Preparation method of lithium battery diaphragm coating slurry and lithium battery diaphragm
Through a unique pulping process and coating technology, combined with porous boehmite, alumina and PVDF materials, it solves the problem that traditional separators cannot meet high performance requirements, and significantly improves the performance and life of lithium battery separators.
Patent Information
- Application Number
- CN202410886225.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-03
- Publication Date
- 2024-10-08
AI Technical Summary
The traditional single-sided coated separator and unchanged slurry powder structure cannot meet the growing comprehensive demand for high performance of lithium batteries.
Using a unique pulping process and simple coating process technology, combined with organic and inorganic coating materials, three different types of separator coating slurries, namely porous boehmite, alumina and PVDF, are prepared through different coating methods Improve diaphragm performance.
It improves the comprehensive performance of the separator, improves the safety and battery life of lithium batteries, and enhances the stability and durability of the separator.
Smart Images

Figure CN118748307A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of lithium battery technology, and in particular to a method for preparing a lithium battery separator coating slurry and a lithium battery separator. Background Art
[0002] Lithium-ion batteries are considered to be one of the most promising energy storage systems. Lithium battery separator is a thin film with a microporous structure, and it is also the key inner component with the most technical barriers in the lithium battery industry chain. As an important component of lithium-ion batteries, the performance of the separator greatly affects the overall performance of the battery to a certain extent. There are also large differences in the performance of base films of different thicknesses in various aspects. Coating on the base film has become an effective, economical and practical means to improve the cycle stability and service life of lithium batteries. However, it has been proved that the traditional single-sided coated separator and the unchanging slurry powder structure can no longer meet the growing high-performance comprehensive needs of lithium batteries. Summary of the invention
[0003] (1) Technical issues to be solved
[0004] The present application provides a method for preparing a lithium battery diaphragm coating slurry and a lithium battery diaphragm, and the technical problem to be solved is that the traditional single-sided coating diaphragm and the unchanging slurry powder structure can no longer meet the growing comprehensive high-performance requirements of lithium batteries.
[0005] (2) Technical solution
[0006] In a first aspect, the present application provides a method for preparing a lithium battery separator coating slurry, comprising:
[0007] 0.2126 parts of dispersant and 1.2622 parts of pure water were mixed and stirred in a dispersion tank at a speed of 840-860 rpm for 30 minutes to dissolve the dispersant in the pure water;
[0008] Add 0.01432 parts of thickener to the solution and stir for 15 minutes at a speed of 840-860 rpm, then add 1 part of porous boehmite powder pretreated with anhydrous ethanol, mix and stir for 50 minutes at a speed of 840-860 rpm;
[0009] Pour the stirred slurry into a grinder and grind it twice. The grinding time is 18 minutes and 42 minutes respectively. The speed of the grinder is 640-660 rpm and the grinding temperature is 25-30°C.
[0010] Pour the ground slurry into the disperser again, add 0.2000 parts of binder and stir for 30 minutes at a speed of 290-310 rpm, then add 0.0020 parts of wetting agent and stir for 20 minutes at a speed of 190-210 rpm;
[0011] The prepared slurry is discharged, and iron is removed and filtered during the discharge, with a magnetic field strength of 10000 gs and a filter element of 300 meshes, to obtain a porous boehmite slurry.
[0012] Furthermore, the method for preparing the lithium battery separator coating slurry further comprises:
[0013] 0.3568 parts of dispersant and 1.1959 parts of pure water were mixed and stirred in a dispersion tank at a speed of 840-860 rpm for 30 minutes to dissolve the dispersant in the pure water;
[0014] Add 0.0120 parts of thickener to the solution and stir for 15 minutes at a speed of 840-860 rpm, then add 1 part of alumina powder, mix and stir for 50 minutes at a speed of 840-860 rpm;
[0015] Pour the stirred slurry into a grinder and grind it twice. The grinding time is 18 minutes and 42 minutes respectively. The speed of the grinder is 640-660 rpm and the grinding temperature is 25-30°C.
[0016] Pour the ground slurry into the disperser again, add 0.1365 parts of binder and stir for 30 minutes at a speed of 290-310 rpm, then add 0.0016 parts of wetting agent and stir for 20 minutes at a speed of 190-210 rpm;
[0017] The prepared slurry is discharged, and iron is removed and filtered during the discharge, with a magnetic field strength of 10000 gs and a filter element of 300 meshes to obtain alumina slurry.
[0018] Furthermore, the method for preparing the lithium battery separator coating slurry further comprises:
[0019] Stir 0.7407 parts of binder and 3.7592 parts of pure water in a disperser for 30 minutes to dissolve the binder in the pure water at a speed of 990-1010 rpm;
[0020] Add 0.6 parts of PVDF to the solution and stir for 15 minutes at a speed of 490-510 rpm, then increase the speed to 1000 rpm and continue stirring for 30 minutes;
[0021] 0.4 parts of PVDF was added to the mixed solution and stirred for 15 minutes, the rotation speed was reduced to 490-510 rpm, and then the rotation speed was increased to 2000 rpm and stirring was continued for 180 minutes;
[0022] Add 3.7593 parts of pure water to the slurry and stir for 60 minutes at 2000 rpm;
[0023] The prepared slurry was discharged, and iron was removed and filtered during the discharge, with a magnetic field strength of 10000 gs and a filter element of 300 meshes to obtain PVDF slurry.
[0024] Furthermore, the thickener includes carboxymethyl cellulose, the binder includes polymethyl methacrylate, and the dispersant includes ammonium salt.
[0025] In the second aspect, the present application provides a lithium battery separator, the base film of which is a polyethylene separator, and the two sides of the base film are coated with different coating slurries, respectively, and the coating slurries include the porous boehmite slurry as described above, the alumina slurry as described above, and the PVDF slurry as described above.
[0026] Furthermore, the base film has a thickness of 7 μm or 12 μm.
[0027] Furthermore, the porosity of the base film is 30-40%.
[0028] Furthermore, the coating slurry has a coating thickness of 3 μm.
[0029] Furthermore, the porous boehmite slurry, the alumina slurry and the PVDF slurry have a solid content of 10-90%, a D50 of 0.6-10 μm and a viscosity of 50-150 mPa·s.
[0030] Furthermore, the porous boehmite slurry and the alumina slurry are coated by roller coating, and the PVDF slurry is coated by spraying.
[0031] (3) Beneficial effects
[0032] The above technical solution of the present application has the following advantages:
[0033] The preparation method of the lithium battery separator coating slurry and the lithium battery separator provided in the present application adopt a unique pulping process and a simple coating process technology to combine organic and inorganic coating materials, thereby improving the comprehensive performance of the separator. The porous boehmite greatly improves the wettability of the separator and also makes the separator more stable. The two coating materials with their respective advantages are coated on the base film, and the comprehensive performance of the coating film can be improved at the same time without losing the original performance of the base film, thereby greatly improving the safety and battery life of the lithium battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] In order to more clearly illustrate the specific implementation methods of the present application or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0035] Figure 1 Schematic diagram of the hollow porous boehmite structure provided for this application;
[0036] Figure 2 Schematic diagram of slurry membrane coating provided for this application;
[0037] Figure 3 Schematic diagram of the diaphragm coating equipment and coating process provided in this application.
[0038] Figure numerals: 11, base film; 12, spraying surface; 13, roller coating surface; 14, double-sided coated diaphragm; 15, single-sided coating (spraying); 16, single-sided coating (roller coating); 21, unwinding device; 22, preheating oven; 23, roller coating / spraying device; 24, oven; 25, winding device. DETAILED DESCRIPTION
[0039] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present application more clearly understood, the present application is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.
[0040] In this application, "at least one" means one or more, and "plurality" means two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c" can all mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or multiple, respectively.
[0041] It should be understood that in the various embodiments of the present application, the size of the serial numbers of the above-mentioned processes does not mean the order of execution, some or all of the steps can be executed in parallel or sequentially, and the execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present application.
[0042] The terms used in the embodiments of the present application are only for the purpose of describing specific embodiments, and are not intended to limit the present application. The singular forms "a", "said" and "the" used in the embodiments of the present application and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.
[0043] The weight of the relevant components mentioned in the embodiment description of the present application can not only refer to the specific content of each component, but also represent the proportional relationship between the weights of the components. Therefore, as long as the content of the relevant components is proportionally enlarged or reduced according to the embodiment description of the present application, it is within the scope disclosed in the embodiment description of the present application. Specifically, the mass described in the embodiment description of the present application can be a mass unit known in the chemical industry such as μg, mg, g, kg, etc.
[0044] The terms "first" and "second" are used only for descriptive purposes to distinguish objects such as substances from each other, and should not be understood as indicating or implying relative importance or implicitly indicating the number of indicated technical features. For example, without departing from the scope of the embodiments of the present application, the first XX may also be referred to as the second XX, and similarly, the second XX may also be referred to as the first XX. Thus, features defined as "first" and "second" may explicitly or implicitly include one or more of the features.
[0045] The importance of lithium battery separators is self-evident due to the important role they play in the battery structure. This is mainly reflected in two aspects: first, the separator can separate the positive and negative electrodes to prevent the positive and negative electrodes from contacting and causing a short circuit in the battery; second, it can "block electrons and pass ions". The micropores in the separator allow ions to pass through while ensuring that electrons cannot pass through, forming a complete charge and discharge circuit. The common separators on the market are mainly divided into PP separators, PE separators, PI separators and PVDF separators, etc. Most of them are coated on one side, but the improvement of the comprehensive performance of the separator is also limited.
[0046] In response to the above problems, the present application provides a method for preparing a lithium battery diaphragm coating slurry and a lithium battery diaphragm, the purpose of which is to adopt a new structure of boehmite and provide three different types of diaphragm coating slurries, namely alumina (Al2O3) slurry, boehmite (AlOOH) slurry and PVDF slurry, and adopt different coating methods and slurry combinations to maximize the durability of the diaphragm and the life and safety of the battery.
[0047] The first aspect of the embodiment of the present application provides a method for preparing a lithium battery separator coating slurry, comprising the following steps:
[0048] 0.2126 parts of dispersant and 1.2622 parts of pure water were mixed and stirred in a dispersion tank at a speed of 840-860 rpm for 30 minutes to dissolve the dispersant in the pure water;
[0049] Add 0.01432 parts of thickener to the solution and stir for 15 minutes at a speed of 840-860 rpm, then add 1 part of porous boehmite powder pretreated with anhydrous ethanol, mix and stir for 50 minutes at a speed of 840-860 rpm;
[0050] Pour the stirred slurry into a grinder and grind it twice. The grinding time is 18 minutes and 42 minutes respectively. The speed of the grinder is 640-660 rpm and the grinding temperature is 25-30°C.
[0051] Pour the ground slurry into the disperser again, add 0.2000 parts of binder and stir for 30 minutes at a speed of 290-310 rpm, then add 0.0020 parts of wetting agent and stir for 20 minutes at a speed of 190-210 rpm;
[0052] The prepared slurry is discharged, and iron is removed and filtered during the discharge, with a magnetic field strength of 10000 gs and a filter element of 300 meshes, to obtain a porous boehmite slurry.
[0053] In application, the preparation of porous boehmite slurry (AlOOH slurry) is based on the weight proportion of the formula components. Boehmite powder is set at 1 part, pure water is 1.2622 parts, thickener is 0.01432 parts, dispersant is 0.2126 parts, binder is 0.2000 parts, and wetting agent is 0.0020 parts. Boehmite must be pretreated with anhydrous ethanol before slurrying. The purpose is to improve the dispersibility of boehmite and reduce the occurrence of agglomeration. More importantly, due to its unique porous structure, using anhydrous ethanol to "dredge" the pores of boehmite can maximize its effect. Boehmite adopts a porous hollow structure with a pore structure of 1-200nm. Its structure is as follows: Figure 1 shown.
[0054] In some embodiments, the method for preparing the lithium battery separator coating slurry further includes:
[0055] 0.3568 parts of dispersant and 1.1959 parts of pure water were mixed and stirred in a dispersion tank at a speed of 840-860 rpm for 30 minutes to dissolve the dispersant in the pure water;
[0056] Add 0.0120 parts of thickener to the solution and stir for 15 minutes at a speed of 840-860 rpm, then add 1 part of alumina powder, mix and stir for 50 minutes at a speed of 840-860 rpm;
[0057] Pour the stirred slurry into a grinder and grind it twice. The grinding time is 18 minutes and 42 minutes respectively. The speed of the grinder is 640-660 rpm and the grinding temperature is 25-30°C.
[0058] Pour the ground slurry into the disperser again, add 0.1365 parts of binder and stir for 30 minutes at a speed of 290-310 rpm, then add 0.0016 parts of wetting agent and stir for 20 minutes at a speed of 190-210 rpm;
[0059] The prepared slurry is discharged, and iron is removed and filtered during the discharge, with a magnetic field strength of 10000 gs and a filter element of 300 meshes to obtain alumina slurry.
[0060] In application, the preparation of alumina slurry (Al2O3 slurry) also measures the formula components according to the weight proportions, and the process is almost the same as that of porous boehmite slurry. The difference is that the proportions of the formula components are different, 1 part of alumina powder, 1.1959 parts of pure water, 0.0120 parts of thickener, 0.3568 parts of dispersant, 0.1365 parts of binder, and 0.0016 parts of wetting agent.
[0061] In some embodiments, the method for preparing the lithium battery separator coating slurry further includes:
[0062] Stir 0.7407 parts of binder and 3.7592 parts of pure water in a disperser for 30 minutes to dissolve the binder in the pure water at a speed of 990-1010 rpm;
[0063] Add 0.6 parts of PVDF to the solution and stir for 15 minutes at a speed of 490-510 rpm, then increase the speed to 1000 rpm and continue stirring for 30 minutes;
[0064] 0.4 parts of PVDF was added to the mixed solution and stirred for 15 minutes, the rotation speed was reduced to 490-510 rpm, and then the rotation speed was increased to 2000 rpm and stirring was continued for 180 minutes;
[0065] Add 3.7593 parts of pure water to the slurry and stir for 60 minutes at 2000 rpm;
[0066] The prepared slurry was discharged, and iron was removed and filtered during the discharge, with a magnetic field strength of 10000 gs and a filter element of 300 meshes to obtain PVDF slurry.
[0067] In application, the preparation of PVDF (polyvinylidene fluoride) slurry also measures the formula components according to the weight percentage. The method is different from the above two slurries. The materials only need pure water, PVDF and binder. The main powder PVDF is still set at 1 part, pure water is 7.5185 parts, and the binder is 0.7407 parts.
[0068] Furthermore, the thickener includes carboxymethyl cellulose, the binder includes polymethyl methacrylate, and the dispersant includes ammonium salt.
[0069] In the application, the thickener used in the slurry is carboxymethyl cellulose (CMC), the binder is polymethyl methacrylate (PMMA), the dispersant is ammonium salt and other small amounts of additives.
[0070] Three different slurries were prepared in this application, and different preparation processes were used according to the physical and chemical properties of the different slurries and the different functions they performed in the membrane coating, thereby improving the comprehensive performance of the membrane to the greatest extent. The parameters of the three different slurries are shown in Table 1, and two tests were conducted on different types of slurries.
[0071]
[0072] Table 1
[0073] In the second aspect, the present application provides a lithium battery separator, the base film of which is a polyethylene separator, and the two sides of the base film are coated with different coating slurries, respectively, and the coating slurries include the porous boehmite slurry as described above, the alumina slurry as described above, and the PVDF slurry as described above.
[0074] In some embodiments, the base film has a thickness of 7 μm or 12 μm.
[0075] In some embodiments, the base film has a porosity of 30-40%.
[0076] In some embodiments, the coating slurry has a coating thickness of 3 μm.
[0077] In some embodiments, the porous boehmite slurry, the alumina slurry, and the PVDF slurry have a solid content of 10-90%, a D50 of 0.6-10 μm, and a viscosity of 50-150 mPa·s.
[0078] In some embodiments, the porous boehmite slurry and the alumina slurry are coated by roller coating, and the PVDF slurry is coated by spraying.
[0079] In the application, the base film used is a polyethylene diaphragm (PE), and the thickness of the base film is 7μm or 12μm. The basic performance parameters of the two thickness base films are shown in Table 2. In order to make the data more universal and extensive, four groups of 7μm and 12μm base films are selected for performance testing in Table 2. Al2O3 slurry AlOOH slurry is coated by roller coating, and PVDF slurry is coated by spraying. The coating thickness of the slurry is uniformly 3μm.
[0080]
[0081]
[0082] Table 2
[0083] Figure 2 This is a schematic diagram of three different slurry membrane coatings. Figure 3 This is a schematic diagram of the membrane coating equipment and coating process. The size of the base film is uniformly 2010mm (length) × 665mm (width), and the core size is 6 inches. When the base film is roller coated on one side, the coating speed is controlled at 80-100m / min, the feeding speed is 300-500, and the control of the tension of the five parts of unwinding, preheating, coating, discharging and winding is particularly important. Random adjustments are made according to the on-site process to ensure the quality of the membrane. The temperature of the preheating oven is about 10℃ higher than that of the oven.
[0084] When spraying the base film on one side, the coating speed remains basically unchanged, and the tension control is consistent with roller coating, but the feeding speed should be reduced to ensure the bonding force between the PVDF slurry and the surface of the base film and the uniform dispersion on the surface. The oven temperature is 5°C lower than that of roller coating. When roller coating the base film on both sides, the coating speed remains unchanged, the tension is increased by 5N, the feeding speed is maintained at about 400, and the oven temperature is consistent with that of roller coating on one side. When spraying and roller coating the base film on both sides, the coating parameters are basically the same as those of single-sided coating, but roller coating should be performed first and then spraying.
[0085] Several diaphragms with different thicknesses and different coating methods can be prepared. Diaphragm type 1 (single-sided coating): 7+3 (indicates that a 3μm coating of different slurry types is coated on a base film with a thickness of 7μm) and 12+3. Since three types of slurries are to be coated, six diaphragms appear in "diaphragm type 1". Diaphragm type 2 (double-sided coating): 7+3+3 (PE+Al2O3+AlOOH), 7+3+3 (PE+Al2O3+PVDF), 7+3+3 (PE+AlOOH+PVDF), 12+3+3 (PE+Al2O3+AlOOH), 12+3+3 (PE+Al2O3+PVDF), 12+3+3 (PE+AlOOH+PVDF). In order to distinguish the six types of "type 2" membranes, they are named "A", "B", "C", "D", "E" and "F" in order. The performance of the six different double-sided coated membranes is shown in Table 3 (the coating surfaces selected when measuring the membrane contact angle are AlOOH, Al2O3, and PVDF, respectively). In Table 3, two groups of performance tests were also conducted on the same type of composite membranes.
[0086]
[0087] Table 3
[0088] In this application, a unique pulping process and a simple coating process technology are used to combine organic and inorganic coating materials to improve the comprehensive performance of the diaphragm. The boehmite slurry uses a new porous hollow structure of boehmite, which is different from the traditional boehmite layer stacking structure. The diaphragm made of the traditional boehmite structure has low wettability and air permeability after slurry coating, and poor thermal shrinkage performance at high temperature. The boehmite with a special porous structure greatly improves the wettability of the diaphragm, and the diaphragm exhibits excellent wettability and high heat resistance.
[0089] It can be seen from Table 3 that double-sided coating of alumina and boehmite on the surface of the base film can greatly improve the thermal stability of the diaphragm at high temperatures, reduce the thermal shrinkage of the diaphragm, and further improve the puncture resistance. At the same time, alumina and boehmite themselves have good thermal stability, which can greatly reduce the film rupture temperature of the base film and resist thermal runaway reactions at high temperatures in lithium batteries. Alumina also has excellent corrosion resistance, and boehmite has good low-temperature performance. Therefore, coating the base film with two coating materials with their own advantages can improve the comprehensive performance of the coating film without losing the original performance of the base film, thereby greatly improving the safety and battery life of lithium batteries.
[0090] The embodiments described above are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, a person skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. Such modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present application, and should all be included in the protection scope of the present application.
Claims
1. A method for preparing a lithium battery separator coating slurry, It is characterized in that include: 0.2126 parts of dispersant and 1.2622 parts of pure water were mixed and stirred in a dispersion tank at a speed of 840-860 rpm for 30 minutes to dissolve the dispersant in the pure water; Add 0.01432 parts of thickener to the solution and stir for 15 minutes at a speed of 840-860 rpm, then add 1 part of porous boehmite powder pretreated with anhydrous ethanol, mix and stir for 50 minutes at a speed of 840-860 rpm; Pour the stirred slurry into a grinder and grind it twice. The grinding time is 18 minutes and 42 minutes respectively. The speed of the grinder is 640-660 rpm and the grinding temperature is 25-30°C. Pour the ground slurry into the disperser again, add 0.2000 parts of binder and stir for 30 minutes at a speed of 290-310 rpm, then add 0.0020 parts of wetting agent and stir for 20 minutes at a speed of 190-210 rpm; The prepared slurry is discharged, and iron is removed and filtered during the discharge, with a magnetic field strength of 10000 gs and a filter element of 300 meshes, to obtain a porous boehmite slurry.
2. The method for preparing the lithium battery separator coating slurry according to claim 1, It is characterized in that Also includes: 0.3568 parts of dispersant and 1.1959 parts of pure water were mixed and stirred in a dispersion tank at a speed of 840-860 rpm for 30 minutes to dissolve the dispersant in the pure water; Add 0.0120 parts of thickener to the solution and stir for 15 minutes at a speed of 840-860 rpm, then add 1 part of alumina powder, mix and stir for 50 minutes at a speed of 840-860 rpm; Pour the stirred slurry into a grinder and grind it twice. The grinding time is 18 minutes and 42 minutes respectively. The speed of the grinder is 640-660 rpm and the grinding temperature is 25-30°C. Pour the ground slurry into the disperser again, add 0.1365 parts of binder and stir for 30 minutes at a speed of 290-310 rpm, then add 0.0016 parts of wetting agent and stir for 20 minutes at a speed of 190-210 rpm; The prepared slurry is discharged, and iron is removed and filtered during the discharge, with a magnetic field strength of 10000 gs and a filter element of 300 meshes to obtain alumina slurry.
3. The method for preparing the lithium battery separator coating slurry according to claim 1, It is characterized in that Also includes: Stir 0.7407 parts of binder and 3.7592 parts of pure water in a disperser for 30 minutes to dissolve the binder in the pure water at a speed of 990-1010 rpm; Add 0.6 parts of PVDF to the solution and stir for 15 minutes at a speed of 490-510 rpm, then increase the speed to 1000 rpm and continue stirring for 30 minutes; 0.4 parts of PVDF was added to the mixed solution and stirred for 15 minutes, the speed was reduced to 490-510 rpm, and then the speed was increased to 2000 rpm and stirring was continued for 180 minutes; Add 3.7593 parts of pure water to the slurry and stir for 60 minutes at 2000 rpm; The prepared slurry was discharged, and iron was removed and filtered during the discharge, with a magnetic field strength of 10000 gs and a filter element of 300 meshes to obtain PVDF slurry.
4. The method for preparing the lithium battery separator coating slurry according to any one of claims 1 to 3, It is characterized in that The thickener includes carboxymethyl cellulose, the binder includes polymethyl methacrylate, and the dispersant includes ammonium salt.
5. A lithium battery separator, It is characterized in that The base film of the lithium battery separator is a polyethylene separator, and different coating slurries are coated on both sides of the base film, respectively. The coating slurries include the porous boehmite slurry as claimed in claim 1, the alumina slurry as claimed in claim 2, and the PVDF slurry as claimed in claim 3.
6. The lithium battery separator according to claim 5, It is characterized in that The base film has a thickness of 7 μm or 12 μm.
7. The lithium battery separator according to claim 5, It is characterized in that The porosity of the base film is 30-40%.
8. The lithium battery separator according to claim 5, It is characterized in that The coating thickness of the coating slurry was 3 μm.
9. The lithium battery separator according to claim 5, It is characterized in that The porous boehmite slurry, the alumina slurry and the PVDF slurry have a solid content of 10-90%, a D50 of 0.6-10 μm and a viscosity of 50-150 mPa·s.
10. The lithium battery separator according to claim 5, It is characterized in that The porous boehmite slurry and the alumina slurry are coated by roller coating, and the PVDF slurry is coated by spraying.
Citation Information
Cited By
Reinforced diaphragm material for power battery and preparation method of reinforced diaphragm material
CN121054956A
Reinforced separator material for power batteries and method for preparing the same
CN121054956B