Method for modifying zinc ion battery diaphragm
By using ultrasonic dispersion of nanodiamonds on zinc-ion battery separators, the problem of zinc dendrites and corrosion during the charge and discharge process of zinc-ion batteries is solved, higher cycle stability and capacity retention rate are achieved, and zinc-ion batteries are improved. Overall battery performance.
Patent Information
- Application Number
- CN202410753147.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-12
- Publication Date
- 2024-10-08
AI Technical Summary
Zinc-ion batteries are prone to zinc dendrites and corrosion problems during the charge and discharge process, which affect their performance. Existing research mainly focuses on the protection of positive electrode materials and zinc anodes, and the improvement potential of separators has not been fully utilized.
The glass fiber separator is modified by ultrasonic dispersion of nanodiamonds in deionized water to form a separator material with suitable pore structure and excellent mechanical properties, which improves the cycle stability and reversible specific capacity of zinc-ion batteries.
Through the modified separator, the cycle stability and capacity retention rate of the zinc-ion battery are significantly improved, the formation of zinc dendrites is reduced, the anti-corrosion performance of the zinc anode is enhanced, and the uniform deposition and transmission rate of zinc ions are improved.
Smart Images

Figure CN118748306A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of zinc ion battery diaphragm modification and modification, and uses nano diamond to modify the diaphragm to improve the performance of the zinc ion battery. Background Art
[0002] In recent years, metal-based energy storage systems have received great attention due to their excellent electrochemical performance. Aqueous zinc-ion batteries (AZIBs) are one of the important energy storage batteries. They usually use metallic zinc as the negative electrode, a neutral or weakly acidic aqueous solution containing zinc ions as the electrolyte, and materials such as glass fiber as the separator. During the charge and discharge process of AZIBs, zinc ions shuttle through the pores of the separator filled with electrolyte, and continuously deposit and dissolve on the surface of the zinc negative electrode. Due to the influence of multiple factors such as electrodes, electrolytes, and separators, zinc ions are prone to form zinc dendrites during the stripping / galvanizing process, produce a passivation layer on the surface of the zinc anode, and even cause serious corrosion to the surface of the zinc anode, which is an urgent problem to be solved. In order to improve the performance of AZIBs, a series of side reaction problems such as irreversible zinc dendrites and corrosion on the surface of the zinc anode must be solved. Current research mainly focuses on the modification of positive electrode materials, protection of zinc anodes, and optimization of electrolytes. Inside the battery structure, the role of the separator is to prevent the electrode contact from causing a short circuit, absorb electrolytes for zinc ion transmission, control the zinc ion transmission rate through the pore size, and regulate the uniform deposition and dissolution of zinc ions, thereby reducing zinc dendrites and byproducts. Therefore, the modification and improvement of zinc ion battery separators is very important. Similar to electrodes and electrolytes, separators also show great research potential and can be modified and improved through different research strategies. Summary of the invention
[0003] The purpose of the present invention is to overcome the shortcomings of the background technology and provide a method for modifying a zinc ion battery diaphragm to improve the charge and discharge capacity, cycle stability and rate performance of the electrode material, and obtain a diaphragm material with a suitable pore structure and excellent mechanical and chemical properties.
[0004] The present invention adopts an ultrasonic dispersion method to add nanodiamonds (NDs) into deionized water to obtain a water-based dispersion of NDs, which is used to modify the diaphragm, thereby obtaining a diaphragm material with a suitable pore structure and excellent mechanical and chemical properties, thereby further improving the cycle stability and reversible specific capacity of AZIBs.
[0005] The technical solution adopted by the present invention is as follows:
[0006] A method for modifying a zinc ion battery separator, comprising the following steps:
[0007] 1) Dispersing 1-10 mg of NDs uniformly in 20-50 mL of deionized water to obtain a NDs water-based dispersion;
[0008] 2) The zinc ion battery separator is completely immersed in the NDs water-based dispersion, taken out after standing for 10 minutes, and finally placed in a drying oven at 60°C for 12 hours to achieve the modification of the zinc ion battery separator;
[0009] The particle size of the NDs is preferably 5 to 10 nm.
[0010] The zinc ion battery separator is preferably glass fiber GF.
[0011] Preferably, in step 1), NDs is 5 mg, deionized water is 20 mL, and the mixture is dispersed by ultrasound.
[0012] Preferably, in step 2), the zinc ion battery separator is a glass fiber GF separator.
[0013] The modified zinc ion battery separator of the present invention is used for assembling zinc||zinc symmetrical battery, zinc||copper asymmetric battery and zinc||manganese dioxide full battery.
[0014] Beneficial effects of the present invention:
[0015] 1. For the samples prepared by the present invention, the dispersion of NDs on the membrane surface is good.
[0016] 2. The sample prepared by the present invention has good ability to adjust the ion transmission rate, can adjust the deposition behavior of zinc ions, and achieve a uniform zinc deposition layer, and can be used as an ideal diaphragm material.
[0017] 3. The samples prepared by the present invention have excellent physical and chemical properties, and the zinc ion batteries made with them have good cycle stability and capacity retention rate. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 The scanning electron microscope photograph of the NDs-GF membrane used in the example.
[0019] Figure 2 The scanning electron microscope photograph of the comparative GF separator is shown in FIG.
[0020] Figure 3 The Zn||Zn symmetric cell assembled with the NDs-GF separator of the embodiment is 2 Scanning electron micrograph of the zinc anode after 10 cycles at a current density of .
[0021] Figure 4 The Zn||Zn symmetric cell assembled with the comparative example GF separator at 1 mA / cm 2 Scanning electron micrograph of the zinc anode after 10 cycles at a current density of .
[0022] Figure 5 The Zn||Zn symmetric cell assembled with the NDs-GF membrane of the embodiment and the GF membrane of the comparative example was operated at a constant current density of 5 mA / cm 2 The following cycle performance comparison chart.
[0023] Figure 6 The Zn / / Cu asymmetric cell assembled with the NDs-GF membrane of the embodiment and the GF membrane of the comparative example was 2 Comparison of Coulombic efficiency at different current densities.
[0024] Figure 7 This is a comparison chart of the charge and discharge specific capacity of a Zn / / MnO2 full battery assembled using the example NDs-GF membrane and the comparative example GF membrane at a current density of 1 A / g. DETAILED DESCRIPTION
[0025] The present application is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be pointed out that the embodiments described below are intended to facilitate the understanding of the present application and do not have any limiting effect thereon.
[0026] Example 1: Preparation of NDs-GF membrane modified with NDs
[0027] The NDs (5 mg) prepared by the detonation method were first dried at a constant temperature, and then the dried NDs and deionized water (20 mL) were added to a beaker and then ultrasonically dispersed.
[0028] The glass fiber GF diaphragm is cut into a circle with a diameter of 16 mm using a special cutting die, and then the diaphragm is modified with a water-based dispersion containing NDs. The commercial diaphragm is completely immersed in the NDs water-based dispersion, left to stand for 10 minutes, then taken out, and finally placed in a drying oven at 60°C for 12 hours to obtain NDs-GF.
[0029] In this embodiment, the drying and evaporation were carried out at a constant temperature of 60°C, the ultrasonic treatment time was 1 hour, and the glass fiber GF membrane was cut into a circle with a diameter of 16 mm using a special cutting die. All operations were carried out at room temperature.
[0030] Example 2: Preparation of GF membrane
[0031] This embodiment is a comparative example and is a prior art. The prepared sample is used for performance comparison with the sample prepared by the NDs-GF membrane of the embodiment (the method of the present invention) to illustrate the effect of the present invention.
[0032] The commercial glass fiber GF separator was cut into a circular shape with a diameter of 16 mm using a special cutting die. The obtained pure GF separator sample was marked as sample GF.
[0033] In this embodiment, all operations were carried out at room temperature.
[0034] Example 3: Using zinc sulfate solution as electrolyte
[0035] Weigh 5.75 g of zinc sulfate heptahydrate into a beaker containing 10 mL of ethanol and stir until the zinc sulfate heptahydrate is completely dissolved to obtain a 2 M zinc sulfate electrolyte.
[0036] Example 4: Using MnO2 material to make the positive electrode of zinc ion battery
[0037] Zn||Zn symmetrical battery, Zn / / Cu asymmetric battery and Zn / / MnO2 full battery use pure metallic zinc and pure metallic copper, which are cut into several electrode discs with a diameter of 12mm using a special cutting die.
[0038] The positive electrode of the Zn / / MnO2 full battery is composed of 70wt% commercial MnO2 material (active substance), 10wt% binder (polyvinylidene fluoride, PVDF) and 20wt% conductive agent Super P. The three are mixed and ground for 30 minutes and then put into a container. 10-12 drops of 1-methyl-2-pyrrolidone (NMP, solvent) are added to the container, and then placed on a magnetic stirrer and stirred at a uniform speed for 6 hours until the mixture becomes a viscous fluid. Using carbon paper as the current collector, apply the above mixed viscous material on the carbon paper, and the coating density must be uniform. Set the temperature of the vacuum drying oven to 80°C, and take the above carbon paper coating and place it in the vacuum drying oven. After timing for 12 hours, take it out for use. Use a special cutting knife mold to cut the prepared carbon paper coating into several electrode discs with a diameter of 12mm.
[0039] Example 5: Preparation and performance testing of zinc ion batteries
[0040] Samples NDs-GF and sample GF were used as separators for zinc-ion batteries to assemble different types of batteries and test their performance for zinc-ion batteries. The zinc-ion batteries prepared in this test were CR-2025 button batteries. Then the mass of the electrode sheet was weighed to prepare for the calculation of subsequent specific capacity parameters. The matching battery positive and negative electrode shells, gaskets, springs, NDs-GF and GF separators, electrolytes, electrode sheets, etc. were taken to operate and encapsulate the batteries in a safe and orderly manner according to the production regulations of zinc-ion batteries. The Zn||Zn symmetric battery, Zn / / Cu asymmetric battery, and Zn / / MnO2 full battery assembled with samples NDs-GF and sample GF as separators were marked as Zn|NDs-GF|Zn, Zn|GF|Zn, Zn|NDs-GF|Cu, Zn|GF|Cu, Zn|NDs-GF|MnO2, and Zn|GF|MnO2, respectively.
[0041] Example 6: Performance test of different zinc ion batteries
[0042] The LAND battery test system (CT2001 1A) was used to test Zn|NDs-GF|Zn, Zn|GF|Zn, Zn|NDs-GF|Cu, Zn|GF|Cu, Zn|NDs-GF|MnO2, and Zn|GF|MnO2. At 25°C, the battery was discharged to 0.8V at a certain current density; after the discharge, it was charged to 1.9V at a certain current density; after the charge, it was discharged to 0.8V at the same current density, and the constant current cycle test was repeated.
[0043] Effect verification:
[0044] 1) Characterization of NDs-GF membrane
[0045] Scanning electron microscopy (SEM) was used to characterize the prepared NDs-GF membrane and GF membrane. Figure 1 As shown in the figure, NDs attached to the surface of the GF membrane, making the membrane surface rougher, increasing the mechanical strength of the membrane and the specific surface area of the membrane. The surface pores of the GF membrane were partially filled by NDs, and the pore size was smaller.
[0046] 2) Characterization of GF membrane
[0047] The commercial GF separator was characterized and tested using scanning electron microscopy (SEM). Figure 2 As shown, the GF diaphragm is composed of glass fibers with smooth surfaces and different pore sizes.
[0048] 3) Characterization of the zinc anode surface using NDs-GF separator
[0049] The Zn||Zn symmetric battery was investigated by scanning electron microscopy (SEM) at 1 mA / cm 2 The zinc anode was characterized after cycling for 10 hours at the current density. Figure 3 As shown, the surface of the zinc anode using the NDs-GF separator is smooth without a large amount of zinc dendrites and byproducts.
[0050] 4) Characterization of the zinc anode surface using GF membrane
[0051] The Zn||Zn symmetric battery was investigated by scanning electron microscopy (SEM) at 1 mA / cm 2 The zinc anode was characterized after cycling for 10 hours at the current density. Figure 4 As shown, a large number of zinc dendrites and byproducts were generated on the surface of the zinc anode using the GF separator.
[0052] 5) Battery testing system tests Zn||Zn
[0053] The Zn|NDs-GF|Zn and Zn|GF|Zn symmetric cells were tested at 5 mA / cm using the LAND battery test system (CT2001 1A). 2 Current density, specific capacitance is 1 mAh / cm 2 The constant current cycle test is carried out under Figure 5 As shown, the cycle life of the Zn|NDs-GF|Zn symmetric battery is close to 1350 h, which is more than 12 times that of Zn|GF|Zn (110 h), indicating that the NDs-modified GF separator is beneficial to the battery cycling stability.
[0054] 6) Battery testing system tests Zn||Cu
[0055] The Zn|NDs-GF|Cu and Zn|GF|Cu asymmetric cells were tested at 2 mA / cm using the LAND battery test system (CT2001 1A). 2 Current density, specific capacitance is 1 mAh / cm 2 The reversible behavior of zinc ions in two asymmetric batteries was studied. Figure 6 As shown in the figure, the Zn|NDs-GF|Cu asymmetric battery can be cycled for more than 400 hours with an average Coulombic efficiency (CE) of up to 99.3%. In contrast, the Zn|GF|Cu asymmetric battery exhibits obvious CE fluctuations throughout the cycle, and the cycle is less than 150 hours, forming side reactions and zinc dendrites.
[0056] 7) Battery testing system tests Zn||MnO2
[0057] The LAND battery test system (CT2001 1A) was used to test the Zn|NDs-GF|MnO2 and Zn|GF|MnO2 at a current density of 1A / g (mass loading of 2.1mg / cm 2 ) under the condition of full battery, the long-term cycle stability was evaluated. Figure 7 As shown in Figure 3, the Zn|NDs-GF|MnO2 full cell has a high reversible capacity of 102.5 mAh / g after 1000 cycles. In contrast, the Zn|GF|MnO2 full cell has a low reversible specific capacity during the entire cycle process.
[0058] When the sample NDs-GF prepared by the method of the present invention is used as a separator for an aqueous zinc ion battery, the obtained Zn|NDs-GF|Zn symmetric battery has extremely high cycle stability. The modified GF separator is characterized by a scanning electron microscope, and it can be seen that the surface of the NDs-GF separator is covered with NDs and the surface becomes rough. It can also be seen from the analysis of the surface morphology of the zinc anode that there are no obvious flaky zinc dendrites on the surface of the zinc anode. When the sample NDs-GF prepared by the method of the present invention is used as a separator for a zinc ion battery, the obtained Zn|NDs-GF|Zn symmetric battery and Zn|NDs-GF|Cu asymmetric battery have good cycle stability and higher coulomb efficiency than the Zn|GF|Zn symmetric battery and the Zn|GF|Cu asymmetric battery; the obtained Zn|NDs-GF|MnO2 full battery has good reversible specific capacity and retention rate compared with the Zn|GF|MnO2 full battery, showing that the material prepared by the present invention has excellent electrochemical properties.
Claims
1. A method for modifying a zinc ion battery separator, characterized in that: Here are the steps: 1) Dispersing 1-10 mg of nanodiamonds uniformly in 20-50 mL of deionized water to obtain a NDs water-based dispersion; 2) The zinc ion battery separator is completely immersed in the NDs water-based dispersion, taken out after standing for 10 minutes, and finally placed in a drying oven at 60°C for 12 hours to achieve the modification of the zinc ion battery separator.
2. The method for modifying the zinc ion battery separator according to claim 1, wherein The nano-diamond particle size described in step 1) is 5-10 nm.
3. The method for modifying the zinc ion battery separator according to claim 1, wherein In step 1), NDs is 5 mg, deionized water is 20 mL, and dispersed by ultrasound.
4. The method for modifying the zinc ion battery separator according to claim 1, wherein The zinc ion battery separator in step 2) is a glass fiber GF separator.
5. A zinc ion battery separator obtained according to the method according to any one of claims 1 to 4.
6. Use of the zinc ion battery separator according to claim 5 for assembling zinc||zinc symmetrical batteries, zinc||copper asymmetric batteries, and zinc||manganese dioxide full batteries.