lithium metal batteries often face problems such as dendrite formation and frequent side reactions during the cycle process, resulting in poor cycle stability and safety hazards. In the existing technology, there are few types of electrolyte additives, complex preparation, and high costs.

Method used

Crown ether-based compounds are used as electrolyte additives. They are adsorbed on the surfaces of the positive and negative electrodes through their strong cation coordination capabilities, forming an interface film with fast ion conductivity, regulating the uniformity of metal ion distribution at the interface, and suppressing side reactions.

Benefits of technology

It significantly improves the kinetic performance and cycle life of the battery, reduces the consumption of electrolyte, and achieves long-term cycle stability of the battery under high voltage conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118745164A_ABST
    Figure CN118745164A_ABST
Patent Text Reader

Abstract

The invention relates to a crown ether compound, a rechargeable battery electrolyte and a rechargeable battery, the rechargeable battery electrolyte is composed of a rechargeable battery electrolyte body and an electrolyte additive, the electrolyte additive is a crown ether compound represented by a formula (i) or a formula (ii): # imgabs0 # rechargeable battery electrolyte contains the electrolyte additive, an electrode and the electrolyte can be effectively isolated, the service life of the rechargeable battery is prolonged, the service life of the rechargeable battery is prolonged, the service life of the rechargeable battery is prolonged, and the service life of the rechargeable battery is prolonged. Therefore, side reaction between the electrolyte and the positive and negative electrodes of the battery is inhibited, the dynamic performance of the battery is improved, the consumption of the electrolyte is reduced, and the cycle life of the battery is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of metal batteries, and in particular to a crown ether compound, a rechargeable battery electrolyte and a rechargeable battery. Background Art

[0002] Lithium metal batteries have attracted much attention due to their high energy density, high operating voltage, no memory effect, long cycle life, no pollution, light weight and low self-discharge, etc. However, during the cycle, lithium metal batteries often face the problems of dendrite formation and frequent side reactions, resulting in poor cycle stability and safety hazards.

[0003] In order to solve these problems, related technologies have proposed a variety of improvement strategies, such as liquid electrolyte modification, construction of solid and quasi-solid electrolytes, design of interface protective films, and construction of three-dimensional conductive skeletons, thereby significantly improving the cycle performance of lithium metal batteries. Among them, the liquid electrolyte modification method is simple, does not change the existing process, has good practical prospects, and during the cycle, the electrolyte directly contacts the positive and negative electrodes; through electrolyte modification, a dense protective film can be constructed at the interface of the positive and negative electrodes at the same time, effectively isolating the electrodes and the electrolyte, while reducing side reactions, which has greater advantages. Therefore, the present application discloses an electrolyte additive for high-voltage lithium metal batteries, which can effectively solve the problems of dendrite formation and positive and negative electrode side reactions, and provide good long-cycle stability under high voltage conditions. It is simple to prepare, low cost, and suitable for various lithium metal electrolytes. Summary of the invention

[0004] Based on the above-mentioned technical problems, the present invention provides a crown ether compound, a rechargeable battery electrolyte and a rechargeable battery, which are used to solve the technical problems of the existing rechargeable battery organic electrolyte additives being few in variety, complex in preparation and high in cost.

[0005] To achieve the above object, according to one aspect of the present invention, the present invention provides a crown ether compound used as an electrolyte additive, which has a chemical structure shown in formula (i) or formula (ii):

[0006]

[0007] The crown ether compound of formula (i) can be synthesized by the synthesis routes shown in the following equations (1) and (2), and the crown ether compound of formula (ii) can be synthesized by the synthesis routes shown in the following equations (1) and (3):

[0008]

[0009] In the above formula (2), the -Br of the compound containing -Br may also be other halogen groups; in the above formula (3), the -I of the compound containing -I may also be other halogen groups.

[0010] According to another aspect of the present invention, the present invention further provides a rechargeable battery electrolyte, which is composed of a rechargeable battery electrolyte main solution and an electrolyte additive, wherein the electrolyte additive is the above-mentioned crown ether-based compound.

[0011] As a further preferred technical solution of the present invention, the rechargeable battery electrolyte is one of ester electrolyte, ether electrolyte, nitrile electrolyte, sulfone electrolyte, aqueous electrolyte, mixed electrolyte, and ionic liquid electrolyte.

[0012] As a further preferred technical solution of the present invention, the ratio of the mass of the electrolyte additive to the volume of the rechargeable battery electrolyte is 0.01-100g:1L.

[0013] According to another aspect of the present invention, the present invention further provides a rechargeable battery, which uses the above-mentioned rechargeable battery electrolyte.

[0014] As a further preferred technical solution of the present invention, the rechargeable battery is one of a metal lithium / lithium ion battery, a metal sodium / sodium ion battery, a metal potassium / potassium ion battery, a metal magnesium / magnesium ion battery, a metal aluminum / aluminum ion battery, a metal zinc / zinc ion battery, and an iron battery.

[0015] Compared with the prior art, the present invention can achieve the following beneficial effects:

[0016] The crown ether-based compound of the present invention is used as an electrolyte additive, and it uses 15-crown ether-5 with strong cation coordination ability as a structural mother core, thereby ensuring that the additive molecule has a strong coordination center, and can be adsorbed on the positive and negative electrode surfaces to coordinate and complex with a large number of lithium ions and participate in the generation of CEI and SEI interface films of fast ion conduction; by modifying the 15-crown ether-5 mother core with different substituents through side chain engineering, the uniformity of the accumulation of the additive molecule at the positive and negative electrode interfaces and the efficiency and stability of film formation can be effectively regulated, thereby regulating the uniformity of the distribution of metal ions at the interface, and effectively inhibiting the microstructural phase change of the positive electrode active material and the growth of the negative electrode metal dendrite. Therefore, the rechargeable battery electrolyte using the electrolyte additive of the present invention can effectively isolate the electrode and the electrolyte, thereby inhibiting the side reactions of the electrolyte and the positive and negative electrodes of the battery, so that the kinetic performance of the battery is improved and the consumption of the electrolyte is reduced, and the battery cycle life is improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] The present invention will be further described in detail below in conjunction with the accompanying drawings and specific embodiments.

[0018] Figure 1-1The cycling curves of Li / Al batteries assembled with blank ester LiPF6 electrolyte and modified electrolytes containing 15-crown ether-5, alkyl chain 15-crown ether-5, and sulfonic acid 15-crown ether-5, respectively.

[0019] Figure 1-2 The cycling curves of Li / Li batteries assembled with blank ester LiPF6 electrolyte and modified electrolytes containing 15-crown ether-5, alkyl chain 15-crown ether-5, and sulfonic acid 15-crown ether-5, respectively.

[0020] Figure 1-3 Performance test diagrams of lithium manganese oxide / Li batteries assembled with blank ester LiPF6 electrolyte and modified electrolytes containing 15-crown ether-5, alkyl chain 15-crown ether-5, and sulfonic acid 15-crown ether-5, respectively.

[0021] Figure 2-1 The cycling curves of Li / Al batteries assembled with blank ester LiPF6 electrolyte and modified electrolytes containing 15-crown ether-5, alkyl chain 15-crown ether-5, and fluorinated 15-crown ether-5, respectively.

[0022] Figure 2-2 The cycling curves of Li / Li batteries assembled with blank ester LiPF6 electrolyte and modified electrolytes containing 15-crown ether-5, alkyl chain 15-crown ether-5, and fluorinated 15-crown ether-5, respectively.

[0023] Figure 2-3 Performance test diagrams of lithium manganese oxide / Li batteries assembled with blank ester LiPF6 electrolyte and modified electrolytes containing 15-crown ether-5, alkyl chain 15-crown ether-5, and fluorinated 15-crown ether-5, respectively.

[0024] The purpose, features and advantages of the present invention will be further described with reference to the accompanying drawings in conjunction with the embodiments. DETAILED DESCRIPTION

[0025] The specific implementation of the present invention is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described here is only used to illustrate and explain the present invention, and is not used to limit the present invention.

[0026] Unless otherwise defined, the technical terms used in the following examples have the same meanings as those generally understood by those skilled in the art to which the present invention belongs. The test reagents used in the following examples, unless otherwise specified, are all conventional biochemical reagents; the experimental methods, unless otherwise specified, are all conventional methods.

[0027] Embodiment 1:

[0028] This embodiment provides a method for preparing a rechargeable battery electrolyte containing a sulfonic acid 15-crown ether-5 electrolyte additive (hereinafter referred to as a modified electrolyte), comprising the following steps:

[0029] Dissolve 0.5 g of sulfonic acid 15-crown ether-5 in 1 L of rechargeable battery electrolyte to prepare a rechargeable battery electrolyte; the rechargeable battery electrolyte used contains 1 mol / L of LiPF 6 The solvent is dimethyl carbonate, ethyl methyl carbonate and ethylene carbonate in a volume ratio of 1:1:1. The rechargeable battery electrolyte is also called ester LiPF in the following experiments. 6 Electrolyte.

[0030] In addition, as a control experiment of Example 1, the preparation method of Example 1 was referred to, and 15-crown ether-5 and alkyl chain 15-crown ether-5 were used to replace sulfonic acid 15-crown ether-5 in equal amounts to prepare a modified electrolyte containing 15-crown ether-5 and a modified electrolyte containing alkyl chain 15-crown ether-5.

[0031] The chemical structures of the above-mentioned 15-crown ether-5, alkyl chain 15-crown ether-5 and sulfonic acid 15-crown ether-5 are:

[0032]

[0033] In order to study the addition of sulfonic acid 15-crown ether-5-ester LiPF 6 The influence of electrolyte performance, this embodiment carries out the following three experiments:

[0034] Experiment 1-1

[0035] Assemble four identical Li / Al button-type symmetrical mold full cells (lithium foil diameter is 1 cm) and load 0.1 mL of ester LiPF into each of the four mold full cells. 6 The electrolyte (marked as blank), 0.1 mL of a modified electrolyte containing 15-crown ether-5 (marked as control 1), 0.1 mL of a modified electrolyte containing an alkyl chain 15-crown ether-5 (marked as control 2), and 0.1 mL of a modified electrolyte containing sulfonic acid 15-crown ether-5 prepared in Example 1 (marked as sulfonic acid additive); the cycle stability of the four batteries was then tested at a current density of 0.5 mV / s, and the results are shown in FIG. Figure 1-1 shown.

[0036] According to Figure 1, compared with the blank ester LiPF 6Compared with the Li / Al battery assembled with the modified electrolyte containing 15-crown ether-5 and the modified electrolyte containing alkyl chain 15-crown ether-5, the voltage of the Li / Al battery with the modified electrolyte containing sulfonic acid 15-crown ether-5 in Example 1 can be stabilized to above 5.0V, indicating that the blank ester LiPF 6 Adding sulfonic acid 15-crown ether-5 to the electrolyte can significantly improve the high voltage stability of the electrolyte, and is significantly better than the modified electrolyte formed by adding 15-crown ether-5 (control 1) or alkyl chain 15-crown ether-5 (control 2).

[0037] Experiment 1-2

[0038] Four identical Li / Li button-type symmetrical mold full cells (lithium foil diameter of 1 cm) were assembled, and 0.1 mL of ester LiPF6 electrolyte (marked as blank), 0.1 mL of modified electrolyte containing 15-crown ether-5 (marked as control 1), 0.1 mL of modified electrolyte containing alkyl chain 15-crown ether-5 (marked as control 2), and 0.1 mL of modified electrolyte containing sulfonic acid 15-crown ether-5 prepared in Example 1 (marked as sulfonic acid additive) were respectively loaded into the four mold full cells; then the cycle stability of the four batteries was tested at a surface loading of 1 mAh·cm-2 and a current density of 2 mA·cm-2, and the results were as follows: Figure 1-2 shown.

[0039] according to Figure 1-2 It can be seen that compared with the Li / Li battery assembled with a blank ester electrolyte, a modified electrolyte containing 15-crown ether-5, and a modified electrolyte containing an alkyl chain 15-crown ether-5, the stable cycle time of the Li / Li battery containing a sulfonic acid 15-crown ether-5 modified electrolyte is increased from 30 h to more than 300 h, indicating that the addition of sulfonic acid 15-crown ether-5 to the ester electrolyte can significantly improve the cycle stability of the Li / Li battery, and is significantly better than the modified electrolyte formed by adding 15-crown ether-5 (control 1) or alkyl chain 15-crown ether-5 (control 2).

[0040] Experiments 1-3

[0041] Assemble four identical lithium nickel manganese oxide / Li full batteries (positive electrode sheet diameter is 1 cm, lithium nickel manganese oxide surface loading is 1.2 mg cm -2 , lithium foil diameter 1 cm), 0.1 mL of ester LiPF was loaded into each of the four mold full batteries. 6The electrolyte (marked as blank), 0.1 mL of a modified electrolyte containing 15-crown ether-5 (marked as control 1), 0.1 mL of a modified electrolyte containing an alkyl chain 15-crown ether-5 (marked as control 2), and 0.1 mL of a modified electrolyte containing sulfonic acid 15-crown ether-5 prepared in Example 1 (marked as sulfonic acid additive); then the cycle stability, capacity and retention rate of the four batteries were tested at a current density of 2C, and the results were as follows: Figure 1-3 shown.

[0042] according to Figure 1-3 It can be seen that at an ultra-high current density of 2C, the capacity of the lithium nickel manganese oxide / Li battery containing the sulfonic acid 15-crown ether-5 modified electrolyte is higher than that of the blank ester LiPF 6 The capacity of the lithium nickel manganese oxide / Li battery of the electrolyte and the two control groups increased by nearly 20mAh / g; the blank ester LiPF 6 The capacity of the LiMnO2 / Li battery with modified electrolyte showed a decreasing trend from the beginning of the cycle, and the capacity was only 27 mAh / g after 800 cycles. However, the capacity of the LiMnO2 / Li battery with modified electrolyte containing sulfonic acid 15-crown ether-5 was stable after 800 cycles with little attenuation. It can be seen that the cycle stability, capacity and retention rate of the LiMnO2 / Li battery with modified electrolyte containing sulfonic acid 15-crown ether-5 were significantly improved, indicating that the ester LiPF 6 Adding sulfonic acid 15-crown ether-5 to the electrolyte can significantly improve the coulombic efficiency, cycle stability, capacity and retention rate of the battery.

[0043] Embodiment 2:

[0044] This embodiment provides a method for preparing a rechargeable battery electrolyte containing a fluorinated 15-crown ether-5 electrolyte additive (hereinafter referred to as a modified electrolyte), comprising the following steps:

[0045] Dissolve 0.5 g of fluorinated 15-crown ether-5 in 1 L of rechargeable battery electrolyte to prepare a rechargeable battery electrolyte; the rechargeable battery electrolyte used contains 1 mol / L of LiPF 6 The solvent is dimethyl carbonate, ethyl methyl carbonate and ethylene carbonate in a volume ratio of 1:1:1. The rechargeable battery electrolyte is also called ester LiPF in the following experiments. 6 Electrolyte.

[0046] In addition, as a control experiment of Example 1, the preparation method of Example 1 was referred to, and 15-crown ether-5 and alkyl chain 15-crown ether-5 were used to replace the fluorinated 15-crown ether-5 in equal amounts to prepare a modified electrolyte containing 15-crown ether-5 and a modified electrolyte containing alkyl chain 15-crown ether-5.

[0047] The chemical structures of the above-mentioned 15-crown ether-5, alkyl chain 15-crown ether-5 and fluorinated 15-crown ether-5 are:

[0048]

[0049] In order to study the effect of adding fluorinated 15-crown ether-5 on the performance of ester LiPF6 electrolyte, the following three experiments were conducted in this example:

[0050] Experiment 2-1

[0051] Assemble four identical Li / Al button-type symmetrical mold full cells (lithium foil diameter is 1 cm) and load 0.1 mL of ester LiPF into each of the four mold full cells. 6 The electrolyte (marked as blank), 0.1 mL of a modified electrolyte containing 15-crown ether-5 (marked as control 1), 0.1 mL of a modified electrolyte containing an alkyl chain 15-crown ether-5 (marked as control 2), and 0.1 mL of a modified electrolyte containing fluorinated 15-crown ether-5 prepared in Example 2 (marked as fluorine-based additive); the cycle stability of the four batteries was then tested at a current density of 0.5 mV / s, and the results were Figure 2-1 shown.

[0052] According to Figure 1, compared with the blank ester LiPF 6 Compared with the Li / Al battery containing the electrolyte modified by control 1 and control 2, the voltage of the Li / Al battery containing the fluorine-based 15-crown ether-5 modified electrolyte can be stabilized to above 5.0V, indicating that the blank ester LiPF 6 Adding fluorinated 15-crown ether-5 into the electrolyte can significantly improve the high voltage stability of the electrolyte, and is better than control 1 and control 2.

[0053] Experiment 2-2

[0054] Four identical Li / Li button-type symmetrical mold full cells (lithium foil diameter of 1 cm) were assembled, and 0.1 mL of ester LiPF6 electrolyte (marked as blank), 0.1 mL of modified electrolyte containing 15-crown ether-5 (marked as control 1), 0.1 mL of modified electrolyte containing alkyl chain 15-crown ether-5 (marked as control 2), and 0.1 mL of modified electrolyte containing fluorinated 15-crown ether-5 prepared in Example 2 (marked as fluorine-based additive) were respectively loaded into the four mold full cells; then the cycle stability of the four batteries was tested at a surface loading of 1 mAh·cm-2 and a current density of 2 mA·cm-2, and the results were as follows: Figure 2-2 shown.

[0055] according to Figure 2-2It can be seen that compared with the Li / Li batteries containing blank ester electrolyte and control 1 and control 2, the stable cycle time of the Li / Li battery containing fluorinated 15-crown ether-5 modified electrolyte is increased from 30h to more than 300h, indicating that the addition of fluorinated 15-crown ether-5 to the ester electrolyte can significantly improve the cycle stability of the Li / Li battery, and is better than control 1 and control 2.

[0056] Experiment 2-3

[0057] Assemble four identical lithium nickel manganese oxide / Li full batteries (positive electrode sheet diameter is 1 cm, lithium nickel manganese oxide surface loading is 1.2 mg cm -2 , lithium foil diameter 1 cm), 0.1 mL of ester LiPF was loaded into each of the four mold full batteries. 6 The electrolyte (marked as blank), 0.1 mL of a modified electrolyte containing 15-crown ether-5 (marked as control 1), 0.1 mL of a modified electrolyte containing an alkyl chain 15-crown ether-5 (marked as control 2), and 0.1 mL of a modified electrolyte containing fluorinated 15-crown ether-5 prepared in Example 2 (marked as fluorine-based additive); then the coulombic efficiency, cycle stability, capacity and retention rate of the four batteries were tested at a current density of 2C, and the results were as follows: Figure 2-3 shown.

[0058] according to Figure 2-3 It can be seen that at an ultra-high current density of 2C, the capacity of the lithium nickel manganese oxide / Li battery containing the fluorinated 15-crown ether-5 modified electrolyte is higher than that of the blank ester LiPF 6 The capacity of lithium nickel manganese oxide / Li battery with electrolyte is significantly improved; blank ester LiPF 6 The capacity of the LiMnO2 / Li battery with modified electrolyte showed a decreasing trend from the beginning of the cycle, and the capacity was only 27 mAh / g after 800 cycles. However, the capacity of the LiMnO2 / Li battery with modified electrolyte containing 15-crown ether-5 was basically unchanged after 800 cycles. It can be seen that the cycle stability, capacity and retention rate of the LiMnO2 / Li battery with modified electrolyte containing 15-crown ether-5 were significantly improved, indicating that the ester LiPF 6 Adding fluorinated 15-crown ether-5 into the electrolyte can significantly improve the coulombic efficiency, cycle stability, capacity and retention rate of the battery, and is better than control 1 and control 2.

[0059] Although specific embodiments of the present invention are described above, those skilled in the art should understand that these are merely examples and that various changes or modifications may be made to the embodiments without departing from the principles and essence of the present invention. The scope of protection of the present invention is limited only by the appended claims.

Claims

1. A crown ether compound, characterized in that It has a chemical structure represented by formula (i) or formula (ii):

2. A rechargeable battery electrolyte, characterized in that: The invention is composed of a rechargeable battery electrolyte and an electrolyte additive, wherein the electrolyte additive is the crown ether compound according to claim 1.

3. The rechargeable battery electrolyte according to claim 2, characterized in that: The rechargeable battery electrolyte is one of ester electrolyte, ether electrolyte, nitrile electrolyte, sulfone electrolyte, aqueous electrolyte, mixed electrolyte and ionic liquid electrolyte.

4. The rechargeable battery electrolyte according to claim 2 or 3, characterized in that: The ratio of the mass of the electrolyte additive to the volume of the rechargeable battery electrolyte is 0.01-100g:1L.

5. A rechargeable battery, characterized in that: The rechargeable battery electrolyte according to any one of claims 2 to 4 is used.

6. The rechargeable battery according to claim 5, characterized in that: The rechargeable battery is one of a metal lithium / lithium ion battery, a metal sodium / sodium ion battery, a metal potassium / potassium ion battery, a metal magnesium / magnesium ion battery, a metal aluminum / aluminum ion battery, a metal zinc / zinc ion battery, and an iron battery.

Citation Information

Patent Citations

  • Crown ether electrolyte and application thereof

    CN111293356A

  • Liquid electrolyte for metal battery, preparation method of liquid electrolyte and metal battery

    CN115295885A

  • Electrolyte additive for improving rate and low-temperature performance of lithium ion battery and electrolyte containing additive

    CN115377496A

  • Secondary battery

    CN115799614A

  • Remote inspection system using drone swarms

    KR1020230030149A

Cited By

  • Lithium ion battery electrolyte additive and electrolyte

    CN119504857A

  • Lithium ion battery electrolyte additive and electrolyte

    CN119504857B

  • Water-based crown ether electrolyte capable of chelating stannous ions as well as preparation and application of water-based crown ether electrolyte

    CN120810014A