Detection method for brazing filler metal interface in-situ reaction and application
Through the method of gradient temperature field heat treatment and microscopic characterization, the problem in the existing technology of detecting the in-situ reaction of the cored solder interface is solved, and the accurate detection of the interface reaction during the brazing process is achieved, which reduces the cost and is suitable for observing volatility. flux.
Patent Information
- Application Number
- CN202411037450.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-10-08
AI Technical Summary
The existing technology lacks a direct and accurate method to detect the in-situ reaction mechanism at the interface between the solder skin and powder core in flux-core solder, resulting in the inability to determine whether there is an interface reaction during the welding process, and the commonly used methods are costly and unsuitable for observing volatilization. Sex flux.
The test sample is heat treated by setting up a gradient temperature field to obtain regions with different melting states. After cooling, the cross-sections of each region are microscopically characterized to infer the interface in-situ reaction mechanism.
This method makes it easier and more accurate to demonstrate the interface reaction and organizational evolution between the filler metal and the base metal or cored filler metal during the brazing process, avoids the shortcomings of static characterization, reduces costs, and is suitable for observing volatile fluxes.
Smart Images

Figure CN118746592A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of brazing, and in particular to a method for detecting an in-situ reaction of a brazing material interface and an application thereof. Background Art
[0002] Flux-cored brazing filler metal consists of a brazing filler metal outer skin and a powder core mixed with a brazing flux and alloy powder. Compared with the combined brazing of conventional brazing filler metal and brazing flux, flux-cored brazing filler metal has the advantages of easy operation, clean and environmentally friendly, high welding quality, wide application, and beautiful joints. It is also used in welding fields such as general mechanical parts, aircraft, ships, and lighting. During the brazing process of flux-cored brazing filler metal, the brazing filler metal outer skin reacts with the powder core in situ to form a new brazing filler metal melt, thereby improving the spreading behavior and wetting properties of the brazing filler metal. In the process of designing the composition of flux-cored brazing filler metal and determining the brazing process parameters, if the microstructure evolution behavior in the flux-cored brazing filler metal can be revealed based on the interface reaction mechanism between the flux-cored brazing filler metal outer skin and the powder core, it will be effective to develop or optimize the flux-cored brazing filler metal products and provide brazing method parameters that match them.
[0003] At present, the most common method for exploring in-situ reactions is to heat the flux core brazing material until it melts and then take the condensed sample for microscopic static characterization, and speculate on the interface reaction mechanism based on the compatibility of the solidified structure of the melt formed by the outer skin and the powder core, the interface state, etc. In other words, there is no clear and direct characterization method for the in-situ reaction at the interface between the brazing material outer skin and the powder core.
[0004] Furthermore, if there is no interface between the brazing material skin and the powder core melt in the brazing solidification structure, it is impossible to determine whether the brazing material skin and the powder core interface react in situ to form a new phase during the brazing heating process. In addition, for some types of brazing materials, the interface between the brazing material skin and the powder core during the brazing process can be observed by laser scanning confocal microscopy. However, this method requires the cavity to be in a vacuum environment and the sample cannot volatilize. Usually, the brazing flux in the flux-cored brazing material volatilizes, seriously contaminates the cavity and makes it impossible to observe, and the cost of the experiment is relatively high.
[0005] In view of this, the present invention is proposed. Summary of the invention
[0006] The first purpose of the present invention is to provide a method for detecting in-situ reaction of solder interface, which is used to solve the technical gap in the detection method of accurate microstructure evolution behavior and interface in-situ reaction principle in flux-cored solder. At the same time, the detection method can also be used to explore the interface reaction principle between the base material and the solder in conventional brazing.
[0007] The second object of the present invention is to provide a method for preparing a flux-cored solder.
[0008] A third object of the present invention is to provide a method for brazing a flux-cored solder.
[0009] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted: A method for detecting an in-situ reaction of a solder interface comprises the following steps: A gradient temperature field is set, and the test sample is heat treated to obtain the first melting zone, the second melting zone, the third melting zone and the unmelted zone with different melting states; after cooling, cross-sectional samples of each zone are taken for microscopic characterization, and the mechanism of in-situ reaction at the heterometallic interface is obtained based on the evolution of the organizational characteristics of each zone; Wherein, the test sample includes flux-cored solder or a combination of solder and base material.
[0010] A method for preparing a flux-cored solder includes a method for detecting an in-situ reaction of a solder interface.
[0011] A method for brazing a flux-cored solder includes a method for detecting an in-situ reaction of a solder interface.
[0012] Compared with the prior art, the present invention has the following beneficial effects: The present invention rapidly heats different parts of the test sample to different temperatures, so that the temperature outside has a certain temperature gradient field, and maintains it for a short time; at this time, the corresponding areas are obtained: unmelted area, partially melted area, completely melted but uneven composition area and completely melted and uniform composition area; then the flux cored solder is rapidly cooled to room temperature, and the different cross-sectional structures of the flux cored solder after solidification are microscopically characterized; from the characterization results, it can be inferred that any interface in-situ reaction mechanism during the brazing process can be summarized as: melting of solder during heat treatment, diffusion melting (between the base material and the solder, or between the outer skin and the inner core of the flux cored solder), and solidification behavior of the alloy melt during cooling. Compared with the static characterization of the solidified structure after complete melting in the prior art, the detection method of the present invention is easier and more accurate to show the interface reaction and organizational evolution between the flux cored solder or the solder and the base material, while the previous static characterization could not infer the accurate interface reaction behavior. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0014] Figure 1 A schematic diagram of in-situ reaction detection of a flux-cored solder of the present invention is provided; Figure 2 A schematic diagram of the in-situ reaction detection of the parent material-solder of the present invention is provided; Figure 3 The SEM image of Example 1 of the present invention is provided; wherein, Figure 3 (1) SEM image of the completely melted component uniform area corresponding to Example 1, Figure 3 (2) SEM image of the completely melted component inhomogeneous region corresponding to Example 1, Figure 3 (3) SEM image corresponding to the partial melting zone of Example 1, Figure 3 (4) corresponds to the SEM image of the non-melting zone in Example 1. DETAILED DESCRIPTION
[0015] The technical scheme of the present invention will be clearly and completely described below in conjunction with the accompanying drawings and specific embodiments, but those skilled in the art will appreciate that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work are within the scope of protection of the present invention. Those who do not specify specific conditions in the embodiments are carried out according to conventional conditions or conditions recommended by the manufacturer. Those who do not specify the manufacturer for reagents or instruments used are conventional products that can be purchased commercially. In addition, the terms "first", "second", "1", "2" are only used for descriptive purposes and cannot be interpreted as indicating or suggesting relative importance.
[0016] The first aspect of the present invention is to provide a method for detecting in-situ reactions at solder interfaces, the method comprising: setting a gradient temperature field, and heat treating a test sample to obtain a first melting zone, a second melting zone, a third melting zone, and an unmelted zone with different melting states; after cooling, cross-sectional samples of each zone are taken for microscopic characterization, and the mechanism of in-situ reactions at the interface of dissimilar metals is obtained based on the evolution of the organizational characteristics of each zone; wherein the test sample comprises a flux-cored solder or a combination of a solder and a base material.
[0017] As a preferred embodiment, the flux-cored solder described in the present invention can be any mixture including an outer skin and an inner core structure and having the function of a solder; according to the purpose of the detection, the flux-cored solder can be an existing finished product or a test product in the research and development stage; the present invention does not impose any limitation on the composition or source of the flux-cored solder. It can be understood that the detection method described in the present invention can be used for the research and development or optimization of the composition of the sample of the flux-cored solder, or it can be used to explore the brazing method of the sample of the flux-cored solder with a fixed composition. Therefore, the composition or source of the flux-cored solder can be arbitrarily replaced or the formula adjusted during the progress of the detection method.
[0018] As a preferred embodiment, the combination of the solder and the base material can also be any metal component with solder function, and the base material can be any element to be welded; this also means that in addition to being applied to the flux-cored solder, the present invention can also be applied to any lamellar heterogeneous material used to connect the brazing interface, for studying its interface reaction mechanism and the formation order of new phases.
[0019] As a preferred embodiment, when the sample to be tested is the flux-cored solder, the gradient temperature field is annularly or tubularly arranged on the periphery of the flux-cored solder to achieve uniform heating of the flux-cored solder; when the sample to be tested is a combination of the solder and a base material, the gradient temperature field is set at 645°C~760°C, including but not limited to any one of 645, 650, 660, 670, 680, 690, 700, 710, 720, 730, 740, 750, 760 (°C) or a numerical range consisting of any two of them.
[0020] As a preferred embodiment, the heat source of the gradient temperature field includes but is not limited to flame, electric arc, resistance, induction heat, laser or high-frequency electromagnetic field, etc.; in some more preferred embodiments, the construction of the gradient temperature field is carried out through a plurality of induction coils and can be carried out in an atmospheric environment.
[0021] As a preferred embodiment, the gradient temperature field includes a first temperature zone, a second temperature zone and a third temperature zone, and the heat source temperature corresponding to the first temperature zone is greater than that of the second temperature zone, and the heat source temperature of the second temperature zone is greater than that of the third temperature zone; further, the first temperature zone corresponds to the first melting zone and the second melting zone of the test sample, the second temperature zone corresponds to the third melting zone of the test sample, and the third temperature zone corresponds to the unmelted zone of the test sample.
[0022] It is worth noting that these three temperature zones correspond to test segments of a certain test sample, and the corresponding test samples in the three temperature zones should be continuous and complete; that is, the first temperature zone and the second temperature zone are spatially connected to each other without overlapping, the second temperature zone and the third temperature zone are spatially connected to each other without overlapping, and the first temperature zone and the third temperature zone are spatially not connected and are separated by the second temperature zone.
[0023] Furthermore, in the present invention, the first temperature zone, the second temperature zone and the third temperature zone with decreasing temperature are obtained based on the gradient temperature field; wherein the temperature of the first temperature zone is higher than the melting point of the test sample, the temperature of the second temperature zone is close to the melting point of the test sample, and the temperature of the third temperature zone is much lower than the melting point of the test sample. It should also be noted that although the temperature is divided into various temperature zones, there is also a trend of gradient change in temperature within each temperature zone, which does not mean that the temperature corresponding to any point in a certain temperature zone is the same.
[0024] As a more preferred embodiment, the temperature setting of the gradient temperature field satisfies the following definition: within the range of the first temperature zone, based on the heat Q1 absorbed by the edge of the test sample, Q1=Q0-Q2-Q3>Q2, wherein Q0 is the Joule heat generated by the heat source in the first temperature zone, Q2 is the heat conducted outward from the core solder corresponding to the first temperature zone, and Q3 is the heat dissipated from the heat source in the first temperature zone to the environment.
[0025] As a further preferred embodiment, the melting point of the flux-cored solder is used as the measurement. Specifically, since the flux-cored solder is a mixture, the melting point of a component with the highest melting point should be used as the measurement, usually the melting point of the solder outer skin, which is named "highest melting point" in the present invention. Correspondingly, the melting point of a component with the lowest melting point in the flux-cored solder is named "lowest melting point". A heat source is set at the edge of the test section of the flux-cored solder, and the temperature of the heat source is at least 10°C higher than the highest melting point.
[0026] like Figure 1 The figure provides a schematic diagram of the heat source, the temperature zone and the melting zone of the flux-cored solder. Based on the heat source, the temperature of the solder decreases from the first to the third temperature zones and forms the gradient temperature field. In some optional embodiments, a second heat source is set in the middle of the test section of the flux-cored solder to maintain the second melting zone to achieve its corresponding melting state. Similarly, Figure 2 The diagram shown is a schematic diagram of the melting zone, heat source, and temperature zone formed by the combination of the base material and the solder. However, it should be noted that Figure 1 , Figure 2 The length setting of the melting zone, the position setting of the heat source, etc. shown are only schematic and are not equivalent to the inherent length or position set in actual implementation.
[0027] As a further preferred embodiment, during the heat treatment, the heat source temperature ≥ the temperature of the cored solder in the first temperature zone ≥ the highest melting point of the cored solder; the lowest melting point of the cored solder < the temperature of the cored solder in the second temperature zone < the highest melting point of the cored solder; the temperature of the cored solder in the third temperature zone can be regarded as the test room temperature (20°C~30°C), or the air temperature of a conventional brazing workshop (10°C~40°C). In some optional embodiments, during the heat treatment, the temperature of the cored solder in the first melting zone is the heat source temperature, i.e., the highest melting point of the cored solder + 10°C, and the temperature of the cored solder in the second melting zone is equal to the highest melting point; in some optional embodiments, 649°C < the temperature of the cored solder in the second temperature zone < 758°C.
[0028] Based on the above embodiment, after the heat treatment and before cooling, the test sample corresponding to the first temperature zone is in a molten state, the test sample corresponding to the second temperature zone is in a partially molten paste state, and the test sample corresponding to the third temperature zone is in an unmelted solid state. By sampling and analyzing each temperature zone and the melting zone, the mechanism of the in-situ reaction at the heterometallic interface can be obtained.
[0029] Furthermore, each temperature zone is analyzed corresponding to each melting zone of the flux-cored solder; according to the different reaction degrees between the solder skin and the powder core during the brazing process of the flux-cored solder, the melting and bonding degrees of the solder skin into the powder core melt are different through the division of gradient temperature field and temperature zones; after the subsequent cooling process, the solder skin and the flux core in the first temperature zone are completely melted in the powder core melt and solidified, but since the first melting zone is close to the heat source, the solute elements in the melted liquid phase are completely diffused and the solute is evenly distributed, achieving a complete reaction between the skin and the flux core, and no obvious interface is seen in the microscopic characterization of the cross-sectional sample at this time; correspondingly, although the second melting zone, which also corresponds to the first temperature zone, is also completely melted into a liquid phase, due to insufficient thermal power of the reaction, the solute elements are incompletely diffused and the solute is unevenly distributed in the liquid phase, indicating that a complete interface reaction has occurred between the skin and the powder core, but the homogenization after the interface reaction has not yet been completed. In the third melting zone corresponding to the second temperature zone, the flux-cored solder partially melts and is in a liquid-solid two-phase state, indicating that the outer skin and the powder core are partially fused in situ. In the unmelted zone corresponding to the third temperature, the flux-cored solder does not melt, indicating that the solder outer skin and the powder core are not fused, and whether a solid-state phase change occurs is further analyzed in combination with microscopic characterization. Similarly, in the case where the test sample is a combination of the solder and the base material, the solder outer skin and the powder core of the flux-cored solder can be replaced with the base material and the solder.
[0030] For any of the flux-cored solders, the outer skin and the powder core have good heat transfer properties, so that the flux-cored solder has relatively stable first to third melting zones and unmelted zones during the heating process; in order to avoid the migration of the four different melting zones, a faster heating rate is required. This is because a lower heating rate will result in the solder outer skin and the alloy powder having enough time to transfer heat, and different transition zones cannot exist. In addition, in order to obtain the solidification structure of the completely melted but uneven composition zone and the completely melted and uniform composition zone, as well as the interface reaction structure during the heating process, the flux-cored solder needs to be quickly cooled after a short heat preservation. As a preferred embodiment, the heating rate of the heat source in the gradient temperature field is 4°C / s to 20°C / s, including but not limited to any one of 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20 (°C / s) or a numerical range consisting of any two of them; in some more preferred embodiments, the heating rate of the heat source in the gradient temperature field is 7°C / s.
[0031] As a preferred embodiment, the holding time of the heat treatment is 15s~60s, including but not limited to any one of 15, 20, 25, 30, 35, 40, 45, 50, 55, 60 (s) or a numerical range consisting of any two of them; in some more preferred embodiments, the holding time of the heat treatment is 30s.
[0032] As a preferred implementation manner, the cooling rate is ≥20°C / s.
[0033] In the present invention, the four melting zones of the test sample correspond to: a completely melted and uniform composition zone, a completely melted and non-uniform composition zone, a partially melted zone, and an incompletely melted zone. Through microstructural characterization, it can be seen that the heat treatment process of the flux-cored solder mainly includes: the dissolution of the flux, the melting of the alloy powder core, and the melting of the solder outer skin into the alloy powder core melt, wherein the solder outer skin and the powder core melt interface react or do not react, and the formed structure is mainly obtained through solidification behavior during the cooling process.
[0034] As a preferred embodiment, the microscopic characterization method includes but is not limited to optical microscopy, electron scanning microscopy, X-ray diffraction analysis, etc.
[0035] The "mechanism of in-situ reaction obtained based on the evolution of organizational characteristics of each zone" described in the present invention includes: obtaining the changes in the organization of the melt at the interface between the outer skin and the powder core in the flux-cored solder through a microscopic characterization spectrum, and then obtaining the in-situ reaction mechanism of the interface between the outer skin and the powder core during brazing.
[0036] Wherein, when the test sample is the flux-cored brazing filler metal, the obtained in-situ reaction mechanism includes: brazing flux dissolution, alloy powder core melting, diffusion melting of the brazing filler metal outer skin into the alloy powder core melt, and solidification behavior of the brazing filler metal alloy melt during cooling. When the test sample is a combination of the brazing filler metal and a base material, the obtained in-situ reaction mechanism includes: melting of the brazing filler metal, homogenization of the composition, and solidification behavior of the brazing filler metal alloy melt during cooling.
[0037] The second aspect of the present invention is to provide a method for preparing a flux-cored solder; it can be understood that the method for detecting the in-situ reaction of the flux-cored solder interface described in the first aspect of the present invention can be used in the research and development or preparation process of the flux-cored solder, and thus can be used as a pre-step in the method for preparing the flux-cored solder; when including the method for detecting the in-situ reaction of the flux-cored solder interface described in the present invention, any preparation method belongs to an embodiment of the present invention.
[0038] The third aspect of the present invention is to provide a method for brazing a flux-cored solder; it can be understood that the method for detecting the in-situ reaction of the flux-cored solder interface described in the first aspect of the present invention can be used to determine the heat treatment process parameters during the brazing process, and thus can be used as a pre-step for brazing using a flux-cored solder; when including the method for detecting the in-situ reaction of the flux-cored solder interface described in the present invention, any brazing method belongs to an embodiment of the present invention.
[0039] Example 1 The flux core solder used in this embodiment has been tested to have an outer skin melting point of 759° C., an inner core melting point of 695° C., a diameter of 2.0 mm, and a test section length of 300 mm.
[0040] Place the flux cored brazing material vertically, and set two induction coils in the test section of the flux cored brazing material, where the first induction coil is located at a height of 290 mm, and the second induction coil is located at a height of 270 mm. The first induction coil is set to: current I is 25 A; the second induction coil is set to: current I is 25 A; correspondingly, the heating temperature of the first induction coil is 770°C, and the heating temperature of the second induction coil is 710°C.
[0041] The two induction coils are started at the same time, heated to the preset temperature within 120 seconds, kept warm for 30 seconds, and then the two induction power supplies are turned off, followed by rapid cooling.
[0042] The cross-sectional tissue sections were sequentially sliced at the core solder heights of 290 mm, 280 mm, 260 mm, and 220 mm, and the corresponding slice samples were characterized by scanning electron microscopy in turn, as shown in the following figure. Figure 3 The SEM image shown, Figure 3(1) to (4) correspond to the cross-sectional structures at the above four heights, respectively, and there are different melting or interface reaction states.
[0043] based on Figure 3 It can be seen that: in the Figure 3 (4) In the "non-melting zone", no melting occurs during the brazing heating process. If the structure is the same as it, it means that no interface reaction or fusion occurs. Figure 3 (3) The structure in the "partially melted zone" is not exactly the same as that in the unmelted zone, but it is similar to the " Figure 3 (2) The microstructure of the “completely melted composition inhomogeneous zone” is partially the same, indicating that melting and resolidification occurred during the heating process. In addition, the “ Figure 3 (3) No new reaction layer is formed at the interface between the unmelted structure and the resolidified structure in the "partial melting zone", indicating that no diffusion reaction occurs at the interface between the solder skin and the core melt during the heating process, but only the solder skin continues to diffuse and dissolve into the core melt. Figure 3 (1) The structure in the "completely melted composition uniform zone" and the Figure 3 (2) There are obvious differences in the microstructure within the "completely melted component inhomogeneous zone", indicating that the insufficient diffusion of the alloy components in the solder skin will affect the solidification behavior of the flux-cored solder, resulting in differences in the solidification microstructure.
[0044] In addition, from the tissue compatibility we know: Figure 3 (1) There is a uniform black and white eutectic structure, indicating that the outer skin of the solder is completely dissolved in the liquid solder, the liquid solder alloy composition is uniform, and the eutectic structure solidifies and precipitates during the cooling process; Figure 3 (2) There are small pieces of black copper-rich phase and eutectic structure in the solder, indicating that the outer skin of the solder is completely dissolved in the liquid solder, but the alloy composition of the liquid solder is unevenly distributed, and the black copper-rich phase and eutectic structure solidify and precipitate during the cooling process; Figure 3 (3) There are large round copper-rich phases and eutectic structures in the solder, indicating that the outer skin of the solder partially dissolves into the liquid flux, the black copper-rich phase does not dissolve, and the eutectic structure solidifies and precipitates during the cooling process; Figure 3 (4) The microstructure of the solder skin did not change, indicating that no dissolution occurred.
[0045] Example 2 In the base material-solder-base material used in this embodiment, the base material composition is T2 copper (melting point: 960° C.), the solder composition is AgCuZnSnB (melting point: 758° C.), and the total length of the base material and the solder is 300 mm.
[0046] The combined base material-solder-base material is fixed and placed vertically, and two induction coils are set in its test section, where the first induction coil is located at a height of 290 mm and the second induction coil is located at a height of 270 mm. The first induction coil is set to: current I is 25 A; the second induction coil is set to: current I is 25 A; correspondingly, the heating temperature of the first induction coil is 770°C, and the heating temperature of the second induction coil is 710°C.
[0047] The two induction coils were started, heated to the preset temperature within 120 s, kept warm for 30 s, and then the two induction power supplies were turned off, followed by rapid cooling.
[0048] Cross-sectional tissue sections were made at base material-brazine-base material heights of 290 mm, 280 mm, 260 mm, and 220 mm, and the corresponding slice samples were characterized by scanning electron microscopy.
[0049] Although the present invention has been illustrated and described with specific embodiments, it should be appreciated that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Those skilled in the art should understand that the technical solutions described in the above embodiments may be modified, or some or all of the technical features thereof may be replaced by equivalents without departing from the spirit and scope of the present invention. However, these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention. Therefore, this means that all such replacements and modifications within the scope of the present invention are included in the appended claims.
Claims
1. A method for detecting in-situ reaction of solder interface, characterized in that: The detection method comprises: A gradient temperature field is set, and the test sample is heat treated to obtain the first melting zone, the second melting zone, the third melting zone and the unmelted zone with different melting states; after cooling, cross-sectional samples of each zone are taken for microscopic characterization, and the mechanism of in-situ reaction at the heterometallic interface is obtained based on the evolution of the organizational characteristics of each zone; Wherein, the test sample includes flux-cored solder or a combination of solder and base material.
2. The method for detecting the in-situ reaction of the solder interface according to claim 1, characterized in that: The heat source of the gradient temperature field includes any one of flame, arc, resistor, induction coil or laser; The detection method is carried out in an atmospheric environment.
3. The method for detecting the in-situ reaction of the solder interface according to claim 1, characterized in that: The heat source of the gradient temperature field is arranged at the edge of the test sample close to the first melting zone; The temperature of the heat source is at least 10° C. higher than the melting point of the test sample.
4. The method for detecting the in-situ reaction of the solder interface according to claim 1, characterized in that: The gradient temperature field includes a first temperature zone, a second temperature zone and a third temperature zone; and the heat source temperature corresponding to the first temperature zone is greater than that of the second temperature zone, and the heat source temperature of the second temperature zone is greater than that of the third temperature zone; The first melting zone and the second melting zone are obtained by heat treatment in the first temperature zone, the third melting zone is obtained by heat treatment in the second temperature zone, and the unmelted zone is obtained by heat treatment in the third temperature zone.
5. The method for detecting the in-situ reaction of the solder interface according to claim 4, characterized in that: In the first temperature zone, the heat Q1 absorbed by the edge of the test sample is taken as the standard, Q1=Q0-Q2-Q3>Q2; Among them, Q0 is the Joule heat generated by the heat source in the first temperature zone, Q2 is the outward conduction heat of the flux core solder corresponding to the first temperature zone, and Q3 is the heat dissipation from the heat source in the first temperature zone to the environment.
6. The method for detecting the in-situ reaction of the solder interface according to claim 4, characterized in that: When the test sample is the flux-cored solder, the melting point of a component with the highest melting point in the flux-cored solder is taken as the highest melting point, and the melting point of a component with the lowest melting point in the flux-cored solder is taken as the lowest melting point; during the heat treatment, the following range is met: The heat source temperature is ≥ the temperature of the flux-cored solder in the first temperature zone ≥ the highest melting point of the flux-cored solder; The lowest melting point of the flux core solder is less than the temperature of the flux core solder in the second temperature zone and less than the highest melting point of the flux core solder; The temperature of the flux core solder in the third temperature zone is the air temperature.
7. The method for detecting the in-situ reaction of the solder interface according to claim 4, characterized in that: The test sample corresponding to the first temperature zone is in a molten state, the test sample corresponding to the second temperature zone is in a partially molten paste state, and the test sample corresponding to the third temperature zone is in an unmelted solid state; Meanwhile, in the first melting zone, the solute elements in the melted liquid phase diffuse completely and the solute is evenly distributed; in the second melting zone, the solute elements in the melted liquid phase diffuse incompletely and the solute is unevenly distributed.
8. The method for detecting the in-situ reaction of solder interface according to claim 1, characterized in that: The heating rate of the heat source in the gradient temperature field is 4°C / s to 20°C / s; And / or, the heat treatment holding time is 15s to 60s; And / or, the cooling rate is ≥20°C / s.
9. A method for preparing a flux-cored solder, characterized in that: The preparation method includes the method for detecting the in-situ reaction of the solder interface as described in any one of claims 1 to 8.
10. A method for brazing a flux-cored brazing material, characterized in that: The brazing method comprises the method for detecting the in-situ reaction of the brazing material interface as described in any one of claims 1 to 8.
Citation Information
Patent Citations
Device and detection system for detecting flow paving process of welding flux or welding flux
CN220419178U