Manufacturing method of high-strength corrosion-resisting steel forged pipe fitting
By using chemical composition design with Cu, Si and other elements and a nano-metal crystal protective layer in steel forged pipe fittings, the problem of insufficient bonding force between coating and metal in the existing technology is solved, and high strength and corrosion resistance are achieved. promote.
Patent Information
- Application Number
- CN202410751325.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-12
- Publication Date
- 2024-10-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
In the existing surface anti-corrosion technology of steel forged pipe fittings, the bonding force between the coating and the metal body is insufficient, causing the pipe fittings to be easily damaged in a corrosive environment.
The chemical composition design of Cu, Si and other elements is used, and chlorine gas is introduced into the melt to perform a replacement reaction to remove impurities and form a uniform structure; then iron powder, chromium powder, and borax are used for mechanical grinding to prepare nano-metal crystals, and the upsetting and reverse processes are carried out. Extrusion-processing-extrusion-precision forging treatment to form a protective layer, and micro-oxidation thermal spraying of metal powder to form an oxide film to isolate the pipe fittings from contact with corrosive liquids.
It significantly improves the strength and corrosion resistance of pipe fittings, ensures a good combination of the protective layer and pipe fittings, enhances the anti-corrosion effect, and optimizes the strength performance of pipe fittings.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of forged pipe fittings, in particular to a method for manufacturing a high-strength corrosion-resistant steel forged pipe fitting. Background Art
[0002] Pipe fittings are widely used in modern life, and their main raw materials are steel alloys. Steel pipes are of great importance to the development of the national economy and the improvement of the quality of human life, far better than other steel materials. From people's daily utensils, furniture, water supply and drainage, gas supply, ventilation and heating facilities to the manufacture of various agricultural machinery and tools, the development of underground resources, guns, bullets, missiles, rockets used in national defense and aerospace, steel pipes are indispensable. Because steel pipes are inseparable from human life and production activities, the production technology of the steel pipe industry has not only developed rapidly, but also been innovative. Steel pipe production occupies an irreplaceable position in the steel industry. The existing surface anti-corrosion technologies for pipe fittings include electrogalvanizing and electrophoretic coating. The above technologies are all surface coatings of internal products, and the coatings do not have a good bonding force with the metal body. Summary of the invention
[0003] The object of the present invention is to provide a method for manufacturing a high-strength corrosion-resistant steel forged pipe fitting to solve the problems existing in the prior art.
[0004] In order to solve the above technical problems, the present invention provides the following technical solutions: A method for manufacturing a high-strength corrosion-resistant steel forged pipe fitting, comprising the following steps:
[0005] (1) preparing materials according to the following chemical composition and their mass percentage: Cu 1.2-1.4%, Si 0.7-0.9%, Ni 0.35-0.60%, C 0.05-0.1%, Mn 0.85-0.9%, Nb 0.02-0.035%, Mo 0.40-0.60%, Ti 0.01-0.2%, and the balance being Fe and unavoidable impurities, heating to 900-1000° C., keeping the temperature for 30 minutes, and then performing the first ventilation. After the ventilation is completed, heating to 1300-1400° C., keeping the temperature for 1 hour, heating to 1600-1650° C., and then performing the second ventilation after keeping the temperature for 1 hour. After the ventilation is completed, heating to 1750-1850° C., keeping the temperature for 1.5-2 hours, cooling to 1600-1620° C., and then performing the third ventilation, and then casting into a steel ingot;
[0006] (2) placing the steel ingot in a heating furnace, heating it to 840-890° C., keeping it at that temperature for 1-3 hours, then heating it to 1100-1200° C., keeping it at that temperature for 12-14 hours, then taking it out of the furnace, using a 165MN hydraulic press to upset it, and then back-extruding and punching it to obtain a hollow billet;
[0007] (3) After the mixed metal powder is melted into a liquid state, the temperature of the hollow billet is lowered to 720-760° C., and the liquid mixed metal powder is sprayed on the surface of the hollow billet in an argon / oxygen mixed atmosphere at a spraying rate of 0.2-0.4 mm / min. After the surface spraying is completed, it is air-cooled to room temperature to obtain a protective layer billet;
[0008] (4) heating the protective layer blank to 1060°C, keeping the temperature for 1.5 to 2 hours, extruding it into a tube blank at an extrusion speed of 35 to 45 mm / s and an extrusion ratio of 2 to 5, and cooling it to room temperature to obtain a tube blank;
[0009] (5) The tube blank is heated to 1000-1030°C, kept at this temperature for 2-3 hours, and then fine forged with a deformation rate of 10-15%, and then tempered at 415-435°C for 10-40 minutes, and cooled to room temperature to obtain a high-strength corrosion-resistant steel forged pipe fitting.
[0010] Furthermore, the specific process of the first ventilation in step (1) is: blowing chlorine gas into the bottom of the melt at 0.5-0.7 L / min·t for 15 minutes.
[0011] Furthermore, the specific process of the second ventilation in step (1) is: blowing chlorine gas into the bottom of the melt at 0.5-0.7 L / min·t for 25 minutes.
[0012] Furthermore, the specific process of the third ventilation in step (1) is: blowing chlorine gas into the bottom of the melt at 0.5-0.7 L / min·t for 10 minutes.
[0013] Furthermore, the upsetting condition in step (2) is: the forging ratio is 1.7.
[0014] Furthermore, the reverse extrusion punching condition in step (2) is: the punching ratio is 1.2 to 1.8.
[0015] Furthermore, the preparation method of the mixed metal powder in step (3) is: ball milling iron powder, borax and chromium powder in a mass ratio of 80:15-23:20-35, with a ball-to-material ratio of 15-20:1, a ball milling speed of 500-600rpm, and a ball milling time of 24h to obtain a mixed metal powder.
[0016] Furthermore, the volume fraction of oxygen in the argon / oxygen mixed atmosphere in step (3) is 0.5-5%.
[0017] Compared with the prior art, the beneficial effects achieved by the present invention are:
[0018] The present invention adopts innovative chemical composition design and combines elements such as Fe, Cu, Si, etc. to produce uniform steel billet structure, so that the strength performance of the pipe fittings is greatly improved. Si can be used to form a large number of heterogeneous cores, which plays a role in modifying and refining the main alloy phase, which is beneficial to improving the strength of the pipe fittings. In the smelting process, chlorine gas is intermittently introduced into the bottom to replace the gas in the melt. At the same time, the impurity elements are chlorinated to generate low-melting point chlorides that volatilize in the form of gas phase, thereby reducing the inclusion content, thereby effectively improving the quality of the steel billet and the strength of the pipe fittings. Then, a staged long-term heat treatment is performed, so that the elements can be fully diffused and evenly diffused, element segregation is eliminated, and a fine and stable structure is formed, thereby ensuring the high-strength product characteristics of the pipe fittings, which is beneficial to the later forging process. Then, a forging process of upsetting-reverse extrusion-processing-extrusion-fine forging is performed. The forging process completely breaks the initial grains, and at the same time, the extrusion speed in the forging process is controlled, thereby ensuring that there is sufficient time to complete dynamic recrystallization during the deformation process, thereby improving the performance of the pipe fittings.
[0019] During the processing, the present invention uses iron powder, chromium powder and borax as raw materials for mechanical grinding to break, refine and alloy them, and then obtain nano metal crystals, thereby ensuring that a protective layer can be formed more easily in the subsequent process, thereby achieving the purpose of corrosion resistance, and then micro-oxidation thermal spraying is performed to spray the molten powder in a mist form evenly on the surface of the pipe fitting. The residual heat of the powder can promote the formation of an oxide film on the pipe fitting, isolating the pipe fitting from direct contact with oxygen and corrosive liquids, and improving the corrosion resistance of the pipe fitting. In the subsequent forging process, the high-pressure forging force promotes better combination of the protective layer and the pipe fitting, improves the quality of the surface protective layer, increases the anti-corrosion effect, and optimizes the strength performance of the pipe fitting. DETAILED DESCRIPTION
[0020] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0021] Example 1
[0022] (1) The materials are prepared according to the following chemical composition and their mass percentage: Cu 1.2%, Si 0.7%, Ni 0.35%, C 0.05%, Mn 0.85%, Nb 0.02%, Mo 0.40%, Ti 0.01%, and the balance is Fe and unavoidable impurities. The temperature is raised to 900°C, kept at this temperature for 30 minutes, chlorine gas is blown into the bottom of the melt at 0.5 L / min·t for 15 minutes, ventilation is stopped, the temperature is raised to 1300°C, kept at this temperature for 1 hour, the temperature is raised to 1600°C, kept at this temperature for 1 hour, chlorine gas is blown into the bottom of the melt at 0.5 L / min·t for 25 minutes, ventilation is stopped, the temperature is raised to 1750°C, kept at this temperature for 1.5 hours, the temperature is lowered to 1600°C, chlorine gas is blown into the bottom of the melt at 0.5 L / min·t for 10 minutes, and cast into a steel ingot;
[0023] (2) placing the steel ingot in a heating furnace, heating it to 840°C, keeping it at that temperature for 1 hour, then heating it to 1100°C, keeping it at that temperature for 12 hours, and then taking it out of the furnace, using a 165MN hydraulic press to upset it, with a forging ratio of 1.7, and then back-extrusion punching it, with a punching ratio of 1.2, to obtain a hollow billet;
[0024] (3) ball milling iron powder, borax and chromium powder in a mass ratio of 80:15:20, a ball-to-material ratio of 15:1, a ball milling speed of 500 rpm, and a ball milling time of 24 h to obtain a mixed metal powder. After melting into a liquid state, the hollow billet is cooled to 720° C. In an argon / oxygen mixed atmosphere, the liquid mixed metal powder is sprayed on the surface of the hollow billet at a spraying rate of 0.2 mm / min. After the surface spraying is completed, air cooling is performed to room temperature to obtain a protective layer billet; the volume fraction of oxygen in the argon / oxygen mixed atmosphere is 0.5%;
[0025] (4) The protective layer blank is heated to 1060°C, kept at this temperature for 1.5 hours, and then extruded into a tube blank at an extrusion speed of 35 mm / s and an extrusion ratio of 2. The tube blank is then cooled to room temperature;
[0026] (5) The tube blank is heated to 1000°C, kept at this temperature for 2 hours, and then fine forged with a deformation rate of 10%. It is then tempered at 415°C for 10 minutes and cooled to room temperature to obtain a high-strength corrosion-resistant steel forged pipe fitting.
[0027] Example 2
[0028] (1) The materials are prepared according to the following chemical composition and their mass percentage: Cu 1.25%, Si 0.79%, Ni 0.51%, C 0.077%, Mn 0.87%, Nb 0.029%, Mo 0.51%, Ti 0.03%, and the balance is Fe and unavoidable impurities. The temperature is raised to 950°C, and after being kept at this temperature for 30 minutes, chlorine gas is blown into the bottom of the melt at 0.6 L / min·t for 15 minutes, and ventilation is stopped. The temperature is then raised to 1350°C, and after being kept at this temperature for 1 hour, the temperature is then raised to 1622°C, and after being kept at this temperature for 1 hour, chlorine gas is blown into the bottom of the melt at 0.6 L / min·t for 25 minutes, and ventilation is stopped. The temperature is then raised to 1760°C, and after being kept at this temperature for 1.8 hours, the temperature is then lowered to 1610°C, and chlorine gas is blown into the bottom of the melt at 0.6 L / min·t for 10 minutes, and cast into a steel ingot.
[0029] (2) placing the steel ingot in a heating furnace, heating it to 870°C, keeping it at that temperature for 2 hours, then heating it to 1150°C, keeping it at that temperature for 13 hours, and then taking it out of the furnace. It was upset by a 165MN hydraulic press with a forging ratio of 1.7, and then back-extruded and punched with a punching ratio of 1.4 to obtain a hollow billet.
[0030] (3) ball milling iron powder, borax and chromium powder in a mass ratio of 80:19:28, a ball-to-material ratio of 18:1, a ball milling speed of 550 rpm, and a ball milling time of 24 h to obtain a mixed metal powder. After melting into a liquid state, the hollow billet is cooled to 740° C. In an argon / oxygen mixed atmosphere, the liquid mixed metal powder is sprayed on the surface of the hollow billet at a spraying rate of 0.3 mm / min. After the surface spraying is completed, the billet is air-cooled to room temperature to obtain a protective layer billet; the volume fraction of oxygen in the argon / oxygen mixed atmosphere is 1.2%;
[0031] (4) The protective layer blank is heated to 1060°C, kept at this temperature for 1.7 hours, and then extruded into a tube blank at an extrusion speed of 40 mm / s and an extrusion ratio of 3. The tube blank is then cooled to room temperature;
[0032] (5) The tube blank is heated to 1015°C, kept at this temperature for 3 hours, and then fine forged with a deformation rate of 12%. It is then tempered at 422°C for 25 minutes and cooled to room temperature to obtain a high-strength corrosion-resistant steel forged pipe fitting.
[0033] Example 3
[0034] (1) The ingredients are prepared according to the following chemical composition and their mass percentage: Cu 1.4%, Si 0.9%, Ni 0.60%, C 0.1%, Mn 0.9%, Nb 0.035%, Mo 0.60%, Ti 0.2%, and the balance is Fe and unavoidable impurities. The temperature is raised to 1000° C., and after being kept at this temperature for 30 minutes, chlorine gas is blown into the bottom of the melt at 0.7 L / min·t for 15 minutes, and ventilation is stopped. The temperature is then raised to 1400° C., and after being kept at this temperature for 1 hour, the temperature is then raised to 1650° C., and after being kept at this temperature for 1 hour, chlorine gas is blown into the bottom of the melt at 0.7 L / min·t for 25 minutes, and ventilation is stopped. The temperature is then raised to 1850° C., and after being kept at this temperature for 2 hours, the temperature is then lowered to 1620° C., and chlorine gas is blown into the bottom of the melt at 0.7 L / min·t for 10 minutes, and cast into a steel ingot.
[0035] (2) placing the steel ingot in a heating furnace, heating it to 890°C, keeping it at that temperature for 3 hours, then heating it to 1200°C, keeping it at that temperature for 14 hours, and then taking it out of the furnace, using a 165MN hydraulic press to upset it, with a forging ratio of 1.7, and then back-extrusion punching it, with a punching ratio of 1.8, to obtain a hollow billet;
[0036] (3) ball milling iron powder, borax and chromium powder in a mass ratio of 80:23:35, a ball-to-material ratio of 20:1, a ball milling speed of 600 rpm, and a ball milling time of 24 h to obtain a mixed metal powder. After melting into a liquid state, the hollow billet is cooled to 760° C. In an argon / oxygen mixed atmosphere, the liquid mixed metal powder is sprayed on the surface of the hollow billet at a spraying rate of 0.4 mm / min. After the surface spraying is completed, air cooling is performed to room temperature to obtain a protective layer billet; the volume fraction of oxygen in the argon / oxygen mixed atmosphere is 5%;
[0037] (4) heating the protective layer blank to 1060°C, keeping it at this temperature for 2 hours, extruding it into a tube blank at an extrusion speed of 45 mm / s and an extrusion ratio of 2 to 5, and cooling it to room temperature to obtain a tube blank;
[0038] (5) The tube blank is heated to 1030°C, kept at this temperature for 2 to 3 hours, and then fine forged with a deformation rate of 15%, and then tempered at 435°C for 40 minutes and cooled to room temperature to obtain a high-strength corrosion-resistant steel forged pipe fitting.
[0039] Comparative Example 1
[0040] The difference between Comparative Example 1 and Example 3 lies in step (1). Step (1) is modified as follows: the ingredients are prepared according to the following chemical composition and their mass percentage: Cu 1.4%, Si 0.9%, Ni 0.60%, C 0.1%, Mn 0.9%, Nb 0.035%, Mo 0.60%, Ti 0.2%, and the balance is Fe and unavoidable impurities; the temperature is raised to 1850° C. and kept warm for 2 h. Chlorine gas is blown into the bottom of the melt at 0.7 L / min·t for 10 min, and the steel is cast into a steel ingot; the remaining steps are the same as those in Example 3.
[0041] Comparative Example 2
[0042] The difference between Comparative Example 2 and Example 3 lies in step (1), in which step (1) is modified as follows: the ingredients are prepared according to the following chemical composition and their mass percentage: Cu 1.4%, Si 0.9%, Ni 0.60%, C 0.1%, Mn 0.9%, Nb 0.035%, Mo 0.60%, Ti 0.2%, and the balance is Fe and unavoidable impurities; the temperature is raised to 1850°C, kept warm for 2 hours, and cast into a steel ingot; the remaining steps are the same as those in Example 3.
[0043] Comparative Example 3
[0044] The difference between Comparative Example 3 and Example 3 is that before upsetting, the temperature is kept at 1200° C. for 2 hours, and the other steps are the same as Example 3.
[0045] Comparative Example 4
[0046] The difference between Comparative Example 4 and Example 3 is that the iron powder, borax and chromium powder are not ball-milled but directly mixed and melted, and the remaining steps are the same as Example 3.
[0047] Comparative Example 5
[0048] The difference between Comparative Example 5 and Example 3 is that extrusion and precision forging are performed first, and then the molten mixed metal powder is sprayed. The remaining steps are the same as Example 3.
[0049] Effect example
[0050] Table 1 below shows the tensile strength and corrosion resistance of the forged pipes of Examples 1 to 3 of the present invention and Comparative Examples 1 to 5 in a NaCl solution. The results are as follows:
[0051] Table 1
[0052] Tensile strength(MPa) Corrosion rate (mm / year) Example 1 1150 0.01078 Example 2 1157 0.01070 Example 3 1158 0.01064 Comparative Example 1 1012 0.01066 Comparative Example 2 1005 0.01070 Comparative Example 3 1088 0.01075 Comparative Example 4 1130 0.02248 Comparative Example 5 1118 0.02397
[0053] From the comparison of the experimental data of the embodiment and the comparative example, it can be found that the present invention has a homogenized steel billet structure produced by innovative chemical composition design, which greatly improves the strength performance of the pipe fittings, and utilizes the forging treatment of upsetting-reverse extrusion-processing-extrusion-fine forging to completely break, deform, and recrystallize the initial grains in the pipe fittings, thereby improving the performance of the pipe fittings. In addition, during the processing, the present invention uses iron powder, chromium powder, and borax as raw materials for mechanical grinding to break, refine, and alloy them, thereby obtaining nano-metal crystals, and then performs micro-oxidation hot spraying to evenly spray the molten powder on the surface of the pipe fitting in the form of mist. The residual heat of the powder can promote the formation of an oxide film on the pipe fitting, isolating the pipe fitting from direct contact with oxygen and corrosive liquids, and improving the corrosion resistance of the pipe fittings. In the subsequent forging process, the high-pressure forging force promotes better combination of the protective layer and the pipe fitting, improves the quality of the surface protective layer, increases the anti-corrosion effect, and optimizes the strength performance of the pipe fittings.
[0054] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.
Claims
1. A method for manufacturing a high-strength corrosion-resistant steel forged pipe fitting, characterized in that: The following steps are involved: (1) preparing materials according to the following chemical composition and their mass percentage: Cu 1.2-1.4%, Si 0.7-0.9%, Ni 0.35-0.60%, C 0.05-0.1%, Mn 0.85-0.9%, Nb 0.02-0.035%, Mo 0.40-0.60%, Ti 0.01-0.2%, and the balance being Fe and unavoidable impurities, heating to 900-1000° C., keeping the temperature for 30 minutes, and then performing the first ventilation. After the ventilation is completed, heating to 1300-1400° C., keeping the temperature for 1 hour, heating to 1600-1650° C., and then performing the second ventilation after keeping the temperature for 1 hour. After the ventilation is completed, heating to 1750-1850° C., keeping the temperature for 1.5-2 hours, cooling to 1600-1620° C., and then performing the third ventilation, and then casting into a steel ingot; (2) placing the steel ingot in a heating furnace, heating it to 840-890° C., keeping it at that temperature for 1-3 hours, then heating it to 1100-1200° C., keeping it at that temperature for 12-14 hours, then taking it out of the furnace, using a 165MN hydraulic press to upset it, and then back-extruding and punching it to obtain a hollow billet; (3) After the mixed metal powder is melted into a liquid state, the temperature of the hollow billet is lowered to 720-760° C., and the liquid mixed metal powder is sprayed on the surface of the hollow billet in an argon / oxygen mixed atmosphere. After the surface spraying is completed, the billet is air-cooled to room temperature to obtain a protective layer billet; (4) heating the protective layer blank to 1060°C, keeping it warm for 1.5 to 2 hours, extruding it into a tube blank, and cooling it to room temperature to obtain a tube blank; (5) The tube blank is heated to 1000-1030°C, kept at this temperature for 2-3 hours, and then fine forged with a deformation rate of 10-15%, and then tempered at 415-435°C for 10-40 minutes, and cooled to room temperature to obtain a high-strength corrosion-resistant steel forged pipe fitting.
2. The method for manufacturing a high-strength corrosion-resistant steel forged pipe fitting according to claim 1, characterized in that: The specific process of the first ventilation in step (1) is: blowing chlorine gas into the bottom of the melt at 0.5-0.7 L / min·t for 15 minutes.
3. The method for manufacturing a high-strength corrosion-resistant steel forged pipe fitting according to claim 1, characterized in that: The specific process of the second ventilation in step (1) is: blowing chlorine gas into the bottom of the melt at 0.5-0.7 L / min·t for 25 minutes.
4. The method for manufacturing a high-strength corrosion-resistant steel forged pipe fitting according to claim 1, characterized in that: The specific process of the third ventilation in step (1) is: blowing chlorine gas into the bottom of the melt at 0.5-0.7 L / min·t for 10 minutes.
5. The method for manufacturing a high-strength corrosion-resistant steel forged pipe fitting according to claim 1, characterized in that: The upsetting condition in step (2) is: the forging ratio is 1.
7.
6. The method for manufacturing a high-strength corrosion-resistant steel forged pipe fitting according to claim 1, characterized in that: The reverse extrusion punching conditions in step (2) are as follows: the punching ratio is 1.2 to 1.
8.
7. The method for manufacturing a high-strength corrosion-resistant steel forged pipe fitting according to claim 1, characterized in that: The preparation method of the mixed metal powder in step (3) is as follows: iron powder, borax and chromium powder are ball-milled in a mass ratio of 80:15-23:20-35, the ball-to-material ratio is 15-20:1, the ball-milling speed is 500-600rpm, and the ball-milling time is 24h to obtain the mixed metal powder.
8. The method for manufacturing a high-strength corrosion-resistant steel forged pipe fitting according to claim 1, characterized in that: The volume fraction of oxygen in the argon / oxygen mixed atmosphere in step (3) is 0.5-5%.
9. The method for manufacturing a high-strength corrosion-resistant steel forged pipe fitting according to claim 1, characterized in that: The spraying conditions in step (3) are: a rate of 0.2 to 0.4 mm / min.
10. The method for manufacturing a high-strength corrosion-resistant steel forged pipe fitting according to claim 1, characterized in that: The extrusion conditions in step (4) are: extrusion speed 35-45 mm / s, extrusion ratio 2-5.
Citation Information
Patent Citations
X100 anti-large deformation pipe steel and manufacturing technology thereof
CN102465235A
Steel for welding structure with excellent marine environment corrosion resistance and manufacturing method of steel
CN104419871A
Hot-rolled steel & method for manufacturing hot-rolled steel
CN111630200A
Preparation method of low-alloy wear-resistant steel
CN114032438A
Niobium-containing low-carbon manganese steel pipe for maritime work machinery and manufacturing method of niobium-containing low-carbon manganese steel pipe
CN117758147A