All-solid-state battery
By using an oxide coating with a different composition from Li transition metal oxide in the positive electrode of an all-solid-state battery, the problem of poor battery cycle characteristics is solved and more efficient charge and discharge performance is achieved.
Patent Information
- Application Number
- CN202280092561.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-02-28
- Filing Date
- 2022-09-30
- Publication Date
- 2024-10-08
AI Technical Summary
The performance of existing all-solid-state batteries deteriorates after multiple charges and discharges, and the cycle characteristics are poor. It is necessary to improve the cycle characteristics.
A positive electrode containing a compound of Ag and a Li transition metal oxide is used, and an oxide having a composition different from that of the Li transition metal oxide is formed as a coating in the positive electrode to ensure that Ag is not oxidized, thereby improving the cycle characteristics of the battery.
By forming an oxide film with a different composition from Li transition metal oxide in the positive electrode, the oxidation of Ag is effectively suppressed and the cycle characteristics and energy efficiency of the all-solid-state battery are improved.
Smart Images

Figure CN118749140A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an all-solid-state battery.
[0002] This application claims priority based on Japanese Patent Application No. 2022-029456 filed in Japan on February 28, 2022, and the contents are cited herein. Background Art
[0003] In recent years, electronic technology has developed significantly, achieving small, light, thin, and multifunctional portable electronic devices. Along with this, there is a strong desire for batteries, which serve as power sources for electronic devices, to be small, light, thin, and have improved reliability. All-solid batteries using solid electrolytes as electrolytes have attracted much attention.
[0004] All-solid batteries are available in thin film and bulk types. Thin film types are made using thin film technologies such as physical vapor deposition (PVD) and sol-gel methods. Bulk types are made using powder forming methods, sintering methods, and the like. Different all-solid batteries can be used with different materials or have different performances due to different manufacturing methods. For example, bulk types that use sintered bodies require materials that can withstand sintering. On the other hand, since each layer can be thickened, it has a high capacity.
[0005] For example, Patent Document 1 discloses a sintered all-solid-state battery using an oxide-based solid electrolyte as a solid electrolyte.
[0006] Prior art literature
[0007] Patent Literature
[0008] [Patent Document 1] International Publication No. 2007 / 135790 Summary of the invention
[0009] Technical problem to be solved by the invention
[0010] In batteries, it is important to minimize degradation in performance even after repeated charging and discharging, and all-solid-state batteries with excellent cycle characteristics are required.
[0011] The present invention has been accomplished in view of the above-mentioned technical problems, and its object is to improve the cycle characteristics of all-solid-state batteries.
[0012] Methods used to solve technical problems
[0013] In order to solve the above technical problems, the following means are provided.
[0014] (1) The first embodiment of an all-solid-state battery comprises a sintered body having: a positive electrode, a negative electrode, and a solid electrolyte layer between the positive electrode and the negative electrode, wherein the positive electrode comprises a compound containing Ag, a Li-containing transition metal oxide, and an oxide having a composition different from that of the Li-transition metal oxide, the oxide comprises Ag, and at least a portion of the compound containing Ag and the Li-transition metal oxide are present inside the positive electrode via the oxide.
[0015] (2) In the all-solid-state battery of the above aspect, the oxide may include a transition metal element constituting the Li transition metal oxide.
[0016] (3) In the all-solid-state battery of the above aspect, the minimum thickness of the oxide between the compound containing Ag and at least a portion of the Li transition metal oxide may be 0.01 μm or more and 2.0 μm or less.
[0017] (4) In the all-solid-state battery of the above aspect, a contact ratio between the Li transition metal oxide and the compound containing Ag in a cross section of the positive electrode may be 0.1% or more and 10% or less.
[0018] (5) In the all-solid-state battery of the above aspect, the compound containing Ag may be any one selected from Ag or Ag / Pd.
[0019] (6) In the all-solid-state battery of the above embodiment, the positive electrode may include: a first layer; and a second layer located on at least one main surface of the first layer, wherein the first layer includes the compound containing Ag, the Li-containing transition metal oxide, and the oxide.
[0020] (7) In the all-solid-state battery of the above aspect, the second layer may include the Li transition metal oxide.
[0021] (8) In the all-solid-state battery of the above aspect, the first layer and the second layer may include Li transition metal oxides having the same composition.
[0022] (9) In the all-solid-state battery of the above aspect, the positive electrode may include lithium cobalt oxide.
[0023] Effects of the Invention
[0024] The all-solid-state battery of the above-described embodiment can improve the cycle characteristics. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is a cross-sectional view of the all-solid-state battery according to the first embodiment.
[0026] Figure 2 This is an enlarged cross-sectional view of a portion of the positive electrode according to the first embodiment.
[0027] Figure 3 This is a cross-sectional view showing an enlarged portion of another example of the positive electrode according to the first embodiment.
[0028] Figure 4 This is an enlarged cross-sectional view of a portion of the negative electrode according to the first embodiment.
[0029] Figure 5 This is a partially enlarged cross-sectional view of another example of the negative electrode according to the first embodiment.
[0030] Description of Reference Numerals
[0031] 1……positive electrode;
[0032] 1A, 1C...positive electrode current collector layer (first layer);
[0033] 1B: positive electrode active material layer (second layer);
[0034] 1D…middle layer;
[0035] 2. 2C… negative electrode;
[0036] 2A……negative electrode current collector layer;
[0037] 2B……Negative electrode active material layer;
[0038] 3...Solid electrolyte layer;
[0039] 4...Laminated body;
[0040] 5, 6……terminal electrodes;
[0041] 10……All-solid-state batteries;
[0042] 11……positive electrode current collector (compound containing Ag);
[0043] 21……negative electrode current collector;
[0044] 12……positive electrode active material (Li transition metal oxide);
[0045] 13 ... oxides (oxides) having a composition different from that of Li transition metal oxides;
[0046] 22……Negative electrode active material;
[0047] 23……Solid electrolyte. DETAILED DESCRIPTION
[0048] Hereinafter, the present embodiment will be described in detail with reference to the accompanying drawings as appropriate. In the accompanying drawings used in the following description, in order to facilitate the understanding of the features of the present invention, the features are sometimes enlarged for convenience, and the dimensional ratios of the various components are sometimes different from the actual ones. The materials, dimensions, etc. illustrated in the following description are examples, and the present invention is not limited thereto, and can be implemented by appropriately changing within the scope of not changing its purpose.
[0049] Define the direction. The stacking direction of the stacked body 4 is set to the z direction, a direction in the plane perpendicular to the z direction is set to the x direction, and a direction perpendicular to the x direction and the z direction is set to the y direction. Hereinafter, a direction in the z direction is sometimes expressed as "up", and the direction opposite to the direction is expressed as "down". Up and down are not necessarily consistent with the direction in which gravity is applied.
[0050] Figure 1 1 is a schematic cross-sectional view of the all-solid battery 10 of the present embodiment. The all-solid battery 10 has a stack 4 and terminal electrodes 5, 6. The terminal electrodes 5, 6 are in contact with the opposite surfaces of the stack 4, respectively. The terminal electrodes 5, 6 extend in the z direction intersecting (orthogonal) with the stacking surface of the stack 4.
[0051] The laminate 4 has a positive electrode 1, a negative electrode 2 and a solid electrolyte layer 3. The laminate 4 is a sintered body formed by stacking the positive electrode 1, the negative electrode 2 and the solid electrolyte layer 3 and sintering them. There is no limit to the number of layers of the positive electrode 1 and the negative electrode 2. The solid electrolyte layer 3 is at least located between the positive electrode 1 and the negative electrode 2. Between the positive electrode 1 and the terminal electrode 6 and between the negative electrode 2 and the terminal electrode 5, for example, there is a solid electrolyte that is the same as the solid electrolyte layer 3. One end of the positive electrode 1 is connected to the terminal electrode 5. One end of the negative electrode 2 is connected to the terminal electrode 6.
[0052] The all-solid-state battery 10 is charged or discharged by transferring ions between the positive electrode 1 and the negative electrode 2 via the solid electrolyte layer 3. Figure 1 In the figure, a stacked battery is shown, but a wound battery may also be used. The all-solid battery 10 may be used, for example, for a laminated battery, a square battery, a cylindrical battery, a coin battery, a button battery, etc. In addition, the all-solid battery 10 may also be a liquid injection type in which the solid electrolyte layer 3 is dissolved or dispersed in a solvent.
[0053] "positive electrode"
[0054] Figure 2This is an enlarged view of a portion of the positive electrode 1 of the first embodiment. In terms of structure, the positive electrode 1 includes, for example, a positive electrode current collector layer 1A (sometimes referred to as "first layer" in this specification) and a positive electrode active material layer 1B (sometimes referred to as "second layer" in this specification). In terms of composition, the positive electrode 1 includes, for example, a compound containing Ag, a Li-containing transition metal oxide, and an oxide having a composition different from that of the Li-containing transition metal oxide (hereinafter referred to as "oxide").
[0055] The oxide includes Ag.
[0056] The compound containing Ag and at least a part of the Li-containing transition metal oxide are present inside the positive electrode (for example, inside the positive electrode collector layer or inside the positive electrode collector layer and the positive electrode active material layer) via the oxide.
[0057] [Positive electrode current collector layer]
[0058] The positive electrode current collector layer (first layer) 1A includes, for example, a positive electrode current collector 11 (sometimes referred to as a "compound containing Ag" in this specification), a positive electrode active material 12 (sometimes referred to as a "Li transition metal oxide" in this specification), and an oxide 13 (oxide) having a composition different from that of the Li transition metal oxide. In this case, the area between the uppermost xy plane passing through the oxide 13 having a composition different from that of the Li transition metal oxide and the xy plane passing through the lowermost area is regarded as the positive electrode current collector layer 1A.
[0059] The positive electrode current collector 11 contains Ag. For example, the positive electrode current collector 11 contains a metal or alloy containing Ag. The Ag metal or alloy does not melt even when the stack 4 is heated in the air atmosphere and is difficult to oxidize. For example, the positive electrode current collector 11 is Ag or AgPd alloy.
[0060] The positive electrode current collector 11 is composed of, for example, a plurality of conductive particles. The plurality of conductive particles are connected to each other and are electrically connected in the xy plane. The positive electrode current collector 11 is not limited to this example, and may be, for example, a foil, a stamped film, or an extended product extending in the xy plane.
[0061] The positive electrode active material 12 is mixed with the positive electrode current collector 11 and exists in the positive electrode current collector layer 1A. When the positive electrode active material 12 is contained in the positive electrode current collector layer 1A, the transfer of electrons between the positive electrode active material 12 and the positive electrode current collector 11 becomes smooth.
[0062] The positive electrode active material 12 is not particularly limited as long as it can reversibly release and adsorb lithium ions, and remove and insert lithium ions. For example, a positive electrode active material used in a known lithium ion secondary battery can be used.
[0063] The positive electrode active material 12 is, for example, a composite transition metal oxide (including a Li transition metal oxide). The positive electrode active material 12 is preferably a transition metal oxide containing at least one selected from Co, Ni, Mn, Fe, and V. The positive electrode active material 12 is preferably a lithium manganese composite oxide, a lithium nickel composite oxide, a lithium cobalt composite oxide, a lithium vanadium composite oxide, a lithium titanium composite oxide, manganese dioxide, titanium oxide, niobium oxide, vanadium oxide, tungsten oxide, etc. For example, the positive electrode active material 12 is LiCoO2 or LiMnO2. These compounds may deviate from the stoichiometric composition.
[0064] For example, the positive electrode active material 12 may be Li x For lithium cobalt oxide represented by CoO2, x varies in the range of 0.4 to 1.2 as the all-solid-state battery is charged and discharged.
[0065] In addition, a positive electrode active material that does not contain lithium can also be used as the positive electrode active material 12. These positive electrode active materials can be used by pre-arranging a negative electrode active material doped with metallic lithium or lithium ions at the negative electrode and starting the battery from discharge. For example, metal oxides (MnO2, V2O5, etc.) that do not contain lithium are examples of these positive electrode active materials.
[0066] The oxide 13 (oxide) having a composition different from the Li transition metal oxide is located between the positive electrode collector 11 and the positive electrode active material 12. The oxide 13 having a composition different from the Li transition metal oxide is an oxide containing Ag. The oxide 13 having a composition different from the Li transition metal oxide prevents oxidation of Ag contained in the positive electrode collector 11, and the cycle characteristics of the all-solid-state battery 10 are improved.
[0067] The oxide 13 having a composition different from that of the Li transition metal oxide preferably contains a constituent element constituting the positive electrode active material 12. For example, when the positive electrode active material 12 is LiCoO2, the oxide 13 having a composition different from that of the Li transition metal oxide is preferably AgCoO2. For example, when the positive electrode active material 12 is LiMn2O4, the oxide 13 having a composition different from that of the Li transition metal oxide is preferably AgMn2O4.
[0068] The thickness of the oxide 13 having a composition different from that of the Li transition metal oxide is, for example, greater than 0.01 μm. The thickness of the oxide 13 having a composition different from that of the Li transition metal oxide is preferably greater than 0.1 μm. The thickness of the oxide 13 having a composition different from that of the Li transition metal oxide can be obtained from a scanning electron microscope image. First, in the image, a first imaginary line passing through the uppermost portion of the positive electrode current collector 11 is drawn. Next, a second imaginary line passing through the uppermost portion of the oxide 13 having a composition different from that of the Li transition metal oxide is drawn. The width between the first imaginary line and the second imaginary line is set to the thickness of the oxide 13 having a composition different from that of the Li transition metal oxide in the image. This processing is performed in 10 images, and the average value thereof is defined as "the thickness of the oxide 13 having a composition different from that of the Li transition metal oxide (the thickness of the oxide containing the Ag compound and at least a portion of the Li transition metal oxide)". Here, the first imaginary line and the second imaginary line are defined as a line passing through the uppermost portion of the positive electrode current collector 11 and a line passing through the uppermost portion of the oxide 13 having a composition different from the Li transition metal oxide, respectively. However, they may be defined by lines passing through their respective lowermost portions.
[0069] [Positive electrode active material layer]
[0070] The positive electrode active material layer 1B (second layer) is formed on one or both sides of the positive electrode collector layer 1A. The positive electrode active material layer 1B contains a positive electrode active material. The positive electrode active material layer 1B may contain a conductive additive, a binding material, and a solid electrolyte described later. When the positive electrode active material layer 1B contains a solid electrolyte, the boundary between the outermost xy plane passing through the positive electrode active material and the positive electrode collector layer 1A is regarded as the positive electrode active material layer 1B.
[0071] The positive electrode active material contained in the positive electrode active material layer 1B is the same as the positive electrode active material 12 contained in the positive electrode current collector layer 1A.
[0072] The conductive aid is not particularly limited as long as it can improve the electron conductivity in the positive electrode active material layer 1B, and a known conductive aid can be used. Examples of the conductive aid include carbon materials such as graphite, carbon black, graphene, and carbon nanotubes, metals such as gold, platinum, silver, palladium, aluminum, copper, nickel, stainless steel, and iron, conductive oxides such as ITO, or mixtures thereof. The conductive aid may be in the form of powder or fiber.
[0073] The binder bonds the positive electrode current collector layer 1A and the positive electrode active material layer 1B, the positive electrode active material layer 1B and the solid electrolyte layer 3 , and various materials constituting the positive electrode active material layer 1B.
[0074] The binding material can be used within the range that the function of the positive electrode active material layer 1B is not lost. The binding material may not be contained unless it is necessary. The content of the binding material in the positive electrode active material layer 1B is, for example, 0.5 to 30% by volume of the positive electrode active material layer. If the content of the binding material is small enough, the resistance of the positive electrode active material layer 1B becomes low enough. Here, the volume % is roughly consistent with the area % in the cross section measured by a scanning electron microscope, for example. Therefore, the area ratio in the cross section measured by a scanning electron microscope can be directly regarded as the volume ratio.
[0075] As long as the bonding material can be joined as described above, for example, fluororesins such as polyvinylidene fluoride (PVDF) and polytetrafluoroethylene (PTFE) can be cited. Furthermore, in addition to the above, as bonding materials, for example, cellulose, styrene-butadiene rubber, ethylene-propylene rubber, polyimide resin, polyamide-imide resin, etc. can also be used. In addition, as bonding materials, conductive polymers with electronic conductivity and ionic conductive polymers with ionic conductivity can also be used. As conductive polymers with electronic conductivity, for example, polyacetylene can be cited. In this case, the bonding material also plays the function of a conductive auxiliary agent, so a conductive auxiliary agent may not be added. As an ionic conductive polymer with ionic conductivity, for example, an ionic conductive polymer that conducts lithium ions can be used, and monomers of polymer compounds (polyether polymer compounds such as polyethylene oxide and polypropylene oxide, polyphosphazenes, etc.) can be cited with lithium salts such as LiClO4, LiBF4, LiPF6, or alkali metal salts with lithium as the main body. The obtained material is compounded. The polymerization initiator used for the composite formation may be, for example, a photopolymerization initiator or a thermal polymerization initiator suitable for the above-mentioned monomers. The properties required of the adhesive material include oxidation and reduction resistance and good adhesiveness.
[0076] So far, a specific example of an example of a positive electrode has been shown, but the positive electrode is not limited to these examples. For example, the positive electrode collector layer (first layer) can be composed only of the positive electrode collector 11 (compound containing Ag). In this case, the oxide 13 (oxide) having a composition different from the Li transition metal oxide is located between the positive electrode collector layer (first layer) and the positive electrode active material layer (second layer). In addition, the positive electrode can be a single layer in which the positive electrode collector 11 (compound containing Ag), the positive electrode active material 12 (Li transition metal oxide) and the oxide 13 (oxide) having a composition different from the Li transition metal oxide are mixed.
[0077] in addition, Figure 3 This is a cross-sectional view along the stacking direction of another example of the positive electrode according to the first embodiment. Figure 3The positive electrode shown has a positive electrode collector layer 1C, an intermediate layer 1D, and a positive electrode active material layer 1B. The positive electrode collector layer 1C has a positive electrode collector 11 and an oxide 13 (oxide) having a composition different from that of the Li transition metal oxide. The intermediate layer 1D is composed of an oxide 13 (oxide) having a composition different from that of the Li transition metal oxide. Figure 3 The example shown corresponds to the thickness ratio of the oxide 13 (oxide) having a composition different from the Li transition metal oxide. Figure 2 The example shown is a thick case.
[0078] "Solid electrolyte layer"
[0079] The solid electrolyte layer 3 includes a solid electrolyte. A solid electrolyte is a substance that can move ions by an electric field applied from the outside. For example, the solid electrolyte layer 3 conducts lithium ions and blocks the movement of electrons. The solid electrolyte layer 3 is, for example, a sintered body obtained by sintering.
[0080] The solid electrolyte layer 3 includes, for example, a solid electrolyte having a γ-Li3PO4 type crystal structure. The solid electrolyte having a γ-Li3PO4 type crystal structure has excellent ion conductivity. The solid electrolyte is, for example, Li 3+x Si x P 1-x O4、Li 3+x Si x V 1- x O4、Li 3+x Ge x P 1-x O4、Li 3+x Ge x V 1-x O4, etc., preferably Li 3+x Si x P 1-x O4. x satisfies 0.4≤x≤0.8. In addition, the solid electrolyte may be a ternary lithium oxide containing Si, V, Ge, etc.
[0081] "negative electrode"
[0082] Figure 4 This is an enlarged view of a portion of the negative electrode 2 of the first embodiment. The negative electrode 2 includes, for example, a negative electrode current collector layer 2A and a negative electrode active material layer 2B containing a negative electrode active material.
[0083] The negative electrode current collector layer 2A includes, for example, a negative electrode current collector 21 and a negative electrode active material 22. In this case, the portion between the xy plane passing through the uppermost portion of the negative electrode current collector 21 and the xy plane passing through the lowermost portion is considered to be the negative electrode current collector layer 2A.
[0084] The negative electrode current collector 21 includes, for example, a metal or an alloy containing any one selected from Ag, Pd, Au, and Pt. The negative electrode current collector 21 is preferably, for example, an AgPd alloy, Au, or Pt.
[0085] The negative electrode current collector 21 is composed of, for example, a plurality of conductive particles. The plurality of conductive particles are connected to each other and are electrically connected in the xy plane. The negative electrode current collector 21 is not limited to this example, and may be, for example, a foil, a stamped film, or an extended product extending in the xy plane.
[0086] The negative electrode active material 22 is mixed with the negative electrode current collector 21 and exists in the negative electrode current collector layer 2A, for example. The negative electrode active material 22 is in contact with the negative electrode current collector 21. If the negative electrode active material 22 is contained in the negative electrode current collector layer 2A, the transfer of electrons between the negative electrode active material 22 and the negative electrode current collector 21 becomes smooth. The negative electrode active material 22 is the same as the negative electrode active material contained in the negative electrode active material layer 2B described later.
[0087] The negative electrode active material layer 2B is formed on one or both sides of the negative electrode collector layer 2A. The negative electrode active material layer 2B contains a negative electrode active material. The negative electrode active material layer 2B may contain a conductive additive, a binder, and the above-mentioned solid electrolyte. When the negative electrode active material layer 2B contains a solid electrolyte, the boundary surface between the outermost xy plane passing through the negative electrode active material and the negative electrode collector layer 2A is regarded as the negative electrode active material layer 2B.
[0088] The negative electrode active material is a compound that can adsorb and release ions. The negative electrode active material is a compound that exhibits a lower potential than the positive electrode active material. As the negative electrode active material, the same material as the positive electrode active material can be used. The negative electrode active material and the positive electrode active material used in the all-solid-state battery 10 are determined in consideration of the potential of the negative electrode active material and the potential of the positive electrode active material. The negative electrode active material is, for example, Li4Ti5O 12 , LiTiO2, Li2TiO3, Li2TiSiO5.
[0089] The conductive additive improves the electron conductivity of the negative electrode active material layer 2B. The conductive additive can be made of the same material as that of the positive electrode active material layer 1B.
[0090] The binder binds the negative electrode current collector layer 2A and the negative electrode active material layer 2B, the negative electrode active material layer 2B and the solid electrolyte layer 3, and various materials constituting the negative electrode active material layer 2B. The binder can use the same material as the positive electrode active material layer 1B. The content ratio of the binder can also be the same as that of the positive electrode active material layer 1B. As long as the binder is not needed, the binder may not be contained.
[0091] exist Figure 4In the example in which the negative electrode 2 is composed of the negative electrode collector layer 2A and the negative electrode active material layer 2B, the present invention is not limited to this case. For example, the negative electrode collector layer 2A may be composed of only the negative electrode collector 21 .
[0092] in addition, Figure 5 This is an enlarged view of a part of another example of the negative electrode according to the first embodiment. Figure 5 The negative electrode 2C shown has a negative electrode collector 21 and a solid electrolyte 23. The negative electrode collector 21 is, for example, a metal or alloy containing Ag. Ag also functions as an active material. When Ag functions as a negative electrode active material, the potential window of the all-solid-state battery is expanded, and a charge and discharge reaction occurs between a high potential (about 3.8V) and a low potential (about 0V). As a result, the all-solid-state battery becomes high-capacity and the energy density of the all-solid-state battery is improved.
[0093] "Method for manufacturing all-solid-state batteries"
[0094] Next, a method for manufacturing the all-solid-state battery 10 is described. First, the stacked body 4 is produced. The stacked body 4 is produced by, for example, a simultaneous firing method or a sequential firing method.
[0095] The simultaneous firing method is a method of manufacturing the laminate 4 by stacking the materials forming each layer and then firing them all at once. The sequential firing method is a method of firing each layer each time it is formed. The simultaneous firing method can manufacture the laminate 4 with fewer operation steps than the sequential firing method. In addition, the laminate 4 manufactured by the simultaneous firing method is denser than the laminate 4 manufactured by the sequential firing method. The following is an example of the case where the simultaneous firing method is used.
[0096] First, the materials constituting the positive electrode current collector layer 1A, the positive electrode active material layer 1B, the solid electrolyte layer 3, the negative electrode active material layer 2B, and the negative electrode current collector layer 2A are made into pastes. Figure 2 In the example shown, the positive electrode current collector 11 is coated with an oxide 13 having a composition different from that of the Li transition metal oxide and then made into a paste. Figure 3 In the case of the example shown, the material constituting the intermediate layer 1D is also in the form of a paste.
[0097] The method of making each material into a paste is not particularly limited, and for example, a method of mixing powders of each material in a carrier to obtain a paste can be used. Here, the carrier is a general term for a medium in a liquid phase. The carrier includes a solvent and a binder.
[0098] Next, a green sheet is prepared. The green sheet is obtained by applying the paste prepared according to each material on a substrate such as a PET (polyethylene terephthalate) film, drying it as needed, and then peeling off the substrate. The method for applying the paste is not particularly limited, and for example, a known method such as screen printing, coating, transfer, and scraper can be used.
[0099] Next, the green sheets made from each material are stacked in the desired order and number of layers to make a laminated sheet. When stacking the green sheets, alignment and cutting are performed as needed. For example, in the case of making a parallel type or a series-parallel type battery, the green sheets are stacked in such a way that the end face of the positive electrode collector layer 1A is not consistent with the end face of the negative electrode collector layer 2A.
[0100] The laminated sheet can be produced by a method of producing a positive electrode unit and a negative electrode unit and stacking these units. The positive electrode unit is a laminated sheet in which a solid electrolyte layer 3, a positive electrode active material layer 1B, a positive electrode collector layer 1A, and a positive electrode active material layer 1B are stacked in this order. Figure 3 In the case of the example shown, the intermediate layer 1D is stacked between the positive electrode collector layer 1A and the positive electrode active material layer 1B. The negative electrode unit is a laminated sheet in which the solid electrolyte layer 3, the negative electrode active material layer 2B, the negative electrode collector layer 2A, and the negative electrode active material layer 2B are stacked in this order. The solid electrolyte layer 3 of the positive electrode unit is stacked in a manner opposite to the negative electrode active material layer 2B of the negative electrode unit, or the positive electrode active material layer 1B of the positive electrode unit is stacked in a manner opposite to the solid electrolyte layer 3 of the negative electrode unit.
[0101] Next, the prepared laminated sheets are pressurized together to improve the adhesion of each layer. Pressing can be performed, for example, by a molding machine, a warm isostatic press (WIP), a cold isostatic press (CIP), an isostatic press, etc. Pressing is preferably performed while heating. The heating temperature during crimping is, for example, set to 40 to 95° C. Next, the pressurized laminate is cut using a cutting device and formed into chips. Then, the chips are debonded and sintered to obtain a laminate 4 consisting of a sintered body.
[0102] The debinding process can be performed as a process different from the firing process. If the debinding process is performed, the binder component contained in the chip is heated and decomposed before the firing process, which can inhibit the rapid decomposition of the binder component in the firing process. The debinding process is performed, for example, by heating at a temperature of 300 to 800°C for 0.1 to 10 hours in an atmospheric atmosphere. The atmosphere of the debinding process is an oxygen partial pressure environment in which the materials constituting the positive electrode, the negative electrode and the solid electrolyte do not undergo oxidation and reduction or are difficult to undergo oxidation and reduction, and the gas type can be arbitrarily selected so that the materials constituting the positive electrode, the negative electrode and the solid electrolyte do not react with the atmospheric gas. For example, it can be performed in a nitrogen atmosphere, an argon atmosphere, a nitrogen-hydrogen mixed atmosphere, a water vapor atmosphere, and an atmosphere mixed with them.
[0103] The sintering process is carried out by placing the chip on a ceramic table, for example. Firing is carried out by heating to 600-1000° C. in an atmospheric atmosphere, for example. The atmosphere of the sintering process is an oxygen partial pressure environment in which the materials constituting the positive electrode, the negative electrode and the solid electrolyte do not undergo oxidation-reduction or are difficult to undergo oxidation-reduction, and the gas type can be arbitrarily selected so that the materials constituting the positive electrode, the negative electrode and the solid electrolyte do not react with the atmospheric gas. For example, it can be carried out in a nitrogen atmosphere, an argon atmosphere, a nitrogen-hydrogen mixed atmosphere, a water vapor atmosphere, and an atmosphere mixed with them.
[0104] In addition, the sintered laminate 4 (sintered body) can also be placed in a cylindrical container together with abrasive materials such as aluminum oxide and drum-ground. Thus, the chamfering of the corners of the laminate can be performed. Grinding can be performed using sandblasting. Sandblasting can only remove specific parts, so it is preferred.
[0105] Terminal electrodes 5 and 6 are formed on the mutually opposite sides of the manufactured stacked body 4. The terminal electrodes 5 and 6 can be formed by means of sputtering, dipping, screen printing, spraying, etc. By going through the above steps, a full solid-state battery 10 can be manufactured. When the terminal electrodes 5 and 6 are formed only in the specified parts, they are covered with tape or the like and the above treatment is performed.
[0106] The cycle characteristics of the all-solid battery of the present embodiment are excellent. The reason is not clear, but it is believed that the oxide 13 having a composition different from the Li transition metal oxide functions as a coating to prevent the oxidation of Ag during charge and discharge. The Ag contained in the positive electrode is oxidized at a potential of 3.84V or more. The use of energy in the reaction of the oxidation of Ag consumes energy in reactions other than the charge and discharge reactions of the all-solid battery, and the energy efficiency is poor. If an oxide 13 having a composition different from the Li transition metal oxide is preformed between the positive electrode collector 11 and the positive electrode active material 12, the oxidation of Ag can be suppressed. As a result, it is believed that the cycle characteristics of the all-solid battery are improved.
[0107] The embodiments of the present invention have been described in detail above with reference to the drawings, but each structure in each embodiment and their combination are merely examples, and addition, omission, replacement and other changes of structures are possible without departing from the gist of the present invention.
[0108] [Example]
[0109] "Example 1"
[0110] (Production of positive electrode paste)
[0111] First, Ag powder and Pd powder are prepared in a volume ratio of Ag powder: Pd powder = 80:20. Next, AgCoO2 powder having an oxide having a composition different from that of the Li transition metal oxide is prepared. Next, these powders are put into a mechanochemical reaction device (manufactured by Hosokawa Micron Co., Ltd., product name: Circulating Mechanical Fusion (Registered Trademark) System AMS). Then, an AgCoO2 coating is formed on the surface of the AgPd powder by a mechanochemical reaction. Then, ethyl cellulose and dihydropinolene are added to a powder of LiCoO2 as a positive electrode active material mixed with the powder in a volume ratio of 50:50, and mixed to prepare a positive electrode collector layer paste. Ethyl cellulose is a binder and dihydropinolene is a solvent.
[0112] The positive electrode active material layer paste is prepared by adding ethyl cellulose and dihydroterpineol to LiCoO2 and mixing them. LiCoO2 is the positive electrode active material.
[0113] (Preparation of Solid Electrolyte Layer Paste)
[0114] Li2CO3, SiO2 and Li3PO4 were used as starting materials and mixed at a molar ratio of 2:1:1. Water was used as a dispersion medium in a ball mill for wet mixing for 16 hours. The mixed material was calcined at 950°C for 2 hours to produce Li 3.5 Si 0.5 P 0.5 O4.
[0115] Then, 100 parts by mass of the calcined powder, 100 parts by mass of ethanol, and 200 parts by mass of toluene were added to a ball mill for wet mixing, and then 16 parts by mass of a polyvinyl butyral binder and 4.8 parts by mass of butyl benzyl phthalate were added and mixed to prepare a solid electrolyte layer paste.
[0116] (Preparation of negative electrode paste)
[0117] The negative electrode paste uses a mixture of Ag, Pd and Li in a volume ratio of 40:10:50. 3.5 Si0.5 P 0.5 The powder obtained by mixing ethyl cellulose and dihydroterpineol was prepared by mixing Ag as a negative electrode current collector and a negative electrode active material. The output voltage of the all-solid-state battery was close to 3.8V because Ag functioned as a negative electrode active material.
[0118] (Fabrication of all-solid-state batteries)
[0119] Next, the positive electrode unit and the negative electrode unit were made in the following order. First, the positive electrode active material layer paste was printed on the above-mentioned solid electrolyte layer sheet using screen printing with a thickness of 5μm. Next, the printed positive electrode active material layer paste was dried at 80°C for 5 minutes. Then, on the dried positive electrode active material layer paste, the positive electrode collector layer paste was printed with a thickness of 5μm using screen printing. Next, the printed positive electrode collector layer paste was dried at 80°C for 5 minutes. Then, on the dried positive electrode collector layer paste, the positive electrode active material layer paste was printed again with a thickness of 5μm using screen printing and dried. Then, the PET film was peeled off. In this way, a positive electrode unit was obtained in which the positive electrode active material layer / positive electrode collector layer / positive electrode active material layer were stacked in sequence on the main surface of the solid electrolyte layer.
[0120] Next, the negative electrode paste was printed on the main surface of the solid electrolyte layer to a thickness of 10 μm. Next, the printed negative electrode paste was dried at 80° C. for 5 minutes. A negative electrode unit was manufactured by this procedure.
[0121] Next, a solid electrolyte unit was made by overlapping 5 solid electrolyte layer sheets. The laminate was made by alternately stacking 50 electrode units (25 positive electrode units and 25 negative electrode units) in a manner of clamping the solid electrolyte unit. At this time, the units were stacked staggered so that the odd-numbered electrode units only extended from one end face, and the even-numbered electrode units only extended from the end face on the opposite side. Six solid electrolyte layer sheets were stacked on the stacked unit. Then, they were formed and cut by hot pressing to make a laminated chip. Then, the laminated chips were fired simultaneously to obtain a laminate. During the simultaneous firing, the temperature was raised to a firing temperature of 800°C at a heating rate of 200°C / hour in an atmospheric atmosphere, maintained at this temperature for 2 hours, and naturally cooled after firing.
[0122] By a known method, terminal electrodes 5 and 6 are arranged on the sintered stack (sintered body) to produce an all-solid-state battery. Then, the cross-section of the produced all-solid-state battery is confirmed by a scanning electron microscope, and the film thickness of the oxide having a composition different from the Li transition metal oxide is measured. The film thickness of the oxide having a composition different from the Li transition metal oxide of Example 1 is 0.01 μm. In addition, the volume ratio of each layer does not change between the paste state before sintering and the state after sintering. Ag exists in the form of Ag monomer and in the form of being contained as a contained element of AgPd alloy.
[0123] Then, the cycle characteristics of the all-solid-state battery made under the same conditions were measured. The cycle characteristics were measured by clamping the first external terminal and the second external terminal with a spring probe in a relative manner and repeatedly performing charge and discharge tests at a temperature of 60°C. The measurement conditions were set as follows: the current during charging and discharging was 100μA, and the termination voltage during charging and discharging was 3.9V and 0V, respectively. The capacity at the tenth discharge when the discharge capacity was stable was taken as the initial discharge capacity. In addition, the cycle characteristics were obtained by dividing the discharge capacity of the 500th cycle by the discharge capacity of the tenth cycle.
[0124] "Examples 2 to 5"
[0125] In Examples 2 to 5, the film thickness of the oxide having a composition different from the Li transition metal oxide was changed, which is different from Example 1. The film thickness of the oxide having a composition different from the Li transition metal oxide was controlled by increasing the amount of AgCoO2 added during the mechanochemical reaction.
[0126] The film thickness of the oxide having a composition different from the Li transition metal oxide in Example 2 was 0.1 μm. The film thickness of the oxide having a composition different from the Li transition metal oxide in Example 3 was 0.5 μm. The film thickness of the oxide having a composition different from the Li transition metal oxide in Example 4 was 1.0 μm. The film thickness of the oxide having a composition different from the Li transition metal oxide in Example 5 was 2.0 μm. The cycle characteristics were obtained in the same manner as in Example 1 under other conditions.
[0127] "Example 6"
[0128] In Example 6, the positive electrode active material contained in the positive electrode current collector layer paste and the positive electrode active material layer paste was changed from LiCoO2 to LiMn2O4, which is different from Example 1. The cycle characteristics were obtained in the same manner as in Example 1 under other conditions.
[0129] "Example 7"
[0130] In Example 7, the positive electrode active material contained in the positive electrode current collector layer paste and the positive electrode active material layer paste was changed from LiCoO2 to LiMn2O4, and AgCoO2, which would become an oxide having a composition different from that of the Li transition metal oxide, was changed to AgMn2O4, which are different from Example 1. The cycle characteristics were obtained in the same manner as in Example 1 under other conditions.
[0131] "Example 8"
[0132] In Example 8, the point which changed AgCoO2 which becomes the oxide which has a composition different from Li transition metal oxide into AgMn2O4 is different from Example 1. The cycle characteristics were obtained similarly to Example 1 under other conditions.
[0133] "Example 9" to "Example 10"
[0134] In Example 9, the film thickness of the oxide having a composition different from the Li transition metal oxide was changed, which is different from Example 1. The film thickness of the oxide having a composition different from the Li transition metal oxide was controlled by increasing the amount of AgCoO2 added during the mechanochemical reaction.
[0135] The film thickness of the oxide having a composition different from the Li transition metal oxide in Example 9 was 0.009 μm. The film thickness of the oxide having a composition different from the Li transition metal oxide in Example 10 was 2.1 μm.
[0136] "Example 11" to "Example 14"
[0137] In Example 11, the contact rate between the positive electrode active material and the positive electrode collector is changed, which is different from Example 1. The contact rate between the positive electrode active material and the positive electrode collector is adjusted by changing the time for the mechanochemical reaction. Specifically, by shortening the time for the mechanochemical reaction, the amount of AgCoO2 coating formed by contacting the surface of the AgPd powder is reduced, thereby increasing the contact rate between the positive electrode active material and the positive electrode collector not covered by the AgCoO2 coating. On the contrary, by extending the time for the mechanochemical reaction, the amount of AgCoO2 coating formed by contacting the surface of the AgPd powder is increased, thereby reducing the contact rate between the positive electrode active material and the positive electrode collector not covered by the AgCoO2 coating.
[0138] The film thickness of the oxide having a composition different from the Li transition metal oxide in Example 9 was 0.009 μm. The film thickness of the oxide having a composition different from the Li transition metal oxide in Example 10 was 2.1 μm.
[0139] "Example 15" to "Example 18"
[0140] In Example 15, the positive electrode current collector was changed from AgPd to Ag, which is different from Example 1. In Examples 16 to 18, the film thickness of the oxide having a composition different from the Li transition metal oxide was changed, which is different from Example 15. The film thickness of the oxide having a composition different from the Li transition metal oxide was controlled by increasing the amount of AgCoO2 added during the mechanochemical reaction.
[0141] The film thickness of the oxide having a composition different from the Li transition metal oxide in Example 15 was 0.01 μm. The film thickness of the oxide having a composition different from the Li transition metal oxide in Example 16 was 0.1 μm. The film thickness of the oxide having a composition different from the Li transition metal oxide in Example 17 was 0.5 μm. The film thickness of the oxide having a composition different from the Li transition metal oxide in Example 18 was 1.0 μm. The cycle characteristics were obtained in the same manner as in Example 1 under other conditions.
[0142] "Comparative Example 1"
[0143] Comparative Example 1 does not form an oxide having a composition different from that of the Li transition metal oxide, and the positive active material contained in the positive collector layer paste and the positive active material layer paste is changed from LiCoO2 to LiMn2O4, which is different from Example 1. The cycle characteristics were obtained under the same conditions as in Example 1.
[0144] "Comparative Example 2"
[0145] Comparative Example 2 is different from Example 1 in that an oxide having a composition different from that of the Li transition metal oxide is not formed. The cycle characteristics were determined in the same manner as in Example 1 under other conditions.
[0146] "Comparative Example 3"
[0147] Comparative Example 3 is different from Example 15 in that an oxide having a composition different from that of the Li transition metal oxide is not formed. The cycle characteristics were determined in the same manner as in Example 15 under other conditions.
[0148] The results of Examples 1 to 18 and Comparative Examples 1 to 3 are summarized in Table 1 below.
[0149] [Table 1]
[0150]
[0151] Examples 1 to 18 were superior in cycle characteristics to Comparative Examples 1 to 3. This is considered to be because the oxide (oxide) having a composition different from that of the Li transition metal oxide suppressed oxidation of Ag during charge and discharge.
[0152] Industrial Applicability
[0153] Compared with the existing technology, the cycle characteristics of all-solid-state batteries can be improved.
Claims
1. An all-solid-state battery, in, A sintered body is provided, the sintered body having: a positive electrode, a negative electrode, and a solid electrolyte layer between the positive electrode and the negative electrode, The positive electrode comprises: a compound containing Ag, a Li-containing transition metal oxide, and an oxide having a composition different from that of the Li-containing transition metal oxide. The oxide comprises Ag, The compound containing Ag and at least a portion of the Li transition metal oxide are present inside the positive electrode via the oxide.
2. The all-solid-state battery according to claim 1, in, The oxide includes a transition metal element constituting the Li transition metal oxide.
3. The all-solid-state battery according to claim 1, in, A minimum thickness of the oxide between the compound including Ag and at least a portion of the Li transition metal oxide is 0.01 μm or more and 2.0 μm or less.
4. The all-solid-state battery according to claim 1, in, A contact ratio between the Li transition metal oxide and the compound containing Ag in a cross section of the positive electrode is 0.1% or more and 10% or less.
5. The all-solid-state battery according to claim 1, in, The compound containing Ag is any one selected from Ag or Ag / Pd.
6. The all-solid-state battery according to claim 1, in, The positive electrode comprises: a first layer; and a second layer located on at least one main surface of the first layer. The first layer includes the compound including Ag, the Li-containing transition metal oxide, and the oxide.
7. The all-solid-state battery according to claim 1, in, The second layer includes the Li transition metal oxide.
8. The all-solid-state battery according to claim 1, in, The first layer and the second layer include Li transition metal oxides having the same composition.
9. The all-solid-state battery according to claim 1, in, The positive electrode includes lithium cobalt oxide.