Method for modifying spherical silica powder by using disilane

The surface modification of spherical silica powder by double silanes solves the problem of increased viscosity and difficulty in dispersion of spherical silica powder at high filling amounts, and improves its uniformity and hydrophobicity in epoxy plastic and liquid packaging materials. , broadening the application fields, reducing costs and simplifying the process.

CN118745291APending Publication Date: 2024-10-08UNIV OF JINAN +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410798482.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-20
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

After the filling amount of spherical silica powder increases, the viscosity of the system increases sharply, the fluidity and permeability become poor, and dispersion is difficult. The high cost of existing modification methods hinders its further application.

Method used

The spherical silica powder was surface modified with bisilanes ((3-isocyanopropyl)triethoxysilane and dimethyldimethoxysilane), treated with NaOH solution, washed and vacuum dried, and then dried in nitrogen Stir with deionized water under protection, slowly add silane dropwise, react and filter, and finally obtain modified spherical silica powder through vacuum drying and grinding.

Benefits of technology

Significantly improves the hydrophobicity of spherical silica powder, promotes its mixing uniformity in epoxy plastic encapsulation materials and liquid encapsulation materials, broadens its application in the fields of electronic packaging and hydrophobic coatings, reduces costs, and simplifies the process flow .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118745291A_ABST
    Figure CN118745291A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of inorganic non-metallic materials, and particularly relates to a method for modifying spherical silica powder by utilizing disilane. Disilane combination of (3-isocyano propyl) triethoxysilane and dimethyldimethoxysilane is used, dominant groups of respective silane are fully utilized, the hydrophobicity of the spherical silica powder is remarkably improved through a modification process, the mixing uniformity of the spherical silica powder in an epoxy molding compound and a liquid packaging material base material is promoted, and the spherical silica powder has the advantages of high hydrophobicity, high hydrophobicity and high stability. Meanwhile, the application range of the spherical silica powder in the fields of electronic packaging and hydrophobic coatings is widened.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of inorganic non-metallic materials, and in particular relates to a method for modifying spherical silicon micropowder by using disilane. Background Art

[0002] Spherical silicon micropowder is a white powder with broad application prospects due to its high purity, fine particles, excellent dielectric properties, low thermal expansion coefficient, high thermal conductivity and other superior properties. Spherical silicon micropowder is a key material in the integrated circuit packaging and IC substrate industries. Spherical silicon micropowder can be used in epoxy molding compounds, liquid packaging materials and high-performance substrates for chip packaging. It also has many applications in high-tech fields such as aviation, aerospace, automobiles, the Internet of Things and special ceramics. Spherical silicon micropowder has the following characteristics: First, the main component SiO2 content of spherical silicon micropowder is more than 99.9%, which makes the performance of spherical silicon micropowder stable and ensures the reliability of related materials; second, the sphericity of spherical silicon micropowder can reach more than 0.93 (assuming that the sphericity of the standard sphere is 1), and the overall spheroidization rate is more than 90%, which reduces the effect of spherical silicon micropowder on the viscosity of the epoxy molding compound after being added to the epoxy molding compound, and improves the fluidity; third, spherical silicon micropowder has a high thermal conductivity, a low linear thermal expansion coefficient, and excellent dielectric properties, which shows outstanding comprehensive performance, which has a very important influence on the quality of epoxy molding compounds.

[0003] However, the application of silicon micropowder also has the following limitations. When silicon micropowder is used as the raw material of epoxy molding compound and liquid packaging material, as the filling amount increases, the viscosity of the system will increase sharply, the fluidity and permeability of the material will deteriorate, and the spherical silicon micropowder is difficult to disperse in the resin, and it is easy to agglomerate. Therefore, the surface modification of silicon micropowder is an important means of its deep processing. To do a good job in the surface modification of the powder, we must first base it on the mechanism of its surface modification, so that its surface properties change from hydrophilic to hydrophobic, thereby improving the wettability of the silicon micropowder surface and making the powder particles easier to disperse in organic compounds. For the modification of silicon micropowder, it will be found that there are two key issues that need to be solved. One is the choice of surfactant; the other is the process requirements and equipment selection of quartz powder surface modification, both of which determine the success or failure of surface modification.

[0004] Some technical methods for modifying the surface of spherical silicon micropowder have been applied in this technical field, but the cost of the raw materials and process methods used remains high, which has a certain hindering effect on the further application of spherical silicon micropowder. Summary of the invention

[0005] The present invention aims at providing a method for modifying spherical silicon micropowder by using disilane. The present invention is not only simple to operate and low in cost, but also has a good surface modification effect on the spherical silicon micropowder.

[0006] The technical solution of the present invention is specifically: a method for modifying spherical silicon powder using disilane, comprising the following steps:

[0007] S1. The spherical silicon powder was surface treated with 4-6 mol / L NaOH solution for 10-12 h, and then washed with pure water and anhydrous ethanol for 2-3 times, and dried in a vacuum drying oven at 90-120 ° C for 1-3 h to obtain the pretreated spherical silicon powder;

[0008] S2. The pretreated spherical silicon powder was added with deionized water at a mass volume ratio (g / ml) of 1:4-5, and then moved to a reaction device, and stirred at 60-100°C for 2-6h under nitrogen protection;

[0009] S3. According to the mass volume ratio (g / ml) of spherical silica powder and (3-isocyanatopropyl) triethoxysilane 2:0.1-10, (3-isocyanatopropyl) triethoxysilane was slowly added dropwise to the reaction apparatus, and the reaction was stirred at 60-100 ° C for 1-3h;

[0010] S4. According to the mass volume ratio of spherical silicon powder to dimethyldimethoxysilane (g / ml) of 2:1-20, dimethyldimethoxysilane was slowly added dropwise to the reaction apparatus, and the reaction was stirred at a temperature of 60-100 ° C for 2-4h;

[0011] S5. Filter the solid product obtained by the reaction in step S4, then wash it with pure water and anhydrous ethanol for 2-3 times respectively, filter the washed sample and put it into a vacuum drying oven, dry it at 90-120°C for 1-3h, and grind it to obtain modified spherical silicon powder.

[0012] Preferably, the concentration of the NaOH solution in step S1 is 5 mol / L, the surface is treated for 12 h, and dried at 105° C. in a vacuum drying oven for 2 h.

[0013] Preferably, in step S2, the mass volume ratio (g / ml) of the spherical silicon powder to deionized water is 1:5, the reaction apparatus is a conical flask, and the mixture is stirred at 500 rpm at 80° C. for 4 h under nitrogen protection.

[0014] Preferably, in step S3, the mass volume ratio (g / ml) of the spherical silicon powder to (3-isocyanatopropyl)triethoxysilane is 2:1, and the reaction device is stirred at 80° C. for 1 hour.

[0015] Preferably, in step S4, the mass volume ratio (g / ml) of the spherical silicon powder to dimethyldimethoxysilane is 1:5, and the reaction device is stirred at 80° C. for 2 hours.

[0016] Preferably, the washed sample in step S5 is filtered and placed in a vacuum drying oven, dried at 105° C. for 2 h, and ground to obtain modified spherical silicon powder.

[0017] The beneficial effects of the present invention are:

[0018] The first silane used in the present invention is (3-isocyanopropyl) triethoxysilane, which contains silicon-oxygen bonds and isocyanate groups. (3-isocyanopropyl) triethoxysilane can effectively combine organic matter with inorganic matter, and play a coupling role, which plays an important role in composite material preparation and modification. (3-isocyanopropyl) triethoxysilane can improve the wettability and adhesion of the material surface, making it easier to coat or bond. The second silane used in the present invention is dimethyldimethoxysilane, which is an organosilicon compound containing two methyldimethoxysilane groups, and has lower viscosity and better fluidity at room temperature. It has good wettability and dispersibility, and hydrolysis reaction can occur under certain conditions to generate silanol and methanol, thereby forming a silicon oxygen bond to combine with the matrix material.

[0019] The present invention uses two silanes to modify the surface of spherical silicon micropowder, which significantly improves the hydrophobicity of the spherical silicon micropowder, promotes the mixing uniformity of the spherical silicon micropowder in epoxy molding compound and liquid packaging material substrate, and broadens the application of spherical silicon micropowder in the field of electronic packaging and hydrophobic coating. In addition, the method of the present invention is not only low in cost, but also simple in preparation process, which is conducive to large-scale application. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention will be described in detail below in conjunction with the accompanying drawings, wherein:

[0021] Figure 1 The contact angle test diagrams of the spherical silicon micropowder modified in Example 1, the spherical silicon micropowder pretreated with sodium hydroxide only prepared in Comparative Example 1, and the spherical silicon micropowder raw material without any treatment;

[0022] Figure 2 The microscopic morphology detection diagram of the spherical silicon micropowder modified in Example 1, the spherical silicon micropowder pretreated with sodium hydroxide only prepared in Comparative Example 1, and the raw material of the spherical silicon micropowder without any treatment;

[0023] Figure 3 Contact angle test graphs of the modified spherical silicon micropowder prepared in Example 1, the spherical silicon micropowder modified with (3-isocyanatopropyl)triethoxysilane in Comparative Example 2, and the spherical silicon micropowder modified with dimethyldimethoxysilane in Comparative Example 3. DETAILED DESCRIPTION

[0024] The present invention is further described in detail below in combination with comparative examples and examples. It should be understood that the specific examples described herein are only used to explain the present invention and are not intended to limit the present invention.

[0025] Example 1

[0026] The method for modifying spherical silicon powder using disilane, the specific steps are as follows:

[0027] S1. The spherical silicon powder was surface treated with 5 mol / L NaOH solution for 12 h, then washed with pure water and anhydrous ethanol for 3 times, and dried in a vacuum drying oven at 105 ° C for 2 h to obtain the pretreated spherical silicon powder;

[0028] S2. Add the spherical silicon powder treated in step 1 to 10 ml of deionized water and transfer it to a three-necked flask. Stir it on a magnetic stirrer at 80°C for 4 h under nitrogen protection;

[0029] S3. Measure 1 ml (3-isocyanopropyl) triethoxysilane and add it to the separatory funnel, install it on the three-necked flask, open the valve and slowly drip the solution into the three-necked flask, and stir for 1 hour;

[0030] S4. Measure 10 ml of dimethyldimethoxysilane and add it to the separatory funnel, install it on the three-necked flask, open the valve and slowly add the solution dropwise into the three-necked flask, and stir for 2h;

[0031] S5. Filter the solid product obtained by the reaction in step S4, then wash it with pure water and anhydrous ethanol for 2-3 times respectively, filter the washed sample and put it into a vacuum drying oven, dry it at 105°C for 2h, and grind it to obtain modified spherical silicon powder.

[0032] Example 2

[0033] The method for modifying spherical silicon powder using disilane, the specific steps are as follows:

[0034] S1. The spherical silicon powder was surface treated with 5 mol / L NaOH solution for 12 h, then washed with pure water and anhydrous ethanol for 3 times, and dried in a vacuum drying oven at 105 ° C for 2 h to obtain the pretreated spherical silicon powder;

[0035] S2. Add the spherical silicon powder treated in step 1 to 10 ml of deionized water and transfer it to a three-necked flask. Stir it on a magnetic stirrer at 80°C for 4 h under nitrogen protection;

[0036] S3. 5 ml (3-isocyanopropyl) triethoxysilane was added to a separatory funnel and installed on a three-necked flask. The valve was opened to allow the solution to be slowly dripped into the three-necked flask and stirred for 1 h.

[0037] S4. Measure 10 ml of dimethyldimethoxysilane and add it to the separatory funnel, install it on the three-necked flask, open the valve and slowly add the solution dropwise into the three-necked flask, and stir for 2h;

[0038] S5. Filter the solid product obtained by the reaction in step S4, then wash it with pure water and anhydrous ethanol for 2-3 times respectively, filter the washed sample and put it into a vacuum drying oven, dry it at 105°C for 2h, and grind it to obtain modified spherical silicon powder.

[0039] Example 3

[0040] The method for modifying spherical silicon powder using disilane, the specific steps are as follows:

[0041] S1. The spherical silicon powder was surface treated with 5 mol / L NaOH solution for 10 h, then washed with pure water and anhydrous ethanol for 3 times, and dried in a vacuum drying oven at 105 ° C for 2 h to obtain the pretreated spherical silicon powder;

[0042] S2. Add the spherical silicon powder treated in step 1 to 10 ml of deionized water and transfer it to a three-necked flask. Stir it on a magnetic stirrer at 80°C for 4 h under nitrogen protection;

[0043] S3. 5 ml (3-isocyanopropyl) triethoxysilane was added to a separatory funnel and installed on a three-necked flask. The valve was opened to allow the solution to be slowly dripped into the three-necked flask and stirred for 1 h.

[0044] S4. Measure 20 ml of dimethyldimethoxysilane and add it to the separatory funnel, install it on the three-necked flask, open the valve and slowly drip the solution into the three-necked flask, and stir for 3h;

[0045] S5. Filter the solid product obtained by the reaction in step S4, then wash it with pure water and anhydrous ethanol for 2-3 times respectively, filter the washed sample and put it into a vacuum drying oven, dry it at 105°C for 2h, and grind it to obtain modified spherical silicon powder.

[0046] Comparative Example 1

[0047] A method for modifying spherical silicon powder, the specific steps are as follows:

[0048] S1. The spherical silicon micropowder was surface treated with 5 mol / L NaOH solution for 10 h, then washed with pure water and anhydrous ethanol for 3 times, and dried in a vacuum drying oven at 105°C for 2 h to obtain the treated spherical silicon micropowder.

[0049] S2. Wash with pure water and anhydrous ethanol for 2-3 times respectively, filter the washed sample and put it into a vacuum drying oven, dry it at 105°C for 2h, and grind it to obtain modified spherical silica powder.

[0050] Comparative Example 2

[0051] A method for modifying spherical silicon powder, the specific steps are as follows:

[0052] S1. The spherical silicon powder was surface treated with 5 mol / L NaOH solution for 12 h, then washed with pure water and anhydrous ethanol for 3 times, and dried in a vacuum drying oven at 105 ° C for 2 h to obtain the pretreated spherical silicon powder;

[0053] S2. Add the spherical silicon powder treated in step 1 to 10 ml of deionized water and transfer it to a three-necked flask. Stir it on a magnetic stirrer at 80°C for 4 h under nitrogen protection;

[0054] S3. Measure 1 ml (3-isocyanopropyl) triethoxysilane and add it to the separatory funnel, install it on the three-necked flask, open the valve and slowly drip the solution into the three-necked flask, and stir for 1 hour;

[0055] S4. Filter the solid product obtained by the reaction in step S3, then wash it with pure water and anhydrous ethanol for 2-3 times respectively, filter the washed sample and put it into a vacuum drying oven, dry it at 105°C for 2h, and grind it to obtain modified spherical silicon powder.

[0056] Comparative Example 3

[0057] A method for modifying spherical silicon powder, the specific steps are as follows:

[0058] S1. The spherical silicon powder was surface treated with 5 mol / L NaOH solution for 12 h, then washed with pure water and anhydrous ethanol for 3 times, and dried in a vacuum drying oven at 105 ° C for 2 h to obtain the pretreated spherical silicon powder;

[0059] S2. Add the spherical silicon powder treated in step 1 to 10 ml of deionized water and transfer it to a three-necked flask. Stir it on a magnetic stirrer at 80°C for 4 h under nitrogen protection;

[0060] S3. Measure 10 ml of dimethyldimethoxysilane and add it to the separatory funnel, install it on a three-necked flask, open the valve and slowly drip the solution into the three-necked flask, and stir for 2h;

[0061] S4. Filter the solid product obtained by the reaction in step S4, then wash it with pure water and anhydrous ethanol for 2-3 times respectively, filter the washed sample and put it into a vacuum drying oven, dry it at 105°C for 2h, and grind it to obtain modified spherical silicon powder.

[0062] The modified spherical silicon powder of Example 1 was taken, and the spherical silicon powder pretreated with sodium hydroxide prepared in Example 1 was compared with the spherical silicon powder raw material without any treatment, and the contact angle test was performed. Figure 1 The test results are shown.

[0063] Figure 1 (a) shows the contact angle picture of unmodified silicon micropowder; (b) shows the contact angle picture of silicon micropowder after pretreatment with sodium hydroxide; (c) shows the contact angle picture of silicon micropowder after modification in Example 1. It can be seen from the results in the figure that the unmodified silicon micropowder is a hydrophilic material. After the silicon micropowder is modified by (3-isocyanatopropyl)triethoxysilane and dimethyldimethoxysilane, a hydrophobic film is formed on the surface of the spherical silicon micropowder, which significantly improves the hydrophobicity of the surface of the spherical silicon micropowder.

[0064] The modified spherical silicon powder of Example 1 was taken, and the spherical silicon powder pretreated with sodium hydroxide prepared in Example 1 was compared with the spherical silicon powder raw material without any treatment, and the microscopic morphology was detected. Figure 2 The test results are shown.

[0065] Figure 2 (a) in the middle shows the microscopic morphology of the original silicon micropowder. It can be seen from the figure that the particle size of the silicon micropowder is uneven and there are impurities on the surface of the particles. Figure 2 (b) shows the silicon micropowder after being treated with sodium hydroxide. It can be clearly observed that the impurities on the surface of the spherical silicon micropowder are removed, and some particles are corroded to form small pits. Figure 2 (c) shows the modified silicon micropowder, with impurities attached to the particle surface. Compared with the original powder, the microscopic morphology has no obvious change. Since this experiment grafted siloxane onto the particle surface, the grafted siloxane is at the molecular level, so the surface morphology does not change significantly.

[0066] The modified spherical silicon powder prepared in Example 1, the spherical silicon powder modified with (3-isocyanatopropyl)triethoxysilane in Comparative Example 2, and the spherical silicon powder modified with dimethyldimethoxysilane in Comparative Example 3 were tested for contact angles. Figure 3 The test results are shown.

[0067] Figure 3 (a) shows the contact angle picture of silicon micropowder after modification in Example 1, (b) shows the contact angle picture of silicon micropowder after modification with (3-isocyanatopropyl)triethoxysilane, and (c) shows the contact angle picture of spherical silicon micropowder after modification with dimethyldimethoxysilane. It can be seen from the results in the figure that after the silicon micropowder is modified with (3-isocyanatopropyl)triethoxysilane and dimethyldimethoxysilane, the hydrophobicity of the surface of the spherical silicon micropowder is significantly improved.

[0068] The modified spherical silicon powder prepared in Example 2-3 was further subjected to contact angle test and microscopic morphology test, and the test results were similar to those of the example.

[0069] The above embodiments fully illustrate that the method disclosed in the present invention for modifying spherical silicon micropowder using disilane significantly improves the hydrophobicity of the spherical silicon micropowder, promotes the mixing uniformity of the spherical silicon micropowder in epoxy molding compounds and liquid packaging material substrates, and broadens the application of spherical silicon micropowder in the fields of electronic packaging and hydrophobic coatings.

Claims

1. A method for modifying spherical silicon powder using disilane, characterized in that: The following steps are involved: S1. The spherical silicon powder was surface treated with 4-6 mol / L NaOH solution for 10-12 h, and then washed with pure water and anhydrous ethanol for 2-3 times, and dried in a vacuum drying oven at 90-120 ° C for 1-3 h to obtain the pretreated spherical silicon powder; S2. The pretreated spherical silicon powder was added with deionized water at a mass volume ratio (g / ml) of 1:4-5, and then moved to a reaction device, and stirred at 60-100°C for 2-6h under nitrogen protection; S3. According to the mass volume ratio (g / ml) of spherical silica powder and (3-isocyanatopropyl) triethoxysilane 2:0.1-10, (3-isocyanatopropyl) triethoxysilane was slowly added dropwise to the reaction apparatus, and the reaction was stirred at 60-100 ° C for 1-3h; S4. According to the mass volume ratio of spherical silicon powder to dimethyldimethoxysilane (g / ml) of 2:1-20, dimethyldimethoxysilane was slowly added dropwise to the reaction apparatus, and the reaction was stirred at a temperature of 60-100 ° C for 2-4h; S5. Filter the solid product obtained by the reaction in step S4, then wash it with pure water and anhydrous ethanol for 2-3 times respectively, filter the washed sample and put it into a vacuum drying oven, dry it at 90-120°C for 1-3h, and grind it to obtain modified spherical silicon powder.

2. The method for modifying spherical silicon powder using disilane according to claim 1, characterized in that: The concentration of the NaOH solution in step S1 is 5 mol / L, the surface is treated for 12 h, and dried in a vacuum drying oven at 105° C. for 2 h.

3. The method for modifying spherical silicon powder using disilane according to claim 1, characterized in that: In step S2, the mass volume ratio (g / ml) of the spherical silicon powder to deionized water is 1:5, the reaction apparatus is a conical flask, and the mixture is stirred at 500 rpm for 4 h at 80° C. under nitrogen protection.

4. The method for modifying spherical silicon powder using disilane according to claim 1, characterized in that: In step S3, the mass volume ratio (g / ml) of the spherical silicon powder to (3-isocyanatopropyl)triethoxysilane is 2:1, and the reaction device is stirred at 80° C. for 1 hour.

5. The method for modifying spherical silicon powder using disilane according to claim 1, characterized in that: In step S4, the mass volume ratio (g / ml) of the spherical silicon powder to dimethyldimethoxysilane is 1:5, and the reaction device is stirred at 80° C. for 2 hours.

6. The method for modifying spherical silicon powder using disilane according to claim 1, characterized in that: The washed sample in step S5 is filtered and placed in a vacuum drying oven, dried at 105° C. for 2 h, and ground to obtain modified spherical silicon micropowder.

Citation Information

Cited By

  • Superfine high-purity spherical silica powder surface modification process

    CN119875395A