Positive dispersing agent and preparation method thereof, positive slurry and positive pole piece
By using a cathode dispersant containing carboxylic acid and phosphate ester groups in lithium-ion batteries, combined with π-π conjugated connection and polymerization reaction technology, the problem of agglomeration and poor dispersion of cathode active materials is solved, and the battery cycle is improved. performance and energy density.
Patent Information
- Application Number
- CN202410754909.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-12
- Publication Date
- 2024-10-08
AI Technical Summary
The existing lithium-ion battery cathode dispersants have insufficient anchor points, resulting in agglomeration of cathode active materials, poor dispersion effect and poor fluidity, and affecting the electrode coating effect and battery cycle performance.
A cathode dispersant containing carboxylic acid groups and phosphate ester groups is used to connect with π-π conjugation on the surface of the cathode active material to increase anchor points and prevent agglomeration. It is also prepared through a specific polymerization process to improve the dispersant. The molecular weight and degree of polymerization are used to improve the dispersion effect and fluidity of the slurry.
It effectively prevents the agglomeration of positive electrode active materials, improves the dispersion effect and fluidity of the positive electrode slurry, reduces the resistance of the electrode piece, improves the battery cycle performance, and enhances the energy density and stability of the battery.
Smart Images

Figure CN118745236A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of lithium-ion batteries, and in particular relates to a positive electrode dispersant and a preparation method thereof, a positive electrode slurry, and a positive electrode sheet. Background Art
[0002] As an energy storage device, lithium-ion batteries have the advantages of long cycle life, low self-discharge, high specific energy, and environmental protection, and have been widely used in the field of 3C products. However, commercial lithium-ion batteries are subject to the embedded energy storage mechanism of their own materials, and their actual energy density increases slowly; therefore, the research and development of secondary batteries with higher energy density has become a social consensus to meet the consumer demand of the electric vehicle market with higher standards.
[0003] In order to improve the energy density of lithium-ion batteries, there are methods that start from the positive electrode active material, such as carbon coating on the surface of the positive electrode active material, or doping with other metal elements. Although the methods of carbon coating or doping with metal elements on the surface of the positive electrode active material can improve the conductivity of the positive electrode active material, it also increases the difficulty of dispersing the positive electrode slurry.
[0004] The positive electrode dispersant for lithium batteries is an additive used to improve the dispersion of positive electrode active material particles. It has the function of preventing particle agglomeration and improving electrode performance and cycle stability. The commonly used positive electrode dispersant is a polymer containing active groups, which can effectively coat the surface of the positive electrode active material to improve the dispersion of the positive electrode active material. For example, the existing polyether phosphate dispersant has the effect of improving the dispersion of positive electrode active material particles, but only contains phosphate groups that can anchor with the positive electrode active material, and there are few anchoring points, which cannot better inhibit the agglomeration of the positive electrode active material. The prepared slurry has poor dispersion effect and fluidity, and the slurry viscosity problem has not been improved, which affects the coating effect of the positive electrode slurry on the aluminum foil. Summary of the invention
[0005] In view of the problems that existing polyether phosphate dispersants have few anchoring points with positive electrode active materials, the prepared slurry has poor dispersion effect and fluidity, and the slurry is viscous, the present application provides a positive electrode dispersant and a preparation method thereof, a positive electrode slurry, and a positive electrode sheet.
[0006] The technical solution adopted by the present invention to solve the above technical problems is as follows:
[0007] The present application provides a positive electrode dispersant, wherein the dispersant is a compound represented by structural formula I,
[0008]
[0009] Wherein, p is 1 to 50, n is 1 to 50, m is 1 to 25, a is 0 to 50, and b is 0 to 50;
[0010] R, R' are each independently selected from H or CH3.
[0011] Preferably, p is 1-50, n is 1-25, m is 5-25, a is 0-50, and b is 0-30.
[0012] Preferably, the molecular weight of the compound represented by structural formula I is 5,000 to 80,000.
[0013] Preferably, the molecular weight of the compound represented by structural formula I is 7500 to 50000.
[0014] In a second aspect, the present application provides a method for preparing the above-mentioned dispersant for lithium-ion battery positive electrode slurry, comprising the following steps:
[0015] S1: adding a solvent, propylene alcohol and a catalyst into a reaction container, heating and pressurizing, and then adding propylene oxide and ethylene oxide to carry out a first polymerization reaction to obtain a first copolymer;
[0016] S2: mixing the first copolymer prepared in step S1, the first monomer and the second monomer, adding an initiator to carry out a second polymerization reaction to obtain a second copolymer;
[0017] S3: mixing the second copolymer prepared in step S2 with phosphorus pentoxide for reaction, and then hydrolyzing to obtain a compound represented by structural formula I;
[0018] The first monomer includes one or both of styrene and methylstyrene; the second monomer includes one or both of acrylic acid and methacrylic acid.
[0019] Preferably, in S1, the mass ratio of the acryl alcohol to the catalyst is 1:(0.1-2.0); the molar ratio of the acryl alcohol to the ethylene oxide is 1:(1-50);
[0020] In S1, the reaction conditions of the first polymerization reaction are: reaction temperature of 20 to 80° C., reaction pressure of 0 to 5 MPa, and reaction time of 6 to 30 h.
[0021] Preferably, in S2, the molar ratio of the first copolymer, the first monomer and the second monomer is 1:(0.1-10):(0.1-10), the reaction temperature of the second polymerization reaction is 50-90° C., and the time of the second polymerization reaction is 2-8 hours.
[0022] Preferably, in S3, the second copolymer contains hydroxyl groups, and the molar ratio of hydroxyl groups to phosphorus pentoxide in the second copolymer is 1:(0.4-1.0);
[0023] The reaction temperature of the mixture of hydroxyl group and phosphorus pentoxide in the second copolymer is 50-90° C., and the reaction time is 2-6 hours.
[0024] In a third aspect, the present application provides a positive electrode slurry, comprising a positive electrode active material and a positive electrode dispersant, wherein the positive electrode dispersant is the positive electrode dispersant described above or the positive electrode dispersant prepared by the preparation method of the positive electrode dispersant described above;
[0025] The positive electrode active material includes one or more compounds represented by formula I, formula II, and formula III.
[0026] LiMO2 Formula Ⅰ
[0027] Wherein, M is selected from one of Co, Mn, Ni and V;
[0028] LiNPO4 Formula Ⅱ
[0029] Wherein, N is selected from one of Fe, Co, Mn and Ni;
[0030] LiNi x Co y L 1-x-y O2 Formula Ⅲ
[0031] Among them, 0≤x≤1, 0≤y≤1; L is selected from one of Mn and Al.
[0032] In a fourth aspect, the present application provides a positive electrode plate, comprising a positive electrode collector, wherein the positive electrode slurry described above is disposed on the surface of the positive electrode collector.
[0033] Beneficial Effects
[0034] Compared with the prior art, the positive electrode dispersant provided by the present application contains carboxylic acid groups and phosphate groups that can be anchored on the surface of the positive electrode active material, increase the anchoring points of the positive electrode active material, effectively prevent the positive electrode active material from agglomerating, and improve the dispersion effect of the positive electrode slurry; the contained benzene ring can be connected to the carbon coated on the surface of the positive active material in a π-π conjugated manner, increase the anchoring points, and further improve the dispersion effect of the positive electrode slurry. The positive electrode dispersant provided by the present application is used in the positive electrode slurry, anchored on the surface of the positive electrode active material, prevents the positive electrode active material from agglomerating, improves the dispersion effect of the slurry, improves the fluidity of the slurry, improves the stability of the slurry, solves the problem of slurry viscosity, improves the coating effect of the pole piece, reduces the pole piece resistance, and improves the battery cycle performance. DETAILED DESCRIPTION
[0035] In order to make the technical problems, technical solutions and beneficial effects solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0036] The present invention provides a positive electrode dispersant, wherein the dispersant is a compound represented by structural formula I.
[0037]
[0038] Wherein, p is 1 to 50, n is 1 to 50, m is 1 to 25, a is 0 to 50, and b is 0 to 50;
[0039] R, R' are each independently selected from H or CH3.
[0040] The positive electrode dispersant provided in the present application contains a carboxylic acid group, and the carboxylic acid group contains a polar bond. The carboxylic acid group can be anchored on the surface of the positive electrode active material. When preparing the slurry, the positive electrode dispersant anchored on the surface of the positive electrode active material prevents the agglomeration of the positive electrode active material and improves the dispersion effect of the positive electrode slurry. The benzene ring contained in the positive electrode dispersant can provide a π-π conjugated effect, and the benzene ring can be connected to carbon in a π-π conjugated manner. For positive electrode active materials containing carbon-coated structures or positive electrode active materials with carbon attached to the surface, the anchoring points are increased, and the dispersion effect of the positive electrode material is improved. The phosphate group contained in the positive electrode dispersant can be anchored on the surface of the positive electrode active material, improving the dispersion effect of the positive electrode active material.
[0041] Compared with the prior art, the positive electrode dispersant provided by the present application contains carboxylic acid groups and phosphate groups that can be anchored on the surface of the positive electrode active material, increase the anchoring points of the positive electrode active material, effectively prevent the positive electrode active material from agglomerating, and improve the dispersion effect of the positive electrode slurry; the contained benzene ring can be connected to the carbon coated or attached to the surface of the positive active material in a π-π conjugated manner, increase the anchoring points, and further improve the dispersion effect of the positive electrode slurry. The positive electrode dispersant provided by the present application is used in the positive electrode slurry, anchored on the surface of the positive electrode active material, prevents the positive electrode active material from agglomerating, improves the dispersion effect of the slurry, improves the fluidity of the slurry, improves the stability of the slurry, solves the problem of slurry viscosity, improves the coating effect of the pole piece, reduces the pole piece resistance, and improves the battery cycle performance.
[0042] The positive electrode dispersant provided in the present application can increase the anchoring points with the positive electrode active material, reduce the risk of secondary aggregation of solid particles in the positive electrode slurry, improve the dispersion effect of the slurry, improve the fluidity of the positive electrode slurry, and increase the solid content of the slurry, while ensuring that the conductive performance of the lithium-ion battery is not affected. At the same time, it can reduce the resistance of the positive electrode sheet, improve the battery cycle efficiency, and improve the battery electrical performance.
[0043] Specifically, in the compound shown in formula I, a is 0-50, b is 0-50, p is 1-50, n is 1-50, and m is 1-25. Specifically, a and b can be 1, 5, 10, 16, 20, 24, 30, 35, 40, 43, 48, 50, etc.; p and n can be 1, 9, 10, 15, 20, 24, 30, 36, 40, 45, 50, etc.; m can be 1, 5, 10, 12, 18, 20, 24, 25, etc. If a is greater than 50, or b is greater than 50, or p or n is greater than 50, or m is greater than 25, the degree of polymerization is large, the molecular chain is long, the steric hindrance of the compound shown in formula I is reduced, the dispersion effect is reduced, the slurry fluidity is poor, and the slurry viscosity increases faster with the increase of the slurry storage time, the slurry coating effect is poor, the electrode sheet resistance is increased, and the battery performance is reduced. In the compound shown in structural formula I, the degree of polymerization n is 0, and there is no (methyl) styrene group, that is, the prepared positive electrode dispersant does not contain a benzene ring, and cannot form π-π conjugation with the carbon on the surface of the positive active material coated with carbon or attached to the surface of carbon, and cannot prevent the agglomeration of the positive active material. The dispersion effect of the slurry is poor, and the slurry has agglomeration and viscosity problems, which affects the further increase of the solid content of the slurry and has a certain negative effect on the slurry coating. If p is 0, the prepared positive electrode dispersant has no carboxylic acid group, the anchoring points between the dispersant and the surface of the positive active material are reduced, the dispersing performance of the dispersant is reduced, the dispersion effect of the slurry is poor, and the slurry is prone to agglomeration and viscosity problems, which affects the coating of the pole piece and the battery performance.
[0044] In some preferred embodiments, p is 1-50, n is 1-25, m is 5-25, a is 0-50, and b is 0-30.
[0045] In a preferred embodiment, the dispersant of the compound shown in structural formula I is mixed with the positive electrode active material, the conductive agent, and the binder, which has a better dispersion effect, is beneficial to hinder the agglomeration of the positive electrode active material, improve the fluidity of the positive electrode slurry, increase the solid content of the slurry, reduce the viscosity of the slurry, improve the fluidity of the slurry, solve the problem of slurry viscosity, and improve the coating effect of the electrode.
[0046] In some embodiments, the molecular weight of the compound represented by structural formula I is 5,000 to 80,000.
[0047] Limiting the molecular weight of the compound represented by structural formula I to 5,000 to 80,000 is beneficial to improving the dispersing effect of the dispersant in the positive electrode slurry, reducing the risk of secondary aggregation of solid particles (such as positive electrode active materials) in the positive electrode slurry, and improving the fluidity of the positive electrode slurry.
[0048] In some preferred embodiments, the molecular weight of the compound represented by structural formula I is 7500 to 50000. More preferably, the molecular weight of the compound represented by structural formula I can also be 10000 to 45000.
[0049] In a second aspect, the present application provides a method for preparing a positive electrode dispersant, comprising the following steps:
[0050] S1: adding a solvent, propylene alcohol and a catalyst into a reaction container, heating and pressurizing, and then adding propylene oxide and ethylene oxide to carry out a first polymerization reaction to obtain a first copolymer;
[0051] S2: mixing the first copolymer prepared in step S1, the first monomer and the second monomer, adding an initiator to carry out a second polymerization reaction to obtain a second copolymer;
[0052] S3: mixing the second copolymer prepared in step S2 with phosphorus pentoxide for reaction, and then hydrolyzing to obtain a compound represented by structural formula I;
[0053] The first monomer includes one or both of styrene and methylstyrene; the second monomer includes one or both of acrylic acid and methacrylic acid.
[0054] Specifically, the first copolymer is a propylene polyoxyethylene polyoxypropylene ether copolymer. The second copolymer is a copolymer containing propylene polyoxyethylene polyoxypropylene ether, a first monomer and a second monomer.
[0055] Specifically, a and b in structural formula I may both be 0. In step S1, when no ethylene oxide is added, a is 0, and when no propylene oxide is added, b is 0. In order to improve the dispersion effect of the positive electrode dispersant, ethylene oxide and propylene oxide are generally added, that is, a satisfies 0<a≤50, and b satisfies 0<b≤50. Further preferably, the range of a is 0<a≤30, and the range of b is 0<b≤30.
[0056] Compared with the prior art, the preparation method of the positive electrode dispersant provided in the present application has a simple preparation process and low cost. The prepared positive electrode dispersant has increased anchor points with the positive electrode active material, which can effectively prevent the agglomeration of the positive electrode active material, improve the dispersion effect of the slurry, and improve the fluidity and stability of the slurry.
[0057] In some embodiments, in S1, the mass ratio of the acryl alcohol to the catalyst is 1:(0.1-0.2); the molar ratio of the acryl alcohol to the ethylene oxide is 1:(1-50), and the molar ratio of the acryl alcohol to the propylene oxide is 1:(1-50);
[0058] In S1, the reaction conditions of the first polymerization reaction are: reaction temperature of 20 to 80° C., reaction pressure of 0 to 5 MPa, and reaction time of 6 to 30 h.
[0059] Specifically, in step S1, the catalyst plays a catalytic role, catalyzing the first polymerization reaction of propylene alcohol with propylene oxide and ethylene oxide, and polymerizing under the conditions of heating temperature of 20 to 80°C and pressure of 0 to 5MPa to obtain a propylene-based polyoxyethylene polyoxypropylene ether copolymer. Among them, the molar ratio of propylene alcohol to propylene oxide can be 1: (1 to 50). Further preferably, the molar ratio of propylene alcohol to propylene oxide can be 1: (1 to 30); the molar ratio of propylene alcohol to ethylene oxide is 1: (1 to 50). The positive electrode dispersant in the prepared compound shown in structural formula I can increase the anchoring point with the positive electrode active material, reduce the risk of secondary aggregation of solid particles in the positive electrode slurry, improve the dispersion effect of the slurry, reduce the internal resistance of the electrode sheet, and improve the battery performance while ensuring that the conductive performance of the lithium-ion battery is not affected.
[0060] If the molar ratio of propylene alcohol to propylene oxide is lower than 1:(1-30), or the molar ratio of propylene alcohol to ethylene oxide is lower than 1:(1-50), the propylene oxide or ethylene oxide contained is too much, the degree of polymerization of the generated compound is large, the molecular chain is long, and under the same addition amount, the longer the molecular chain of the compound shown in structural formula I, the fewer the number of molecules, and the overlong molecular chain will bend and fold in the solvent, which is generally manifested as reduced steric hindrance, reduced dispersion effect, and poor slurry fluidity. Further preferably, the molar ratio of propylene alcohol to ethylene oxide is 1:(1-30).
[0061] The reaction temperature of the first polymerization reaction can be 20° C., 24° C., 30° C., 33° C., 38° C., 40° C., 43° C., 47° C., 50° C., 56° C., 60° C., 66° C., 70° C., 74° C., 80° C., etc., as long as the reaction temperature of the first polymerization reaction is within the range of 20 to 80° C. If the reaction temperature is too high, the reaction is too fast, and implosion is likely to occur, which makes it impossible to implement; if the reaction temperature is too low, the polymerization reaction cannot occur.
[0062] In some preferred embodiments, the reaction conditions of the first polymerization reaction are: reaction temperature of 30-70° C., and reaction pressure of 1-4 MPa.
[0063] The reaction temperature of the first polymerization reaction is 30-70° C., and the reaction pressure is 1-4 MPa, which can ensure that propylene alcohol, ethylene oxide, and propylene oxide undergo the first polymerization reaction under the catalyst conditions while also reducing the production cost.
[0064] In some embodiments, the solvent includes one or both of anhydrous tetrahydrofuran and NMP (N-methyl-2-pyrrolidone).
[0065] In some embodiments, the catalyst includes one or more of potassium naphthalene, sodium naphthalene, and an alkali metal.
[0066] In some embodiments, in S2, the molar ratio of the first copolymer, the first monomer, and the second monomer is 1:(0.1-10):(0.1-10), the reaction temperature of the second polymerization reaction is 50-90° C., and the time of the second polymerization reaction is 2-8 hours.
[0067] The molar ratio of the first copolymer, the first monomer, and the second monomer is in the range of 1: (0.1-10): (0.1-10). The positive electrode dispersant of the compound shown in the structural formula 1 can increase the anchoring points with the positive electrode active material under the premise of ensuring that the conductive performance of the lithium-ion battery is not affected, reduce the risk of secondary aggregation of solid particles in the positive electrode slurry, improve the dispersion effect of the slurry, improve the fluidity of the positive electrode slurry, increase the solid content of the slurry, and at the same time reduce the resistance of the positive electrode sheet and improve the battery performance. If the molar ratio of the first copolymer, the first monomer, and the second monomer is too low, the first monomer and the second monomer contained are too low, n is less than 1, and p is less than 1, the content of the compound shown in the structural formula 1 generated is reduced, the aggregation of the positive electrode active material cannot be prevented, the anchoring points are reduced, and the dispersion effect of the dispersant is deteriorated. If the molar ratio of the first copolymer, the first monomer, and the second monomer is too high, n is greater than 50, p is greater than 50, the degree of polymerization is large, the molecular chain is long, the steric hindrance of the compound shown in the structural formula I is reduced, the dispersion effect is reduced, the slurry coating effect is deteriorated, the electrode sheet resistance is increased, and the battery performance is reduced.
[0068] Specifically, the second polymerization reaction temperature can be 50°C, 53°C, 56°C, 60°C, 62°C, 66°C, 70°C, 74°C, 75°C, 80°C, 83°C, 86°C, 90°C, etc., as long as the reaction temperature of the second polymerization reaction is within the range of 50-90°C. The second polymerization reaction time can be 2h, 2.5h, 2.8h, 3.0h, 3.5h, 4.0h, 4.5h, 5.0h, 6.0h, 7.0h, 8h, etc. If the polymerization reaction temperature is too high, the reaction is too fast, and implosion is likely to occur, which cannot be implemented; if the polymerization reaction temperature is too low, the polymerization reaction cannot occur.
[0069] Under the condition of the second polymerization reaction temperature of 50-90° C., the first copolymer, the first monomer and the second monomer undergo a second polymerization reaction to generate a compound containing a phenyl group and a carboxyl group.
[0070] More preferably, the second polymerization temperature is 60-80° C., and the second polymerization time is 3-7 hours. More preferably, the molar ratio of the propylene polyoxyethylene polyoxypropylene ether copolymer, (methyl) styrene and (methyl) acrylic acid is 1: (1-8): (0.5-8).
[0071] Specifically, the first copolymer, the first monomer, and the second monomer undergo a second polymerization reaction to generate a second copolymer, wherein the second copolymer is a copolymer containing propylene polyoxyethylene polyoxypropylene ether copolymer, styrene, and acrylic acid, or the second copolymer is a copolymer containing propylene polyoxyethylene polyoxypropylene ether copolymer, methylstyrene, and acrylic acid, or the second copolymer is a copolymer containing propylene polyoxyethylene polyoxypropylene ether copolymer, methylstyrene, and methacrylic acid, or the second copolymer is a copolymer containing propylene polyoxyethylene polyoxypropylene ether copolymer, styrene, and methacrylic acid.
[0072] In some preferred embodiments, the second polymerization reaction temperature is 60-70° C. In some embodiments, the initiator includes at least one of azobisisobutyronitrile (AIBN) and dibenzoyl peroxide (BPO).
[0073] In some embodiments, in S3, the second copolymer contains hydroxyl groups, and the molar ratio of hydroxyl groups to phosphorus pentoxide in the second copolymer is 1:(0.4-1.0);
[0074] The reaction temperature of the mixture of hydroxyl group and phosphorus pentoxide in the second copolymer is 50-90° C., and the reaction time is 2-6 hours.
[0075] Specifically, the molar ratio of hydroxyl group to phosphorus pentoxide in the second copolymer can be in the following ranges: 1: (0.4-0.5), 1: (0.5-0.6), 1: (0.6-0.7), 1: (0.7-0.8), 1: (0.9-1.0) or 1: (0.8-0.9). The molar ratio of hydroxyl group to phosphorus pentoxide in the second copolymer is in the range of 1: (0.4-1.0), which can reduce the generation of impurities, generate a larger content of the compound shown in structural formula 1, increase the anchoring points of the positive electrode active material, effectively prevent the agglomeration of the positive electrode active material, and improve the dispersion effect of the positive electrode slurry.
[0076] If the molar ratio of hydroxyl group to phosphorus pentoxide in the second copolymer is too low, the phosphorus pentoxide contained is too much, and the excess phosphorus pentoxide will directly form phosphoric acid. If the molar ratio of the two is too high, hydroxyl groups will remain or diesters will be formed. Whether the molar ratio of hydroxyl group to phosphorus pentoxide in the second copolymer is lower than 1: (0.4-1.0) or higher than 1: (0.4-1.0), the impurities in the generated dispersant increase, affecting the dispersing effect of the dispersant.
[0077] More preferably, the reaction temperature of the mixture of hydroxyl group and phosphorus pentoxide in the second copolymer is 55-80° C., and the reaction time is 3-5 hours.
[0078] It should be noted that the hydrolysis in step S3 of the present application is to hydrolyze the phosphorus pentoxide into phosphoric acid, and the hydrolysis reaction temperature is generally above 60° C. The specific hydrolysis reaction temperature and hydrolysis reaction time can refer to the prior art.
[0079] In some embodiments, adding the solvent, propylene alcohol, and catalyst into a reaction container comprises the following steps: introducing a protective gas into the reaction container, exhausting the air in the reaction container, and then adding the solvent, propylene alcohol, and catalyst.
[0080] The protective gas includes nitrogen and rare gas, and the rare gas includes argon, helium, argon, etc. The rare gas is limited to argon.
[0081] In some embodiments, in the step of mixing the second copolymer prepared in step S2 with phosphorus pentoxide, the second copolymer prepared in step S2 is first cooled to room temperature and then mixed with phosphorus pentoxide for reaction.
[0082] In a third aspect, the present application provides a positive electrode slurry, comprising a positive electrode active material and a positive electrode dispersant, wherein the positive electrode dispersant is the positive electrode dispersant described above or the positive electrode dispersant prepared by the preparation method of the positive electrode dispersant described above;
[0083] The positive electrode active material includes one or more compounds represented by formula I, formula II, and formula III.
[0084] LiMO2 Formula Ⅰ
[0085] Wherein, M is selected from one of Co, Mn, Ni and V;
[0086] LiNPO4 Formula Ⅱ
[0087] Wherein, N is selected from one of Fe, Co, Mn and Ni;
[0088] LiNi x Co y L 1-x-y O2 Formula Ⅲ
[0089] Among them, 0≤x≤1, 0≤y≤1; L is selected from one of Mn and Al.
[0090] In some embodiments, the positive electrode slurry further includes a conductive agent, a solvent and a binder, wherein the conductive agent includes one or more of graphite, graphene, carbon nanotubes, conductive carbon black, acetylene black, and carbon fiber. The binder includes fluororesins such as polytetrafluoroethylene, polyvinylidene fluoride resin, and polyvinylidene fluoride; polyolefin resins such as polyethylene and polypropylene; acrylic resins such as polyacrylic acid, polymethyl acrylate, and ethylene-acrylic acid copolymer; vinyl resins such as polyacrylonitrile and polyvinyl acetate; and one or more of rubber-like materials such as styrene-butadiene copolymer rubber. The solvent includes N-methyl-2-pyrrolidone (NMP), ethanol, and the like.
[0091] The positive electrode slurry obtained by mixing and stirring the positive electrode dispersant provided in the present application with the positive electrode active material, the conductive agent, the solvent and the binder has the advantages of reducing the risk of agglomeration of the positive electrode active material in the positive electrode slurry, having good slurry dispersibility and fluidity, increasing the solid content of the slurry, improving the coating effect of the electrode sheet, reducing the electrode sheet resistance, and improving the battery cycle performance.
[0092] In a fourth aspect, the present application provides a positive electrode plate, comprising a positive electrode collector, wherein the positive electrode slurry described above is disposed on the surface of the positive electrode collector.
[0093] The positive electrode slurry provided in the present application is coated on the surface of the positive electrode collector to obtain a positive electrode sheet. The positive electrode slurry has good fluidity and dispersibility, which is beneficial to reducing the resistance of the positive electrode sheet, improving the cycle efficiency of the battery, and improving the electrical performance of the battery.
[0094] The present invention is further described below by way of examples.
[0095] Example 1
[0096] The preparation method of the positive electrode dispersant comprises the following steps:
[0097] 1) A 250mL reaction bottle equipped with a magnetic stirrer was repeatedly evacuated and baked, and then filled with argon gas. After cooling, 150mL of anhydrous tetrahydrofuran (THF), 0.025mol of propylene alcohol, 0.025mol of potassium naphthalene, and 0.10mol of ethylene oxide (EO) were added under air isolation. After the first polymerization reaction temperature of 50°C was reacted for 6 hours, the reaction pressure was 1Mpa; 0.25mol of propylene oxide (PO) was added, and the reaction was continued for 16 hours, the reaction pressure was 4Mpa, and then the temperature was lowered to obtain the first copolymer, which was a copolymer containing propylene polyoxyethylene polyoxypropylene ether. The nuclear magnetic resonance results can calculate that the chain number a of the propylene polyoxyethylene polyoxypropylene ether copolymer is 4, b is 10, and the molecular weight is about 800.
[0098] 2) 1 mol of the above-synthesized propylene polyoxyethylene polyoxypropylene ether copolymer, methyl styrene, and acrylic acid monomer were mixed, and 0.1 mol of initiator AIBN was added to carry out a second polymerization reaction. The second polymerization reaction temperature was 60° C. and the reaction was carried out for 4 hours to obtain a second copolymer, which was a copolymer containing propylene polyoxyethylene polyoxypropylene ether-methyl styrene and acrylic acid.
[0099] 3) The copolymer was cooled to room temperature, 0.5 mol of phosphorus pentoxide was slowly added, the molar ratio of hydroxyl group and phosphorus pentoxide in the second polymer was 1:0.5, stirred for 30 minutes, and then reacted for 4 hours at a reaction temperature of 70°C, and an appropriate amount of water was added. After hydrolysis for 1 hour, the final product was obtained, which was the positive electrode dispersant shown in structural formula I, marked as SL1. The nuclear magnetic resonance results can be calculated that the number of chain links a of the final product is 4, b is 10, n is 10, m is 10, p is 10, and the molecular weight is 10000.
[0100] Example 2
[0101] Most of the steps in Example 2 are the same as step 1) in Example 1, except that 0 mol of propylene oxide is added in Example 2.
[0102] The propylene polyoxyethylene ether copolymer prepared in Example 2, i.e., the first copolymer, is reacted with styrene and methacrylic acid, the molar ratio of the first copolymer to styrene and methacrylic acid is 1:2:3, and the initiator BPO is added for a second polymerization reaction, and the reaction is carried out at 60°C for 4 hours to prepare a second copolymer, which is a copolymer containing propylene polyoxyethylene ether copolymer, styrene and methacrylic acid. The above-mentioned second copolymer is cooled to room temperature, phosphorus pentoxide is slowly added, the ratio of hydroxyl to phosphorus pentoxide is 1:0.6, stirred for 30 minutes, and then reacted at 70°C for 4 hours, and an appropriate amount of water is added. After hydrolysis for 1 hour, the final product is the dispersant shown in structural formula I, marked as SL2. The nuclear magnetic results can calculate that the number of chain links a of the final product is 45, b is 0, n is 20, m is 10, p is 30, and the molecular weight is 25000.
[0103] Example 3
[0104] Most of the steps of this embodiment are the same as those of embodiment 1, except that in step 2), 1 mol of propylene polyoxyethylene polyoxypropylene ether copolymer, 10 mol of methyl styrene, and 10 mol of acrylic acid monomer are added. The prepared dispersant has a final product with a chain number a of 4, b of 10, n of 20, m of 2, p of 20, and a molecular weight of 5500, as calculated by NMR results.
[0105] Example 4
[0106] Most of the steps of this embodiment are the same as those of embodiment 1, except that in step 2), 1 mol of propylene polyoxyethylene polyoxypropylene ether copolymer, 5 mol of styrene, and 5 mol of methacrylic acid monomer are added, and an appropriate amount of initiator is used to control the molecular weight. The prepared dispersant, according to the NMR results, can be calculated that the number of chain segments a of the final product is 4, b is 10, n is 20, m is 4, p is 20, and the molecular weight is 7000.
[0107] Example 5
[0108] Most of the steps of this embodiment are the same as those of embodiment 1, except that: in step 1), the first polymerization reaction temperature is 60°C; in step 2), the second polymerization reaction temperature is 70°C; in step 3), the molar ratio of hydroxyl group and phosphorus pentoxide in the second polymer is 1:0.7, stirring for 30 minutes, and then reacting for 5 hours at a reaction temperature of 60°C. The rest is the same as embodiment 1.
[0109] The prepared dispersant has a final product with chain number a of 4, b of 10, n of 8, m of 8, p of 8 and a molecular weight of 8000, calculated from the NMR results.
[0110] Example 6
[0111] Most of the steps of this embodiment are the same as those of embodiment 1, except that in step 3), the molar ratio of the hydroxyl group in the second polymer to phosphorus pentoxide is 1:1.2. The prepared dispersant has a final product with a chain number a of 4, b of 10, n of 8, m of 8, p of 8, and a molecular weight of 8000, as calculated by NMR results.
[0112] Example 7
[0113] Most of the steps of this embodiment are the same as those of embodiment 1, except that in step 3), the molar ratio of the hydroxyl group in the second polymer to phosphorus pentoxide is 1:0.2. The prepared dispersant, according to the nuclear magnetic resonance results, can be calculated that the number of chain segments a of the final product is 4, b is 10, n is 8, m is 8, p is 8, and the molecular weight is 20000. The increase in molecular weight is mainly caused by the reduction of phosphorus pentoxide, which leads to the formation of diesters or triesters of phosphate esters.
[0114] Comparative Example 1
[0115] Most of the steps of this comparative example are the same as those of Example 1, except that no methyl styrene is added in step 2). The prepared dispersant, according to the NMR results, can be calculated that the number of chain segments a of the final product is 4, b is 10, n is 0, m is 10, p is 10, and the molecular weight is 9000.
[0116] Comparative Example 2
[0117] Most of the steps of this comparative example are the same as those of Example 1, except that no acrylic acid is added in step 2). The prepared dispersant has a final product with a chain number a of 4, b of 10, n of 10, m of 10, p of 0, and a molecular weight of 9300, as calculated by NMR results.
[0118] Comparative Example 3
[0119] This comparative example is similar to Example 1 in most steps, except that: in step 2), 1 mol of propylene polyoxyethylene polyoxypropylene ether copolymer, 15 mol of methyl styrene, and 15 mol of acrylic acid monomer are added. The prepared dispersant has a final product with a chain number a of 4, b of 10, n of 75, m of 5, p of 75, and a molecular weight of 18,500, as calculated by NMR results.
[0120] Comparative Example 4
[0121] The positive electrode dispersant of Comparative Example 4 is a commercially available phosphate ester dispersant polyether phosphate.
[0122] Performance Testing
[0123] The positive electrode dispersant prepared in the above-mentioned embodiments and comparative examples is uniformly mixed with the positive electrode active material lithium iron phosphate, the conductive agent conductive carbon black, and the binder polyvinylidene fluoride in a mass ratio of 0.2:96.5:1.5:2.0, and then dispersed and stirred with the solvent NMP to prepare a positive electrode slurry, and then the positive electrode slurry is coated on at least one side of the positive electrode current collector to obtain a positive electrode sheet.
[0124] Viscosity test: The positive electrode slurry prepared above was left to stand for viscosity tests at time intervals of 0 min, 4 h, and 24 h. The specific test results are shown in Table 1.
[0125] Table 1
[0126]
[0127] It can be seen from Table 1 that, in comparison between Example 1 and Comparative Examples 1, 2, and 4, there is no methyl styrene in Comparative Example 1, and the prepared dispersant does not contain a benzene ring, the prepared slurry has a high viscosity, and the dispersion effect is poor, indicating that the first monomer is added to the dispersant, the dispersant contains a benzene ring, and can be connected to the carbon in a π-π conjugated manner, for the positive electrode active material containing a carbon-coated structure, the anchor point is increased, and the dispersion effect of the positive electrode slurry is improved; in Comparative Example 2, no second monomer acrylic acid or methacrylic acid is added, the prepared dispersant has no carboxylic acid group, and the viscosity of the slurry is poor. The degree is high and the dispersion effect is poor, indicating that the carboxylic acid group contained in the dispersant can be anchored on the surface of the positive active material, increase the anchoring points, and improve the dispersion effect of the positive electrode slurry; in Comparative Example 4, there is no benzene ring or carboxylic acid group, and only contains phosphate groups. The viscosity of the slurry is high and the stability is low, indicating that the positive electrode dispersant provided by the present application contains carboxylic acid groups and phosphate groups that can increase the anchoring points, and the benzene ring can be connected to the carbon coated on the surface of the positive active material in a π-π conjugated manner, which also increases the anchoring points. The three synergistically improve the dispersion effect of the positive electrode dispersant.
[0128] The comparison between Example 1 and Comparative Example 3 shows that the prepared positive electrode dispersant, even if it conforms to the structural formula I provided in the present application, still has the problem of poor dispersion effect if n is not in the range of 1 to 50 and p is not in the range of 1 to 50. It is speculated that this is because the degree of polymerization is large and the molecular chain is long, the steric hindrance of the compound shown in structural formula I is reduced, the dispersion effect is reduced, and the slurry fluidity becomes poor.
[0129] By comparing Examples 1-4, the molar content of the propylene polyoxyethylene polyoxypropylene ether copolymer and the first monomer and the second monomer is changed, and the prepared dispersant is the compound shown in structural formula I, and p is 1 to 50, n is 1 to 50, m is 1 to 25, a is 0 to 50, and b is in the range of 0 to 50. The prepared positive electrode slurry has low viscosity, good dispersion effect, good fluidity, and good slurry stability.
[0130] Comparing Examples 1 and 5 with Examples 6 and 7, in the process of preparing the dispersant, the molar ratio of hydroxyl group and phosphorus pentoxide in the added second polymer is lower than 1:0.4 or higher than 1:1.0, the content of the compound shown in Structural Formula 1 is reduced, and the dispersion effect is poor; the molar ratio of hydroxyl group and phosphorus pentoxide in the added second polymer is in the range of 1:(0.4 to 1.0), the content of the compound shown in Structural Formula 1 is relatively high, which can increase the anchoring points of the positive electrode active material, effectively prevent the agglomeration of the positive electrode active material, and improve the dispersion effect of the positive electrode slurry.
[0131] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A positive electrode dispersant, characterized in that The dispersant is a compound represented by structural formula I, Wherein, p is 1 to 50, n is 1 to 50, m is 1 to 25, a is 0 to 50, and b is 0 to 50; R, R' are each independently selected from H or CH3.
2. The positive electrode dispersant according to claim 1, characterized in that The p is 1-50, n is 1-25, m is 5-25, a is 0-50, and b is 0-30.
3. The positive electrode dispersant according to claim 1, characterized in that The molecular weight of the compound represented by the structural formula I is 5,000 to 80,000.
4. The positive electrode dispersant according to claim 3, characterized in that The molecular weight of the compound represented by the structural formula I is 7500 to 50000.
5. A method for preparing a positive electrode dispersant according to any one of claims 1 to 4, characterized in that: The following steps are involved: S1: adding a solvent, propylene alcohol and a catalyst into a reaction container, heating and pressurizing, and then adding propylene oxide and ethylene oxide to carry out a first polymerization reaction to obtain a first copolymer; S2: mixing the first copolymer prepared in step S1, the first monomer and the second monomer, adding an initiator to carry out a second polymerization reaction to obtain a second copolymer; S3: mixing the second copolymer prepared in step S2 with phosphorus pentoxide for reaction, and then hydrolyzing to obtain a compound represented by structural formula I; The first monomer includes one or both of styrene and methylstyrene; the second monomer includes one or both of acrylic acid and methacrylic acid.
6. The method for preparing a positive electrode dispersant according to claim 5, characterized in that: In S1, the mass ratio of the acryl alcohol to the catalyst is 1:(0.1-2.0); the molar ratio of the acryl alcohol to the ethylene oxide is 1:(1-50), and the molar ratio of the acryl alcohol to the propylene oxide is 1:(1-50); In S1, the reaction conditions of the first polymerization reaction are: reaction temperature of 20 to 80° C., reaction pressure of 0 to 5 MPa, and reaction time of 6 to 30 h.
7. The method for preparing a positive electrode dispersant according to claim 5, characterized in that: In S2, the molar ratio of the first copolymer, the first monomer and the second monomer is 1:(0.1-10):(0.1-10), the reaction temperature of the second polymerization reaction is 50-90° C., and the time of the second polymerization reaction is 2-8 hours.
8. The method for preparing a positive electrode dispersant according to claim 5, characterized in that: In S3, the second copolymer contains hydroxyl groups, and the molar ratio of hydroxyl groups to phosphorus pentoxide in the second copolymer is 1:(0.4-1.0); The reaction temperature of the mixture of hydroxyl group and phosphorus pentoxide in the second copolymer is 50-90° C., and the reaction time is 2-6 hours.
9. A positive electrode slurry, characterized in that: It comprises a positive electrode active material and a positive electrode dispersant, wherein the positive electrode dispersant is a positive electrode dispersant according to any one of claims 1 to 4 or a positive electrode dispersant prepared by the preparation method of the positive electrode dispersant according to any one of claims 5 to 8; The positive electrode active material includes one or more compounds represented by formula I, formula II, and formula III. LiMO2 Formula Ⅰ Wherein, M is selected from one of Co, Mn, Ni and V; LiNPO4 Formula Ⅱ Wherein, N is selected from one of Fe, Co, Mn and Ni; LiNi x Co y L 1-x-y O2 Formula Ⅲ Among them, 0≤x≤1, 0≤y≤1; L is selected from one of Mn and Al.
10. A positive electrode sheet, characterized in that: It comprises a positive electrode current collector, on the surface of which the positive electrode slurry according to claim 9 is arranged.
Citation Information
Cited By
Dispersing agent for electrode slurry as well as preparation method and application of dispersing agent
CN120904410A
Manufacturing method and structure of coupling mechanism based on PCB polar plate
CN120916325A
Composite lithium ion battery electrode slurry dispersing agent, preparation method, electrode slurry and battery
CN121394406A
Dispersing and softening agent for positive electrode of lithium iron phosphate battery, preparation method of dispersing and softening agent, positive electrode slurry of lithium iron phosphate battery and positive electrode piece prepared from positive electrode slurry
CN122060108A