Preparation method of carbon-coated current collector for improving rate capability of lithium battery
Through the combination of modified carbon black and NiCo2O4 in lithium batteries, an efficient carbon-coated current collector is formed, which solves the problem of insufficient rate performance of lithium batteries, achieves better conductivity and electrochemical activity, and improves the overall performance of lithium batteries. .
Patent Information
- Application Number
- CN202410990681.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-10-08
AI Technical Summary
When improving battery cell rate performance, existing lithium battery manufacturers mainly focus on the optimization of cathode materials and ignore the improvement of auxiliary materials such as carbon-coated current collectors, resulting in insufficient rate performance.
A carbon-coated current collector preparation method is adopted, by heat-treating carbon black and NiCo2O4 in concentrated nitric acid, adding a silane coupling agent to form modified carbon black, and mixing it with polyacrylic acid and isopropyl alcohol to prepare a coating slurry , coated on the aluminum foil to form a carbon-coated aluminum foil, which improves the conductive performance and electrochemical activity of the carbon-coated current collector.
The nitric acid solvent promotes surface nitration of carbon black and forms chemical bonding with the silane coupling agent, thereby improving the combination of NiCo2O4 and carbon black, significantly improving the electrochemical performance of carbon-coated current collectors, and enhancing the rate performance and cycle stability of lithium batteries.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of lithium batteries, and in particular to a method for preparing a carbon-coated current collector for improving the rate performance of lithium batteries. Background Art
[0002] In today's society, with the rapid development of new energy, more and more consumers prefer new energy vehicles to traditional fuel vehicles. While people are concerned about the endurance of new energy vehicles, they also pay more attention to the rate performance of their batteries.
[0003] At present, battery manufacturers mainly focus on optimizing the active materials of the battery (mainly the positive electrode material) to improve the rate performance of the battery cell, while ignoring the improvement of some auxiliary materials. Therefore, improving battery performance by modifying the current collector has become one of the breakthroughs.
[0004] Therefore, we propose a method for preparing carbon-coated current collectors to improve the rate performance of lithium batteries. Summary of the invention
[0005] The object of the present invention is to provide a method for preparing a carbon-coated current collector for improving the rate performance of a lithium battery, so as to solve the problems raised in the above-mentioned background technology.
[0006] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0007] A method for preparing a carbon-coated current collector for improving the rate performance of a lithium battery comprises the following steps:
[0008] Step S1: Preparation of modified carbon black: adding carbon black, NiCo2O4 and a silane coupling agent into concentrated nitric acid, stirring evenly, performing heat treatment, washing and drying to obtain modified carbon black;
[0009] Step S2: Preparation of coating slurry: uniformly mix modified carbon black, polyacrylic acid and deionized water, add isopropanol, and stir uniformly to obtain coating slurry;
[0010] Step S3: Preparation of carbon-coated aluminum foil: coating the coating slurry on the surface of the aluminum foil, and drying it to obtain the carbon-coated aluminum foil, i.e., the carbon-coated current collector.
[0011] Furthermore, in step S1, the mass ratio of carbon black to NiCo2O4 is (13-20): (1.0-1.5).
[0012] Furthermore, in step S1, the heat treatment process conditions are: baking at 145-165° C. for 10-14 hours.
[0013] Furthermore, in step S1, the silane coupling agent is γ-aminopropyltriethoxysilane or vinyltriethoxysilane, and the amount thereof is 1.0-1.4% of the mass of carbon black.
[0014] Furthermore, in step S1, the concentration of concentrated nitric acid is 68wt%, and its usage is 17-20 times the mass of carbon black.
[0015] Furthermore, in step S2, the mass ratio of polyacrylic acid to modified carbon black is (1-3): (3-8).
[0016] Furthermore, in step S2, the mass of isopropanol is 0.01-0.10 times the mass of the modified carbon black.
[0017] Furthermore, in step S2, the solid content of the coating slurry is 8-12 wt%.
[0018] Furthermore, in step S3, the coating process conditions are: coating speed 40-80 m / min, single layer coating surface density 0.5-0.8 g / m 2 .
[0019] Furthermore, in step S3, the drying temperature is 80-120°C.
[0020] An application of a carbon-coated current collector for improving the rate performance of a lithium battery, comprising the following preparation method:
[0021] Preparation of negative electrode sheet: coating the negative electrode slurry on the negative electrode current collector, drying, rolling and compacting to obtain a negative electrode sheet;
[0022] Preparation of positive electrode sheet: coating the positive electrode slurry on the carbon-coated current collector prepared by the preparation method according to any one of claims 1 to 9, drying, rolling and compacting to obtain a positive electrode sheet;
[0023] Preparation of the battery: The positive electrode sheet, separator, and negative electrode sheet are stacked in order, and the battery core is obtained after winding or laminating, which is placed in a battery case, and the electrolyte is added. After packaging, standing, formation, and capacity division processes, a lithium battery is obtained.
[0024] Furthermore, the preparation of the negative electrode slurry includes uniformly mixing graphite, styrene butadiene rubber, carboxymethyl cellulose, a conductive agent and pure water to obtain the negative electrode slurry; the mass ratio of the graphite, styrene butadiene rubber, carboxymethyl cellulose, a conductive agent and pure water is 94.6:1.2:1.8:2.4:1.88.
[0025] Furthermore, the negative electrode current collector is copper foil.
[0026] Furthermore, the compaction density of the negative electrode plate is 1.38 g / cc.
[0027] Furthermore, the preparation of the positive electrode sheet includes uniformly mixing the ternary active material NCM811, the conductive agent, polyvinylidene fluoride and N-methylpyrrolidone to obtain a positive electrode slurry; the mass ratio of the ternary active material NCM811, the conductive agent, polyvinylidene fluoride and N-methylpyrrolidone is 92:4:4:2.13.
[0028] Furthermore, the compaction density of the positive electrode plate is 2.8 g / cc.
[0029] Furthermore, the electrolyte includes ethylene carbonate and ethyl methyl carbonate, the volume ratio of the ethylene carbonate to the ethyl methyl carbonate is 4:6, and the concentration of the electrolyte is 1 mol / L.
[0030] Compared with the prior art, the present invention has the following beneficial effects:
[0031] 1. The present invention provides a method for preparing a carbon-coated current collector for improving the rate performance of a lithium battery. By selecting nitric acid as a solvent, a nitration reaction is promoted on the surface of carbon black, a nitro group is introduced, and the surface activity is increased, providing a more favorable bonding environment for NiCo2O4 and carbon black. In addition, the addition of a silane coupling agent allows a portion of the groups in the carbon black molecules to react with NiCo2O4 to form a stable chemical bond. This bond contributes to the synergistic effect between the NiCo2O4 material and the carbon black, further improving the high rate performance of the NiCo2O4 material after bonding with the carbon black.
[0032] 2. The present invention provides a method for preparing a carbon-coated current collector for improving the rate performance of a lithium battery. By adding NiCo2O4 and carbon black, the conductivity and electrochemical activity of the carbon-coated current collector can be improved, thereby improving the rate performance of the lithium battery. NiCo2O4, as a positive electrode material, has excellent electrochemical properties and can improve the capacity and cycle stability of the battery; while carbon black has good electrical conductivity, can reduce resistance and improve the charge and discharge efficiency of the battery. When the two are used in combination, NiCo2O4 provides high capacity and stability, and carbon black provides good electrical conductivity. The synergistic effect of the two can effectively improve the electrochemical properties of the carbon-coated current collector, thereby improving the rate performance of the lithium battery. DETAILED DESCRIPTION
[0033] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0034] It should be noted that the purchase manufacturers of all raw materials involved in the present invention are not subject to any special restrictions and exemplarily include: carbon black: brand SUPER P Li (Swiss Termega), purchased from Guangdong Lvwei New Materials Technology Co., Ltd.; NiCo2O4: crystal spinel nickel cobalt oxide, purchased from Beijing Beike New Materials Technology Co., Ltd.; polyacrylic acid: solid content 25%, purchased from Wuhan Proloff Biotechnology Co., Ltd.; aluminum foil: thickness 12 μm, brand H18-1100, purchased from Shenzhen Honglei Metal Materials Co., Ltd.; positive electrode active material: lithium iron phosphate, Defang Nano DF5F; binder is polyvinylidene fluoride, brand Japan Kureha KF7200, purchased from Shanghai Huahenghui New Materials Technology Co., Ltd.; conductive agent: conductive carbon black SUPER P Li (Swiss Termega), purchased from Guangdong Lvwei New Materials Technology Co., Ltd.; copper foil: T2 copper foil, 8 μm thick, purchased from Shandong Huiya Metal Technology Co., Ltd.; battery case: model CR2032, purchased from Foshan Jiaying Battery Co., Ltd.; diaphragm: PE film, 20 μm thick, purchased from Dongguan Xuecheng Plastic Products Co., Ltd.; lithium sheet: item number xk-li28, purchased from Changsha Xinkang New Materials Co., Ltd.; gasket: 304 stainless steel disc, purchased from Wenzhou Chenghang Fastener Co., Ltd.; spring: item number 2032, purchased from Dongguan Meichang Spring Co., Ltd.
[0035] Example 1: A method for preparing a carbon-coated current collector for improving the rate performance of a lithium battery, comprising the following processes:
[0036] Step S1: Preparation of modified carbon black: 150 g carbon black, 10 g NiCo2O4 and 1.8 g silane coupling agent were added to 3000 g 68 wt% concentrated nitric acid, stirred evenly, and baked at 150° C. for 12 h. After washing and drying, modified carbon black was obtained;
[0037] Step S2: Preparation of coating slurry: 150 g of modified carbon black, 50 g of polyacrylic acid and deionized water were mixed evenly, 15 g of isopropanol was added, and the mixture was stirred evenly to obtain a coating slurry with a solid content of 10 wt %;
[0038] Step S3: Preparation of carbon-coated aluminum foil: Coat the coating slurry on the surface of the aluminum foil (coating speed 60 m / min, single-layer coating surface density 0.6 g / m 2 ), and after drying (drying temperature is 100° C.), a carbon-coated aluminum foil, i.e., a carbon-coated current collector, is obtained;
[0039] An application of a carbon-coated current collector for improving the rate performance of a lithium battery comprises the following steps:
[0040] Step 1: Preparation of negative electrode sheet: Graphite, styrene butadiene rubber, carboxymethyl cellulose, conductive agent and pure water are mixed evenly to obtain negative electrode slurry (the mass ratio of graphite, styrene butadiene rubber, carboxymethyl cellulose, conductive agent and pure water is 94.6:1.2:1.8:2.4:1.88), the negative electrode slurry is coated on copper foil, baked at 130°C for 12h, and rolled to obtain a negative electrode sheet (compacted density is 1.38g / cc);
[0041] Step 2: Preparation of positive electrode sheet: The ternary active material NCM811, the conductive agent, polyvinylidene fluoride and N-methylpyrrolidone are mixed evenly to obtain a positive electrode slurry (the mass ratio of the ternary active material NCM811, the conductive agent, polyvinylidene fluoride and N-methylpyrrolidone is 92:4:4:2.13); the positive electrode slurry is coated on the carbon-coated current collector, baked at 130°C for 12h, and rolled to obtain a positive electrode sheet (the compaction density is 2.8g / cc);
[0042] Step 3: Preparation of electrolyte: Ethylene carbonate and ethyl methyl carbonate are mixed evenly in a volume ratio of 4:6, and lithium hexafluorophosphate is added and mixed evenly to obtain an electrolyte with a concentration of 1 mol / L;
[0043] Step 4: Preparation of the battery: Use PE film as the separator, stack the positive electrode, separator, and negative electrode in order, and obtain the battery cell after winding. Put it into the battery shell, add electrolyte, and obtain the lithium battery after packaging, standing, formation, and capacity division processes.
[0044] Example 2: A method for preparing a carbon-coated current collector for improving the rate performance of a lithium battery, comprising the following processes:
[0045] Step S1: Preparation of modified carbon black: 130 g of carbon black, 10 g of NiCo2O4 and 1.8 g of silane coupling agent were added to 2210 g of 68 wt% concentrated nitric acid, stirred evenly, and baked at 140° C. for 14 h. After washing and drying, modified carbon black was obtained;
[0046] Step S2: Preparation of coating slurry: 130 g of modified carbon black, 65 g of polyacrylic acid and deionized water were mixed evenly, 1.3 g of isopropanol was added, and stirred evenly to obtain a coating slurry with a solid content of 8 wt %;
[0047] Step S3: Preparation of carbon-coated aluminum foil: Coat the coating slurry on the surface of the aluminum foil (coating speed 40 m / min, single-layer coating surface density 0.5 g / m 2 ), and after drying (drying temperature is 80° C.), a carbon-coated aluminum foil, i.e., a carbon-coated current collector, is obtained;
[0048] Compared with Example 1, the mass ratio of carbon black to NiCo2O4 in step S1 of Example 2 is 13:1, and the other steps are the same as Example 1.
[0049] Example 3: A method for preparing a carbon-coated current collector for improving the rate performance of a lithium battery, comprising the following processes:
[0050] Step S1: Preparation of modified carbon black: 140 g carbon black, 10 g NiCo2O4 and 1.8 g silane coupling agent were added to 2520 g 68 wt% concentrated nitric acid, stirred evenly, and baked at 160° C. for 10 h. After washing and drying, modified carbon black was obtained;
[0051] Step S2: Preparation of coating slurry: 140 g of modified carbon black, 52.5 g of polyacrylic acid and deionized water were mixed evenly, 7 g of isopropanol was added, and stirred evenly to obtain a coating slurry with a solid content of 12 wt%;
[0052] Step S3: Preparation of carbon-coated aluminum foil: Coat the coating slurry on the surface of the aluminum foil (coating speed 80 m / min, single-layer coating surface density 0.8 g / m 2 ), and after drying (drying temperature is 120° C.), a carbon-coated aluminum foil, i.e., a carbon-coated current collector, is obtained;
[0053] Compared with Example 1, the mass ratio of carbon black to NiCo2O4 in step S1 of Example 3 is 14:1, and the other steps are the same as Example 1.
[0054] Example 4: A method for preparing a carbon-coated current collector for improving the rate performance of a lithium battery, comprising the following processes:
[0055] Step S1: Preparation of modified carbon black: 160 g carbon black, 10 g NiCo2O4 and 1.8 g silane coupling agent were added to 3000 g 68 wt% concentrated nitric acid, stirred evenly, and baked at 150° C. for 12 h. After washing and drying, modified carbon black was obtained;
[0056] Step S2: Preparation of coating slurry: 150 g of modified carbon black, 50 g of polyacrylic acid and 600 g of deionized water were mixed evenly, 15 g of isopropanol was added, and stirred evenly to obtain a coating slurry with a solid content of 10 wt %;
[0057] Step S3: Preparation of carbon-coated aluminum foil: Coat the coating slurry on the surface of the aluminum foil (coating speed 60 m / min, single-layer coating surface density 0.6 g / m 2 ), and after drying (drying temperature is 100° C.), a carbon-coated aluminum foil, i.e., a carbon-coated current collector, is obtained;
[0058] Compared with Example 1, the mass ratio of carbon black to NiCo2O4 in step S1 of Example 4 is 16:1, and the other steps are the same as Example 1.
[0059] Example 5: A method for preparing a carbon-coated current collector for improving the rate performance of a lithium battery, comprising the following processes:
[0060] Step S1: Preparation of modified carbon black: 170 g carbon black, 10 g NiCo2O4 and 1.8 g silane coupling agent were added to 3000 g 68 wt% concentrated nitric acid, stirred evenly, and baked at 150° C. for 12 h. After washing and drying, modified carbon black was obtained;
[0061] Step S2: Preparation of coating slurry: 150 g of modified carbon black, 50 g of polyacrylic acid and 600 g of deionized water were mixed evenly, 15 g of isopropanol was added, and stirred evenly to obtain a coating slurry with a solid content of 10 wt %;
[0062] Step S3: Preparation of carbon-coated aluminum foil: Coat the coating slurry on the surface of the aluminum foil (coating speed 60 m / min, single-layer coating surface density 0.6 g / m 2 ), and after drying (drying temperature is 100° C.), a carbon-coated aluminum foil, i.e., a carbon-coated current collector, is obtained;
[0063] Compared with Example 1, the mass ratio of carbon black to NiCo2O4 in step S1 of Example 5 is 17:1, and the other steps are the same as Example 1.
[0064] Example 6: A method for preparing a carbon-coated current collector for improving the rate performance of a lithium battery, comprising the following process:
[0065] Step S1: Preparation of modified carbon black: 150 g of carbon black, 10 g of NiCo2O4 and 1.5 g of silane coupling agent are added to 3000 g of 68 wt% concentrated nitric acid, stirred evenly, and baked at 150° C. for 12 h. After washing and drying, modified carbon black is obtained;
[0066] Step S2: Preparation of coating slurry: 150 g of modified carbon black and 50 g of polyacrylic acid were mixed evenly, 15 g of isopropanol was added, and the mixture was stirred evenly to obtain a coating slurry with a solid content of 10 wt %;
[0067] Step S3: Preparation of carbon-coated aluminum foil: Coat the coating slurry on the surface of the aluminum foil (coating speed 60 m / min, single-layer coating surface density 0.6 g / m 2 ), and after drying (drying temperature is 100° C.), a carbon-coated aluminum foil, i.e., a carbon-coated current collector, is obtained;
[0068] Compared with Example 1, the mass of the silane coupling agent in step S1 of Example 6 is 1% of the mass of the carbon black, and the other steps are the same as Example 1.
[0069] Example 7: A method for preparing a carbon-coated current collector for improving the rate performance of a lithium battery, comprising the following process:
[0070] Step S1: Preparation of modified carbon black: 150 g of carbon black, 10 g of NiCo2O4 and 1.65 g of silane coupling agent were added to 3000 g of 68 wt% concentrated nitric acid, stirred evenly, and baked at 150° C. for 12 h. After washing and drying, modified carbon black was obtained;
[0071] Step S2: Preparation of coating slurry: 150 g of modified carbon black, 50 g of polyacrylic acid and 600 g of deionized water were mixed evenly, 15 g of isopropanol was added, and stirred evenly to obtain a coating slurry with a solid content of 10 wt %;
[0072] Step S3: Preparation of carbon-coated aluminum foil: Coat the coating slurry on the surface of the aluminum foil (coating speed 60 m / min, single-layer coating surface density 0.6 g / m 2 ), and after drying (drying temperature is 100° C.), a carbon-coated aluminum foil, i.e., a carbon-coated current collector, is obtained;
[0073] Compared with Example 1, the mass of the silane coupling agent in step S1 of Example 7 is 1.1% of the mass of the carbon black, and the other steps are the same as Example 1.
[0074] Example 8: A method for preparing a carbon-coated current collector for improving the rate performance of a lithium battery, comprising the following process:
[0075] Step S1: Preparation of modified carbon black: 150 g of carbon black, 10 g of NiCo2O4 and 1.95 g of silane coupling agent were added to 3000 g of 68 wt% concentrated nitric acid, stirred evenly, and baked at 150° C. for 12 h. After washing and drying, modified carbon black was obtained;
[0076] Step S2: Preparation of coating slurry: 150 g of modified carbon black, 50 g of polyacrylic acid and 600 g of deionized water were mixed evenly, 15 g of isopropanol was added, and stirred evenly to obtain a coating slurry with a solid content of 10 wt %;
[0077] Step S3: Preparation of carbon-coated aluminum foil: Coat the coating slurry on the surface of the aluminum foil (coating speed 60 m / min, single-layer coating surface density 0.6 g / m 2 ), and after drying (drying temperature is 100° C.), a carbon-coated aluminum foil, i.e., a carbon-coated current collector, is obtained;
[0078] Compared with Example 1, the mass of the silane coupling agent in step S1 of Example 8 is 1.3% of the mass of the carbon black, and the other steps are the same as Example 1.
[0079] Example 9: A method for preparing a carbon-coated current collector for improving the rate performance of a lithium battery, comprising the following process:
[0080] Step S1: Preparation of modified carbon black: 150 g carbon black, 10 g NiCo2O4 and 2.1 g silane coupling agent were added to 3000 g 68 wt% concentrated nitric acid, stirred evenly, and baked at 150° C. for 12 h. After washing and drying, modified carbon black was obtained;
[0081] Step S2: Preparation of coating slurry: 150 g of modified carbon black, 50 g of polyacrylic acid and 600 g of deionized water were mixed evenly, 15 g of isopropanol was added, and stirred evenly to obtain a coating slurry with a solid content of 10 wt %;
[0082] Step S3: Preparation of carbon-coated aluminum foil: Coat the coating slurry on the surface of the aluminum foil (coating speed 60 m / min, single-layer coating surface density 0.6 g / m 2 ), and after drying (drying temperature is 100° C.), a carbon-coated aluminum foil, i.e., a carbon-coated current collector, is obtained;
[0083] Compared with Example 1, the mass of the silane coupling agent in step S1 of Example 9 is 1.4% of the mass of the carbon black, and the other steps are the same as Example 1.
[0084] Comparative Example 1: A method for preparing a carbon-coated current collector for improving the rate performance of a lithium battery, comprising the following processes:
[0085] Compared with Example 1, in Comparative Example 1, the concentrated nitric acid in step S1 is replaced with pure water, and the other steps are the same as those in Example 1.
[0086] Comparative Example 2: A method for preparing a carbon-coated current collector for improving the rate performance of a lithium battery, comprising the following processes:
[0087] Compared with Example 1, no silane coupling agent is added in step S1 of Comparative Example 2, and the other steps are the same as those of Example 1.
[0088] Comparative Example 3: A method for preparing a carbon-coated current collector for improving the rate performance of a lithium battery, comprising the following processes:
[0089] Compared with Example 1, NiCo2O4 is not added in step S1 of Comparative Example 3, and the other steps are the same as those of Example 1.
[0090] Experiment: Mix lithium iron phosphate, polyvinylidene fluoride, conductive agent and N-methylpyrrolidone evenly to obtain positive electrode material slurry (the composition of the positive electrode slurry is: lithium iron phosphate 95%, polyvinylidene fluoride 2%, conductive agent 3%, N-methylpyrrolidone as solvent, and the overall solid content is 50%); the positive electrode material slurry is coated on the surface of the carbon-coated current collector obtained in Examples 1-9 and Comparative Examples 1-3, vacuum dried at 120°C for 12h, and rolled to obtain a positive electrode sheet; in an inert gas atmosphere, the button battery is assembled in the order of battery shell-placement of positive electrode sheet-drip electrolyte-placement of diaphragm-drip electrolyte-placement of lithium sheet-placement of gasket shrapnel-battery shell. The button battery is charged and discharged at different rates (0.2C, 0.5C, 1C, 2C) using a button battery charge and discharge tester (Wuhan Blue Electric, CT2001A), and the voltage range is 2.0-3.65V.
[0091] The test results are shown in the table:
[0092] 0.2C 0.5C 1C 2C Example 1 98.9% 96.2% 93.1% 91.5% Example 2 97.1% 94.8% 91.9% 90.1% Example 3 97.0% 94.5% 91.6% 89.8% Example 4 97.4% 94.9% 92.2% 90.2% Example 5 97.1% 94.4% 92.0% 90.1% Example 6 97.9% 95.0% 92.2% 90.2% Example 7 97.8% 94.8% 92.4% 90.4% Example 8 97.6% 94.4% 92.0% 90.0% Example 9 97.4% 95.1% 92.0% 89.7% Comparative Example 1 96.4% 94.1% 91.1% 88.5% Comparative Example 2 96.2% 94.0% 91.6% 88.3% Comparative Example 3 96.0% 93.5% 90.8% 87.6%
[0093] According to the data in the above table, we can clearly draw the following conclusions:
[0094] 1. Compared with Examples 1-9, the rate performance of the product obtained in Comparative Example 1 is reduced, indicating that compared with pure water, the present invention uses nitric acid as a solvent to cause nitration reaction on the surface of carbon black, introduce nitro groups, increase surface activity, and provide a more favorable binding environment for NiCo2O4 and carbon black.
[0095] 2. Compared with Examples 1-9, the rate performance of the product obtained in Comparative Example 2 is reduced, which indicates that the addition of silane coupling agent in the present invention enables some groups in the carbon black molecules to react with NiCo2O4 to form chemical bonds, so that the NiCo2O4 material exhibits high rate performance after combining with carbon black.
[0096] 3. Compared with Examples 1-9, the rate performance of the product obtained in Comparative Example 3 is reduced. It can be seen that the addition of NiCo2O4 in the present invention can play a synergistic role with carbon black, thereby achieving a better performance improvement effect.
[0097] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process method article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process method article or device.
[0098] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a carbon-coated current collector for improving the rate performance of a lithium battery, characterized in that: The steps include: Step S1: Preparation of modified carbon black: adding carbon black, NiCo2O4 and a silane coupling agent into concentrated nitric acid, stirring evenly, performing heat treatment, washing and drying to obtain modified carbon black; Step S2: Preparation of coating slurry: uniformly mix modified carbon black, polyacrylic acid and deionized water, add isopropanol, and stir uniformly to obtain coating slurry; Step S3: Preparation of carbon-coated aluminum foil: coating the coating slurry on the surface of the aluminum foil, and drying it to obtain the carbon-coated aluminum foil, i.e., the carbon-coated current collector.
2. A method for preparing a carbon-coated current collector for improving the rate performance of a lithium battery according to claim 1, characterized in that: In the step S1, the mass ratio of carbon black to NiCo2O4 is (13-20): (1.0-1.5).
3. A method for preparing a carbon-coated current collector for improving the rate performance of a lithium battery according to claim 1, characterized in that: In step S1, the heat treatment process conditions are: baking at 145-165° C. for 10-14 hours.
4. The method for preparing a carbon-coated current collector for improving the rate performance of a lithium battery according to claim 1, characterized in that: In the step S1, the silane coupling agent is γ-aminopropyltriethoxysilane or vinyltriethoxysilane, and the amount thereof is 1.1-1.3% of the mass of carbon black.
5. The method for preparing a carbon-coated current collector for improving the rate performance of a lithium battery according to claim 1, characterized in that: In the step S1, the concentration of concentrated nitric acid is 68wt%, and the amount thereof is 17-20 times the mass of carbon black.
6. A method for preparing a carbon-coated current collector for improving the rate performance of a lithium battery according to claim 1, characterized in that: In the step S2, the mass ratio of polyacrylic acid to modified carbon black is (1-3): (3-8).
7. A method for preparing a carbon-coated current collector for improving the rate performance of a lithium battery according to claim 1, characterized in that: In step S2, the solid content of the coating slurry is 8-12 wt%.
8. The method for preparing a carbon-coated current collector for improving the rate performance of a lithium battery according to claim 1, characterized in that: In step S3, the coating process conditions are: coating speed 40-80 m / min, single layer coating surface density 0.5-0.8 g / m 2 .
9. A carbon-coated current collector for improving the rate performance of a lithium battery, obtained by the preparation method according to any one of claims 1 to 8.
10. An application of a carbon-coated current collector for improving the rate performance of a lithium battery, characterized in that: The invention comprises the following preparation methods: Preparation of negative electrode sheet: coating the negative electrode slurry on the negative electrode current collector, drying, rolling and compacting to obtain a negative electrode sheet; Preparation of positive electrode sheet: coating the positive electrode slurry on the carbon-coated current collector prepared by the preparation method according to any one of claims 1 to 9, drying, rolling and compacting to obtain a positive electrode sheet; Preparation of the battery: The positive electrode sheet, separator, and negative electrode sheet are stacked in order, and the battery core is obtained after winding or laminating, which is placed in a battery case, and the electrolyte is added. After packaging, standing, formation, and capacity division processes, a lithium battery is obtained.