Adhesive film for metal terminal and method for manufacturing same, metal terminal equipped with adhesive film for metal terminal, electric storage device using said adhesive film for metal terminal, kit comprising adhesive film for metal terminal and exterior material for electric storage device, and method for manufacturing electric storage device

By placing a homopolymer polybutylene terephthalate film between the metal terminal and the outer packaging material of the electrical storage device, the problem of insufficient sealing and water vapor barrier properties of the metal terminal in high temperature environments is solved, and high efficiency is achieved. The metal terminal seal and water vapor isolation improve battery performance.

CN118749159APending Publication Date: 2024-10-08DAI NIPPON PRINTING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380018037.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-01-19
Filing Date
2023-01-19
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

In the existing technology, the adhesive film between the metal terminal and the heat-weldable resin layer has insufficient sealing and water vapor barrier properties in high-temperature environments, especially during the high-speed charging and discharging process of all-solid-state batteries, resulting in reduced sealing properties. and performance degradation.

Method used

Homopolymer polybutylene terephthalate film is used as the material for the adhesive film for metal terminals. By placing this film between the metal terminals and the outer packaging material for the electrical storage device, high sealing properties are ensured in high-temperature environments. and excellent water vapor barrier properties.

Benefits of technology

It achieves high sealing performance and excellent water vapor barrier properties for metal terminals in high temperature environments, extending the service life of power storage devices and improving their performance stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004954095760000111
    Figure BDA0004954095760000111
  • Figure BDA0004954095760000231
    Figure BDA0004954095760000231
  • Figure HDA0004954095780000011
    Figure HDA0004954095780000011
Patent Text Reader

Abstract

This adhesive film for a metal terminal is provided between a metal terminal that is electrically connected to an electrode of an electricity storage device element and an exterior material for an electricity storage device that seals the electricity storage device element. The adhesive film for a metal terminal is characterized in that at least one surface of the adhesive film for a metal terminal is formed from a homopolymerized polybutylene terephthalate layer comprising a homopolymerized polybutylene terephthalate film.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an adhesive film for metal terminals and a method for producing the same, a metal terminal with the adhesive film for metal terminals, a storage device using the adhesive film for metal terminals, a kit including the adhesive film for metal terminals and an outer packaging material for the storage device, and a method for producing the storage device. Background Art

[0002] In the past, various types of storage devices have been developed, but in all storage devices, in order to seal storage device components such as electrodes and electrolytes, storage device outer packaging materials have become indispensable components. In the past, as storage device outer packaging materials, metal storage device outer packaging materials were mostly used. However, in recent years, with the high performance of electric vehicles, hybrid electric vehicles, personal computers, cameras, portable phones, etc., various shapes are required for storage devices, and thinning and lightening are required. However, in the metal storage device outer packaging materials that were mostly used in the past, there are disadvantages that it is difficult to follow the diversification of shapes, and lightening also has a limit.

[0003] Therefore, in recent years, a laminated sheet in which a base material layer / adhesive layer / barrier layer / thermo-fusible resin layer are sequentially laminated has been proposed as an outer packaging material for a storage device that is easy to process into various shapes and can achieve thinning and lightening, etc. When such a film-shaped outer packaging material for a storage device is used, the outer packaging material for a storage device can be used to seal the storage device element by heat-sealing the peripheral edge of the outer packaging material for a storage device while the innermost heat-fusible resin layers of the outer packaging material for a storage device are facing each other.

[0004] The metal terminal extends from the heat-sealed portion of the outer packaging material for the storage device, and the storage device element sealed by the outer packaging material for the storage device is electrically connected to the outside through the metal terminal electrically connected to the electrode of the storage device element. That is, the portion of the heat-sealed portion of the outer packaging material for the storage device where the metal terminal exists is heat-sealed in a state where the metal terminal is sandwiched by the heat-fusible resin layer. The metal terminal and the heat-fusible resin layer are composed of different materials from each other, so the adhesion is easily reduced at the interface between the metal terminal and the heat-fusible resin layer.

[0005] Therefore, an adhesive film may be disposed between the metal terminal and the heat-adhesive resin layer for the purpose of improving the adhesion between them. As such an adhesive film, for example, an adhesive film described in Patent Document 1 can be cited.

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent Application Publication No. 2015-79638 Summary of the invention

[0009] Technical problem to be solved by the invention

[0010] The adhesive film disposed between the metal terminal and the heat-fusible resin layer is heat-sealed between the outer packaging material for the power storage device and the metal terminal at high temperature and high pressure.

[0011] In addition, as a storage device using an adhesive film, a storage device containing an electrolyte such as a lithium ion battery is generally used, but an all-solid-state battery in which the electrolyte is a solid electrolyte is also known. Since the electrolyte of the all-solid-state battery is solid, it can be charged at a high speed at a high temperature compared to a storage device using an electrolyte, and it is assumed that it can be used in an environment with a higher temperature than a lithium ion battery.

[0012] In order to improve the ion conductivity of the solid electrolyte, etc., during the manufacturing process of the all-solid-state battery, the metal terminal is installed on the battery cell under high temperature and high pressure (for example, temperature 120℃~150℃, pressure about 100MPa), so the metal terminal part may reach high temperature. Moreover, during the rapid charge and discharge process, the temperature of the metal terminal sometimes reaches about 150℃ due to resistance heating. Therefore, when the above-mentioned adhesive film is applied to the all-solid-state battery, high sealing performance of the metal terminal is particularly required in a high temperature environment.

[0013] Furthermore, when moisture penetrates from the outside of the power storage device into the inside, the performance of the power storage device deteriorates. Therefore, the adhesive film disposed between the metal terminal and the heat-fusible resin layer is also required to have high water vapor barrier properties.

[0014] Under such circumstances, the main purpose of the present invention is to provide an adhesive film for metal terminals having both high sealing properties for metal terminals and excellent water vapor barrier properties in a high temperature environment. In addition, the present invention also aims to provide a metal terminal with an adhesive film for metal terminals using the adhesive film for metal terminals, a storage device using the adhesive film for metal terminals, and a method for manufacturing the storage device.

[0015] Means for solving technical problems

[0016] The inventors of the present invention have conducted intensive research to solve the above technical problems. As a result, it was found that when homopolymerized polybutylene terephthalate is used in an adhesive film for metal terminals, high sealing properties and excellent water vapor barrier properties can be exerted on metal terminals in a high temperature environment. The present invention was completed through further repeated research based on such insights.

[0017] That is, the present invention provides the following technical solutions.

[0018] An adhesive film for metal terminals, which is arranged between a metal terminal electrically connected to an electrode of a storage device element and an outer packaging material for the storage device that seals the storage device element, and the adhesive film for metal terminals is characterized in that: a surface of at least one side of the adhesive film for metal terminals is formed by a homopolymer polybutylene terephthalate layer containing a homopolymer polybutylene terephthalate film.

[0019] Effects of the Invention

[0020] The present invention can provide an adhesive film for metal terminals having both high sealing properties for metal terminals and excellent water vapor barrier properties in a high temperature environment. Furthermore, the present invention can also provide a metal terminal with the adhesive film for metal terminals using the adhesive film for metal terminals, a storage device using the adhesive film for metal terminals, and a method for manufacturing the storage device. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 This is a schematic plan view of the power storage device of the present invention.

[0022] Figure 2 for Figure 1 Schematic cross-sectional view along line A-A'.

[0023] Figure 3 for Figure 1 Schematic cross-sectional view of line BB'.

[0024] Figure 4 This is a schematic cross-sectional view of the adhesive film for a metal terminal of the present invention.

[0025] Figure 5 This is a schematic cross-sectional view of the adhesive film for a metal terminal of the present invention.

[0026] Figure 6 This is a schematic cross-sectional view of the adhesive film for a metal terminal of the present invention.

[0027] Figure 7 This is a schematic cross-sectional view of the adhesive film for a metal terminal of the present invention.

[0028] Figure 8 This is a schematic cross-sectional view of the outer packaging material for an electric storage device according to the present invention. DETAILED DESCRIPTION

[0029] The adhesive film for metal terminals of the present invention is provided between a metal terminal electrically connected to an electrode of an electric storage device element and an outer packaging material for an electric storage device that seals the electric storage device element, and the adhesive film for metal terminals is characterized in that at least one surface of the adhesive film for metal terminals is formed by a homopolymer polybutylene terephthalate layer including a homopolymer polybutylene terephthalate film. The adhesive film for metal terminals of the present invention has such a structure, and has both high sealing properties for metal terminals and excellent water vapor barrier properties in a high temperature environment.

[0030] In addition, the electric storage device of the present invention includes: an electric storage device element including at least a positive electrode, a negative electrode and an electrolyte; an outer packaging material for an electric storage device that seals the electric storage device element; and metal terminals electrically connected to the positive electrode and the negative electrode, respectively, and extending to the outside of the outer packaging material for the electric storage device, wherein the electric storage device is characterized in that an adhesive film for metal terminals of the present invention is provided between the metal terminals and the outer packaging material for the electric storage device. The adhesive film for metal terminals of the present invention, the metal terminal with the adhesive film for metal terminals, the electric storage device using the adhesive film for metal terminals, and the method for manufacturing the electric storage device are described in detail below.

[0031] In addition, in this specification, regarding numerical ranges, numerical ranges expressed with "~" mean "above... below". For example, the expression 2 to 15 mm means "above 2 mm and below 15 mm". In the numerical ranges recorded in gradients in this specification, the upper limit value or lower limit value recorded in a certain numerical range can be replaced by the upper limit value or lower limit value of the numerical range recorded in other gradients. In addition, upper limits and upper limits, upper limits and lower limits, or lower limits and lower limits recorded separately can also be combined as numerical ranges. In addition, in the numerical ranges recorded in this specification, the upper limit value or lower limit value recorded in a certain numerical range can also be replaced by the values ​​shown in the embodiments.

[0032] In addition, as a method for confirming the MD of the adhesive film for metal terminals, XRD, Raman spectroscopy, polarized IR, etc. can be used. In addition, for example, the heat shrinkage rate of the adhesive film for metal terminals after being placed in an environment of 200° C. for 2 minutes can be measured, and the direction with a larger shrinkage rate can be determined as MD.

[0033] 1. Adhesive film for metal terminals

[0034] The adhesive film for metal terminals of the present invention is provided between a metal terminal electrically connected to an electrode of an electric storage device element and an outer packaging material for an electric storage device that seals the electric storage device element. Figure 1 to Figure 3As shown, the adhesive film 1 for metal terminals of the present invention is provided between a metal terminal 2 electrically connected to an electrode of an electric storage device element 4 and an outer packaging material 3 for an electric storage device that seals the electric storage device element 4. In addition, the metal terminal 2 extends to the outside of the outer packaging material 3 for an electric storage device, and is sandwiched by the outer packaging material 3 for an electric storage device via the adhesive film 1 for metal terminals at the peripheral edge portion 3a of the outer packaging material 3 for an electric storage device that is heat-sealed.

[0035] As described above, it is assumed that a high temperature of about 150°C may be reached during the heating and pressing process in the manufacturing process of the all-solid-state battery, during rapid charging, etc., and a durable temperature of about 150°C is required. Therefore, a heat-fusible resin layer having a melting point of 150°C or higher is required in the outer packaging material 3 for the storage device. The heating temperature when heat-sealing the sides formed by the outer packaging materials for the storage device is usually in the range of about 160 to 250°C, and the pressure is usually in the range of about 0.5 to 2.0 MPa. A flat metal sealing rod (heat sealing rod) is used for sealing. For the side where the metal terminal and the outer packaging material for the storage device are heat-sealed via the adhesive film for the metal terminal, the temperature is also usually in the range of about 160 to 250°C, and the pressure is usually in the range of about 0.5 to 2.0 MPa. A metallic sealing head with a step is used, and a step for adjusting the difference caused by the thickness of the metal terminal and / or the adhesive film for the metal terminal is provided at the corresponding part of the sealing head as needed. In addition, it is preferred that the adhesive film is bonded to a predetermined position of the metal terminal in advance. For example, in the case of bonding by heat fusion, heating and pressurization are usually performed multiple times, as in the temporary bonding process and the formal bonding process on the metal terminal. The temporary bonding process is a process of temporarily fixing the adhesive film for the metal terminal on the metal terminal and removing bubbles, and the formal bonding process is a process of bonding the adhesive film for the metal terminal to the metal terminal by heating / pressurizing once or multiple times under a higher temperature condition than the temporary bonding process. The temporary bonding process of temporarily bonding the adhesive film for the metal terminal to the metal terminal is carried out under the conditions of, for example, a temperature of about 160 to 230°C, a pressure of about 0.1 to 0.5 MPa, a time of about 10 to 20 seconds, and a metal sealing head coated with a heat-resistant rubber having a hardness of about 20 to 50 and a thickness of about 2 to 5 mm, for about 1 to 2 times. The formal bonding process is for the purpose of thermally fusing the adhesive film for the metal terminal to the metal terminal, and is carried out under the conditions of, for example, a temperature of about 180 to 250°C, a pressure of about 0.2 to 1.0 MPa, a time of about 10 to 30 seconds, and a metal sealing head coated with a heat-resistant rubber having a hardness of about 20 to 50 and a thickness of about 2 to 5 mm, for about 1 to 2 times. In addition, by providing a step for adjusting the difference caused by the thickness of the metal terminal and / or the adhesive film for the metal terminal at the corresponding part of the sealing head as needed, efficient welding can be performed. In addition, when the storage device to which the adhesive film for metal terminals of the present invention is applied is an all-solid battery, a particularly high temperature / pressure is applied to the adhesive film for metal terminals. The method for mounting the adhesive film for metal terminals illustrated here is an example and is not limited to a specific method. For example, the pressing time can be appropriately adjusted according to the thickness of the adhesive film for metal terminals.

[0036] The adhesive film 1 for metal terminals of the present invention is provided to improve the adhesion between the metal terminal 2 and the outer packaging material 3 for the storage device. By improving the adhesion between the metal terminal 2 and the outer packaging material 3 for the storage device, the sealing of the storage device element 4 can be improved. As described above, when the storage device element 4 is heat-sealed, the storage device element is sealed in such a way that the metal terminal 2 electrically connected to the electrode of the storage device element 4 extends to the outside of the outer packaging material 3 for the storage device. At this time, the adhesive film 1 for metal terminals and the heat-fusible resin layer 35 located in the innermost layer of the outer packaging material 3 for the storage device are both required to have a durability of about 150°C, but when they are formed of different materials, the sealing of the storage device element is easily reduced at the interface with the heat-fusible resin layer 35.

[0037] The surface of at least one side of the adhesive film 1 for metal terminals of the present invention is formed by a homopolymer polybutylene terephthalate layer. The homopolymer polybutylene terephthalate layer is a resin layer formed by a homopolymer polybutylene terephthalate film (hereinafter sometimes also referred to as a homopolymer PBT layer). That is, the adhesive film 1 for metal terminals of the present invention includes at least one homopolymer PBT layer, and among the surfaces of the adhesive film 1 for metal terminals, at least one side of the surface is formed by a homopolymer PBT layer. To the extent that the effects of the present invention are achieved, the adhesive film 1 for metal terminals of the present invention can be as follows Figure 4 Single layer shown, can also be Figures 5 to 7 Multiple layers shown.

[0038] When the adhesive film 1 for metal terminals of the present invention is a single layer, the adhesive film 1 for metal terminals is formed by a homopolymer PBT layer, and the surface on the metal terminal side and the surface of the outer packaging material for the storage device are formed by the homopolymer PBT layer. In this case, the resin forming the surface on the outer packaging material side of the adhesive film 1 for metal terminals and the resin forming the surface on the metal terminal side are the same resin (i.e., the resin constituting the homopolymer PBT layer). In addition, the resin forming the surface on the outer packaging material side of the adhesive film 1 for metal terminals and the resin forming the surface on the metal terminal side are the same, which means that the components in these resins are, for example, 80% or more of the same, 90% or more of the same, 95% or more of the same, or 100% of the same.

[0039] When the adhesive film 1 for metal terminals of the present invention is multi-layered, at least one layer may be formed of a homopolymer PBT layer. Figure 5As shown, when the adhesive film 1 for metal terminals of the present invention has a double-layer structure, the adhesive film 1 for metal terminals is a laminate of a first resin layer 12a and a second resin layer 12b, and at least one of the two layers is formed by a homopolymer PBT layer. When the adhesive film 1 for metal terminals of the present invention has multiple layers, it is also preferred that the resin forming the surface on the side of the outer packaging material for the storage device and the resin forming the surface on the side of the metal terminal are the same resin.

[0040] For example, Figure 6 As shown, when the adhesive film 1 for metal terminals of the present invention has a three-layer structure, the adhesive film 1 for metal terminals is a laminated body in which a first resin layer 12a, an intermediate layer 11, and a second resin layer 12b are sequentially laminated. Among the three layers, at least one of the first resin layer 12a and the second resin layer 12b is formed by a homopolymer PBT layer. The intermediate layer 11 preferably has excellent heat resistance. When insulation is preferred, the melting point of the intermediate layer 11 is preferably above 250°C, and more preferably 250 to 330°C.

[0041] The adhesive film 1 for metal terminals of the present invention may also be composed of four or more layers. Figure 7 As shown, the adhesion promoter layer 13 may be stacked between the first resin layer 12a and the intermediate layer 11, and between the second resin layer 12b and the intermediate layer 11, respectively.

[0042] In addition, in the present invention, the first resin layer 12a is arranged on the metal terminal side, and the second resin layer 12b is arranged on the storage device outer packaging material 3 side. The surface of the metal terminal side of the adhesive film 1 for metal terminals of the present invention has heat-melting properties that can be heat-melted with metal (metal constituting the metal terminal), and the surface of the storage device outer packaging material side has heat-melting properties that can be heat-melted with the heat-melting resin layer described later. The surface on the metal terminal side is preferably formed by a homopolymer PBT layer. In addition, it is also preferred that the surface on the storage device outer packaging material side is formed by a homopolymer PBT layer.

[0043] The melting point of at least one homopolymer PBT layer in the adhesive film for metal terminal 1 of the present invention is, for example, 220 to 230° C. The melting point of the homopolymer PBT layer is an endothermic peak measured by differential scanning calorimetry (DSC).

[0044] The homo-PBT layer is a resin layer composed of a homo-polybutylene terephthalate film, and the resin contained in the homo-PBT layer is substantially (for example, 99% by mass or more, and further 100% by mass) only polybutylene terephthalate. That is, the homo-PBT layer does not substantially contain a resin different from homo-polybutylene terephthalate, but is formed of a homo-polybutylene terephthalate film. For example, the homo-PBT layer is a layer composed of a homo-polybutylene terephthalate film that does not contain an elastomer and copolymerized polybutylene terephthalate.

[0045] Furthermore, the homopolybutylene terephthalate may or may not be acid-modified. When the homopolybutylene terephthalate is an acid-modified homopolybutylene terephthalate, the acid-modification of the homopolybutylene terephthalate may be performed using an acid component such as maleic anhydride or acrylic acid.

[0046] From the viewpoint of better exerting the effect of the present invention, the thickness of the homopolymer PBT layer is preferably about 20 μm or more, more preferably about 30 μm or more, and further preferably about 50 μm or more. In addition, from the same viewpoint, the thickness is preferably about 300 μm or less, more preferably about 200 μm or less, and further preferably about 100 μm or less. In addition, the preferred range of the thickness is about 20 to 300 μm, about 20 to 200 μm, about 20 to 100 μm, about 30 to 300 μm, about 30 to 200 μm, about 30 to 100 μm, about 50 to 300 μm, about 50 to 200 μm, and about 50 to 100 μm.

[0047] The adhesive film 1 for metal terminals of the present invention may contain at least one other resin layer different from the homopolymer PBT layer. However, from the viewpoint of ensuring the high sealing property and excellent water vapor barrier property of the adhesive film 1 for metal terminals of the present invention to the metal terminals under high temperature environment, the other resin layer preferably has a melting point of 150°C or more and a low water vapor permeability coefficient. The melting point of the other resin layer is preferably about 150 to 330°C, more preferably about 180 to 280°C. The melting point of the other resin layer is an endothermic peak measured by a differential scanning calorimeter (DSC).

[0048] In addition, when two or more other resin layers are included, the compositions of the other resin layers may be the same or different. In the case of two or more homopolymer PBT layers, the compositions of the homopolymer PBT layers may be the same or different.

[0049] As for the thickness of other resin layers, from the viewpoint of better exerting the effect of the present invention, it is preferably about 20 μm or more, more preferably about 50 μm or more, and further preferably about 80 μm or more. In addition, from the same viewpoint, the thickness is preferably about 300 μm or less, more preferably about 200 μm or less, and further preferably about 100 μm or less. In addition, as a preferred range of the thickness, it is about 20 to 300 μm, about 20 to 200 μm, about 20 to 100 μm, about 50 to 300 μm, about 50 to 200 μm, about 50 to 100 μm, about 80 to 300 μm, about 80 to 200 μm, and about 80 to 100 μm.

[0050] When the adhesive film for metal terminal 1 of the present invention includes other resin layers, examples of the laminated structure of the adhesive film for metal terminal 1 include: Figure 5 The first resin layer 12a is a homopolymer PBT layer, and the second resin layer 12b is a laminate of other resin layers; Figure 5 The second resin layer 12b is a homopolymer PBT layer, and the first resin layer 12a is a laminate of other resin layers; Figure 6 or Figure 7 The first resin layer 12a is a homopolymer PBT layer, and the intermediate layer 11 and the second resin layer 12b are laminated bodies of other resin layers; Figure 6 or Figure 7 The second resin layer 12b is a homopolymer PBT layer, and the intermediate layer 11 and the first resin layer 12a are laminated bodies of other resin layers; Figure 6 or Figure 7 The first resin layer 12a and the second resin layer 12b are homopolymer PBT layers, and the intermediate layer 11 is a laminate of other resin layers; Figure 6 or Figure 7 The first resin layer 12a and the intermediate layer 11 are homopolymer PBT layers, and the second resin layer 12b is a laminate of other resin layers; Figure 6 or Figure 7 The second resin layer 12b and the intermediate layer 11 are homopolymer PBT layers, and the first resin layer 12a is a laminate of other resin layers.

[0051] As resins constituting other resin layers, there are no particular restrictions as long as the purpose of the adhesive film for metal terminals of the present invention is not impaired, and examples thereof include polyolefin resins, polyamide resins, polyester resins, epoxy resins, acryl resins, fluororesins, silicone resins, phenolic resins, polyetherimides, polyimides, polycarbonates, and mixtures and copolymers thereof, etc., and polyethylene terephthalate, polyethylene naphthalate, polyphenylene sulfide, polyetheretherketone, polyimide, etc. are particularly preferred because of their excellent heat resistance. In the case where the adhesive film for metal terminals 1 of the present invention is multilayered, specific examples of the laminated structure include a laminated structure in which homopolymer PBT layer / fluororesin layer / homopolymer PBT layer are laminated in sequence, a laminated structure in which homopolymer PBT layer / polyethylene naphthalate layer / homopolymer PBT layer are laminated in sequence, and the like.

[0052] The homopolymer PBT layer and other resin layers may each contain additives such as fillers as needed. By containing fillers, the fillers act as spacers, so that short circuits between the metal terminal 2 and the barrier layer 33 of the outer packaging material 3 for the storage device can be effectively suppressed. As the particle size of the filler, a range of about 0.1 to 35 μm, preferably about 5.0 to 30 μm, and more preferably about 10 to 25 μm can be cited. In addition, as the content of the filler, about 5 to 30 parts by mass, more preferably about 10 to 20 parts by mass, can be cited relative to 100 parts by mass of the resin components forming the homopolymer PBT layer and other resin layers.

[0053] As fillers, any of inorganic or organic fillers can be used. As inorganic fillers, for example, carbon (carbon, graphite), silica, aluminum oxide, barium titanate, iron oxide, silicon carbide, zirconium oxide, zirconium silicate, magnesium oxide, titanium dioxide, calcium aluminate, calcium hydroxide, aluminum hydroxide, magnesium hydroxide, calcium carbonate, etc. can be cited. In addition, as organic fillers, for example, fluororesins, phenolic resins, urea-formaldehyde resins, epoxy resins, acryl resins, benzoguanamine formaldehyde condensates, melamine formaldehyde condensates, polymethyl methacrylate cross-linked products, polyethylene cross-linked products, etc. can be cited. From the viewpoint of shape stability, rigidity and resistance to corrosion of contents, preferably aluminum oxide, silica, fluororesins, acryl resins, benzoguanamine formaldehyde condensates, among which, particularly spherical aluminum oxide and silica are more preferred. As a mixing method for mixing the filler into the resin components forming the homopolymer PBT layer and other resin layers, a method of preliminarily melt-blending the two using a Banbury mixer or the like to prepare a masterbatch of a specified mixing ratio, or a method of directly mixing with the resin components can be adopted.

[0054] In addition, as required, the homopolymer PBT layer and other resin layers may contain pigments respectively. As the pigment, various inorganic pigments can be used. As a specific example of the pigment, the carbon (carbon, graphite) illustrated in the above filler can be cited as a preferred example. Carbon (carbon, graphite) is a material commonly used inside the storage device, and there is no risk of dissolving into the electrolyte. In addition, the coloring effect is high, and a sufficient coloring effect can be obtained with an amount added that does not damage the adhesion, and it will not melt due to heat, and the apparent melt viscosity of the added resin can be increased. In addition, it is possible to prevent the pressurized portion from becoming thinner during thermal bonding (heat sealing), thereby imparting excellent sealing properties between the outer packaging material for the storage device and the metal terminal.

[0055] When a pigment is added to the homopolymer PBT layer and other resin layers, the amount of pigment added can be about 0.05 to 0.3 parts by mass, preferably about 0.1 to 0.2 parts by mass, relative to 100 parts by mass of the resin components forming the homopolymer PBT layer and other resin layers, for example, when carbon black having a particle size of about 0.03 μm is used. By adding a pigment to the homopolymer PBT layer or other resin layers, the presence or absence of the adhesive film 1 for metal terminals can be detected by a sensor or visually.

[0056] The adhesion promoter layer 13 is a layer provided as needed for the purpose of firmly bonding the intermediate layer 11 to the first resin layer 12a and the intermediate layer 11 to the second resin layer 12b (see Figure 7 The adhesion promoter layer 13 may be provided on only one side between the intermediate layer 11 and the first resin layer 12a and the second resin layer 12b, or may be provided on both sides.

[0057] The adhesion promoter layer 13 can be formed using known adhesion promoters such as isocyanate, polyethyleneimine, polyester, polyurethane, and polybutadiene. From the viewpoint of obtaining a strong adhesion strength, it is preferably formed by an isocyanate adhesion promoter. As an isocyanate adhesion promoter, an isocyanate adhesion promoter containing an isocyanate component selected from a triisocyanate monomer and polymeric MDI has excellent lamination strength and less reduction in lamination strength at high temperatures. It is particularly preferably formed by an adhesion promoter containing triphenylmethane-4,4',4"-triisocyanate as a triisocyanate monomer and polymethylene polyphenyl polyisocyanate (NCO content of about 30%, viscosity 200 to 700 mPa·s) as a polymeric MDI. In addition, it is also preferably formed by a two-component curing type adhesion promoter with tri(p-isocyanatophenyl)thiophosphate as a triisocyanate monomer and a polyethyleneimine system as the main agent and polycarbodiimide as a crosslinking agent.

[0058] The adhesion promoter layer 13 can be formed by coating and drying by a known coating method such as a bar coating method, a roll coating method, or a gravure coating method. The coating amount of the adhesion promoter is 20 to 100 mg / m2 in the case of an adhesion promoter composed of triisocyanate. 2 About 40 to 60 mg / m 2 In the case of an adhesion promoter composed of polymeric MDI, it is 40 to 150 mg / m 2 About 60 to 100 mg / m 2 In the case of a two-component curing adhesion promoter with polyethylene imine as the main agent and polycarbodiimide as the crosslinking agent, it is 5 to 50 mg / m 2 About 10 to 30 mg / m 2In addition, the triisocyanate monomer is a monomer having three isocyanate groups in one molecule, and the polymerized MDI is a mixture of MDI and MDI oligomers obtained by polymerization of MDI, which is represented by the following formula.

[0059]

[0060] The water vapor permeability coefficient of the adhesive film 1 for metal terminals of the present invention is preferably 5.0 g·mm / m 2 · days or less, more preferably 3.0g·mm / m 2 ·day or less, more preferably 1.0g·mm / m 2 ·day or less, more preferably 0.5g·mm / m 2 The water vapor transmission coefficient is measured as follows.

[0061] <Measurement of water vapor permeability coefficient (Evaluation of water vapor barrier properties)>

[0062] Prepare two pieces of 100×100mm aluminum foil (thickness 50μm), and sinter them with a treatment agent composed of three components: acrylic resin, chromium (III) nitrate compound and phosphoric acid in such a way that the treatment layer becomes about 100nm thick to produce aluminum foil. Prepare two pieces of adhesive film for metal terminals with a size of 100×100mm. Sandwich the two pieces of adhesive film for metal terminals between the two pieces of aluminum foil, and heat seal the three sides with a width of 3mm. On the side that has not been heat-sealed, put 0.3g of silica gel (particle size Φ2~5mm) between the two pieces of adhesive film for metal terminals. Heat seal the side that has not been heat-sealed (before) with a width of 3mm, seal the silica gel, and store it at 65℃ and 90%RH for one month. Calculate the water vapor permeability coefficient (g·mm / m 2 ·sky).

[0063] From the viewpoint of better exerting the effect of the present invention, the total thickness of the adhesive film 1 for metal terminals of the present invention is preferably about 50 μm or more, more preferably about 80 μm or more, and further preferably about 100 μm or more. In addition, from the same viewpoint, the thickness is preferably about 500 μm or less, more preferably about 300 μm or less, and further preferably about 200 μm or less. In addition, as a preferred range of the thickness, it is about 50 to 500 μm, about 50 to 300 μm, about 50 to 200 μm, about 80 to 500 μm, about 80 to 300 μm, about 80 to 200 μm, about 100 to 500 μm, about 100 to 300 μm, and about 100 to 200 μm.

[0064] The adhesive film 1 for metal terminals of the present invention can be formed into a film shape by a known method such as an extrusion lamination method, a T-die method, an inflation method, and a heat lamination method using a resin (homopolymer polybutylene terephthalate) forming a homopolymer PBT layer. In the case of forming multiple layers, each layer can be stacked using a co-extrusion type extruder. In the case of stacking the intermediate layer 11, the first resin layer 12a, and the second resin layer 12b via the adhesion promoter layer 13, the adhesion promoter constituting the adhesion promoter layer 13 can be applied on the intermediate layer 11 and dried using the above method, and the first resin layer 12a and the second resin layer 12b can be stacked on the adhesion promoter layer 13, respectively.

[0065] There is no particular limitation on the method of providing the adhesive film 1 for metal terminals between the metal terminals 2 and the outer packaging material 3 for power storage devices. For example, Figure 1 to Figure 3 As shown, at the portion where the metal terminal 2 is clamped by the outer packaging material 3 for the storage device, the adhesive film 1 for the metal terminal is arranged on the metal terminal 2. In addition, although the illustration is omitted, at the portion where the metal terminal 2 is clamped by the outer packaging material 3 for the storage device, the adhesive film 1 for the metal terminal can be arranged on both sides of the metal terminal 2 in a manner that the adhesive film 1 for the metal terminal spans over the two metal terminals 2.

[0066] [Metal terminal 2]

[0067] The adhesive film 1 for metal terminals of the present invention is used in a manner of being arranged between a metal terminal 2 and an outer packaging material 3 for an electrical storage device. The metal terminal 2 (connector) is a conductive component electrically connected to an electrode (positive electrode or negative electrode) of an electrical storage device element 4, and is composed of a metal material. There is no particular limitation on the metal material constituting the metal terminal 2, and examples thereof include aluminum, nickel, and copper. For example, the metal terminal 2 connected to the positive electrode of a lithium-ion electrical storage device is usually composed of aluminum or the like, and the metal terminal 2 connected to the negative electrode of a lithium-ion electrical storage device is usually made of copper, nickel, or the like. From the viewpoint of low resistance and prevention of surface degradation, it is made of copper plated with nickel, a cladding material of nickel and copper, or the like.

[0068] From the viewpoint of improving electrolyte resistance, it is preferred to perform chemical conversion treatment on the surface of the metal terminal 2. For example, when the metal terminal 2 is made of aluminum, as a specific example of chemical conversion treatment, a known method of forming a corrosion-resistant film such as phosphate, chromate, fluoride, triazine thiol compound, acrylate, etc. is cited. Among the methods for forming a corrosion-resistant film, it is preferred to use a phosphate chromate treatment such as a composition consisting of three components of a phenolic resin, a chromium (III) fluoride compound, and phosphoric acid, and a composition consisting of three components of an acrylic resin, a chromium (III) nitrate compound, and phosphoric acid.

[0069] The size of the metal terminal 2 can be appropriately set according to the size of the power storage device used. As the thickness of the metal terminal 2, it is preferably about 50 to 1000 μm, and more preferably about 70 to 800 μm. In addition, as the length of the metal terminal 2, it is preferably about 1 to 200 mm, and more preferably about 3 to 150 mm. In addition, as the width of the metal terminal 2, it is preferably about 1 to 200 mm, and more preferably about 3 to 150 mm.

[0070] [Outer packaging materials for power storage devices 3]

[0071] As the outer packaging material 3 for a storage device, there can be mentioned an outer packaging material for a storage device having a laminate structure composed of a laminate, wherein the laminate has at least a base layer 31, a barrier layer 33, and a heat-fusible resin layer 35 in this order. Figure 8 In the figure, as an example of the cross-sectional structure of the outer packaging material 3 for a storage device, a substrate layer 31, an adhesive layer 32 provided as required, a barrier layer 33, an adhesive layer 34 provided as required, and a heat-fusible resin layer 35 are stacked in this order. In the outer packaging material 3 for a storage device, the substrate layer 31 becomes the outer layer side, and the heat-fusible resin layer 35 becomes the innermost layer. When assembling the storage device, the heat-fusible resin layers 35 located at the periphery of the storage device element 4 are brought into surface contact with each other and heat-fused to seal the storage device element 4. In addition, although Figure 1 to Figure 3 The figure shows the storage device 10 when the embossed storage device outer packaging material 3 is formed by embossing, etc., but the storage device outer packaging material 3 may also be a soft-pack type without forming. In addition, the soft-pack type includes three-side seal, four-side seal, pillow type, etc., and any type is acceptable.

[0072] There is no particular limitation on the thickness of the laminate constituting the outer packaging material 3 for a storage device. However, from the viewpoint of reducing costs and improving energy density, the upper limit is preferably about 180 μm or less, about 160 μm or less, about 155 μm or less, about 140 μm or less, about 130 μm or less, or about 120 μm or less. From the viewpoint of maintaining the function of the outer packaging material 3 for a storage device to protect the storage device element 4, the lower limit is preferably about 35 μm or more, about 45 μm or more, about 60 μm or more, or about 80 μm or more. The preferred range is, for example, about 35 to 180 μm, about 35 to 160 μm, about 35 to 15 ...60 μm, about 35 to 155 μm, about 35 to 160 μm, about 35 to 160 μm, about 35 to 160 μm, about 35 to 160 μm, about 35 to 160 μm, about 35 to 160 μm, about 35 to 160 μm, about 35 About 5 to 140 μm, about 35 to 130 μm, about 35 to 120 μm, about 45 to 180 μm, about 45 to 160 μm, about 45 to 155 μm, about 45 to 140 μm, about 45 to 130 μm, about 45 to 120 μm, about 60 to 180 μm, about 60 to 160 μm, about 60 to 155 μm, about 60 to 140 μm, about 60 to 130 μm, about 60 to 120 μm, about 80 to 180 μm, about 80 to 160 μm, about 80 to 155 μm, about 80 to 140 μm, about 80 to 130 μm, about 80 to 120 μm.

[0073] In addition, the adhesive film 1 for metal terminals of the present invention can be applied to the outer packaging material for all-solid batteries. The thickness of the laminate constituting the outer packaging material for all-solid batteries is not particularly limited, but from the viewpoints of reducing costs and improving energy density, preferably, it is about 10000 μm or less, about 8000 μm or less, or about 5000 μm or less; from the viewpoint of maintaining the function of protecting battery elements of the outer packaging material for all-solid batteries, preferably, it is about 100 μm or more, about 100 μm or less, about 200 μm or less, about 300 μm or less, about 500 μm or less. About 150μm or more, about 200μm or more; preferred ranges include, for example, about 100-10000μm, about 100-8000μm, about 100-5000μm, about 150-10000μm, about 150-8000μm, about 150-5000μm, about 200-10000μm, about 200-8000μm, about 200-5000μm, and particularly preferably about 100-500μm.

[0074] (Base material layer 31)

[0075] In the electricity storage device packaging material 3 , the base material layer 31 is a layer that functions as a base material of the electricity storage device packaging material and is a layer formed on the outermost layer side.

[0076] The material forming the substrate layer 31 is not particularly limited as long as it has insulating properties. Examples of the material forming the substrate layer 31 include polyester, polyamide, epoxy resin, acryl resin, fluororesin, polyurethane, silicone resin, phenolic resin, polyetherimide, polyimide, and mixtures and copolymers thereof. Polyesters such as polyethylene terephthalate have advantages such as excellent resistance to electrolyte and are not prone to whitening due to the adhesion of electrolyte, and are suitable for use as a material for forming the substrate layer 31. In addition, polyamide films have excellent stretchability and can prevent the occurrence of whitening caused by resin cracking of the substrate layer 31 during the molding process, and are suitable for use as a material for forming the substrate layer 31.

[0077] The substrate layer 31 may be formed of a uniaxially or biaxially stretched resin film, or may be formed of an unstretched resin film. Among them, a uniaxially or biaxially stretched resin film, especially a biaxially stretched resin film, has improved heat resistance due to crystal orientation and is therefore suitable for use as the substrate layer 31 .

[0078] Among them, nylon and polyester are preferred as the resin film forming the substrate layer 31, and biaxially stretched nylon and biaxially stretched polyester are more preferred. In addition, the service life temperature of the all-solid-state battery is above 150°C, so it is often sealed at a high temperature of above 200°C, and biaxially stretched polyester is the most suitable.

[0079] In order to improve the pinhole resistance and the insulation when the packaging body of the power storage device is made, the substrate layer 31 can also be formed by stacking resin films of different materials. Specifically, a multilayer structure of a polyester film and a nylon film, a multilayer structure of a biaxially stretched polyester and a biaxially stretched nylon, etc. can be cited. In the case where the substrate layer 31 forms a multilayer structure, each resin film can be bonded via an adhesive, or can be directly stacked without an adhesive. For example, in the case of bonding without an adhesive, methods such as coextrusion, sandwich lamination, and hot lamination in a hot melt state can be cited. For the above-mentioned high-temperature sealing, it is preferred that at least the outermost layer is a biaxially stretched polyester.

[0080] In addition, in order to improve the formability, the base layer 31 may also be set to have a low friction coefficient. When the friction coefficient of the base layer 31 is lowered, the friction coefficient of the surface thereof may be, for example, but not particularly limited to, 1.0 or less. In order to lower the friction coefficient of the base layer 31, for example, matte treatment, formation of a lubricant film layer, and a combination thereof may be used.

[0081] The thickness of the base material layer 31 is, for example, about 10 to 50 μm, preferably about 15 to 30 μm.

[0082] (Adhesive layer 32)

[0083] In the power storage device packaging material 3 , the adhesive layer 32 is a layer disposed on the base layer 31 as necessary to impart adhesion to the base layer 31 . That is, the adhesive layer 32 is provided between the base layer 31 and the barrier layer 33 .

[0084] The adhesive layer 32 is formed of an adhesive capable of bonding the substrate layer 31 to the barrier layer 33. The adhesive used in forming the adhesive layer 32 may be a two-component curing adhesive or a one-component curing adhesive. In addition, the bonding mechanism of the adhesive used in forming the adhesive layer 32 is not particularly limited, and may be any of a chemical reaction type, a solvent volatilization type, a hot melt type, a hot pressing type, and the like.

[0085] As the resin component of the adhesive that can be used to form the adhesive layer 32, preferably, from the viewpoint of excellent performance in terms of ductility, durability under high humidity conditions, yellowing inhibition, thermal degradation inhibition during heat sealing, etc., and being able to inhibit the reduction in the lamination strength between the substrate layer 31 and the barrier layer 33 and effectively inhibit the occurrence of delamination, polyurethane-based two-component curing adhesives, polyamides, polyesters or blended resins of these with modified polyolefins can be cited.

[0086] In addition, the adhesive layer 32 may be formed of multiple layers of different adhesive components. When the adhesive layer 32 is formed of multiple layers of different adhesive components, from the viewpoint of improving the lamination strength between the substrate layer 31 and the barrier layer 33, it is preferred to select a resin having excellent adhesion to the substrate layer 31 as the adhesive component disposed on the substrate layer 31 side, and it is preferred to select an adhesive component having excellent adhesion to the barrier layer 33 as the adhesive component disposed on the barrier layer 33 side. When the adhesive layer 32 is formed of multiple layers of different adhesive components, specifically, as the adhesive component disposed on the barrier layer 33 side, preferably, acid-modified polyolefins, metal-modified polyolefins, mixed resins of polyesters and acid-modified polyolefins, resins containing copolyesters, etc. can be cited.

[0087] The thickness of the adhesive layer 32 is, for example, about 2 to 50 μm, preferably about 3 to 25 μm.

[0088] (Barrier layer 33)

[0089] In the outer packaging material 3 for the storage device, the barrier layer 33 is a layer that has the function of preventing water vapor, oxygen, light, etc. from invading the interior of the storage device in addition to the function of improving the strength of the outer packaging material for the storage device. The barrier layer 33 is preferably a metal layer, that is, a layer formed of metal. As the metal constituting the barrier layer 33, specifically, aluminum, stainless steel, titanium, etc. can be cited, and aluminum can be preferably cited. The barrier layer 33 can be formed, for example, by metal foil, metal vapor-deposited film, inorganic oxide vapor-deposited film, carbon-containing inorganic oxide vapor-deposited film, a film provided with these vapor-deposited films, etc., preferably formed by metal foil, and more preferably formed by aluminum foil. From the viewpoint of preventing the barrier layer 33 from developing wrinkles, pinholes, etc. during the process of manufacturing the outer packaging material for the power storage device, the barrier layer is more preferably formed of a soft aluminum foil such as annealed aluminum (JIS H4160: 1994A8021H-O, JIS H4160: 1994A8079H-O, JIS H4000: 2014A8021P-O, JIS H4000: 2014A8079P-O).

[0090] From the viewpoint of making the packaging material for a power storage device thin and less likely to form pinholes even when molded, the thickness of the barrier layer 33 is preferably about 10 to 200 μm, more preferably about 20 to 100 μm, about 20 to 45 μm, about 45 to 65 μm, or about 65 to 85 μm.

[0091] In order to stabilize adhesion, prevent dissolution and corrosion, etc., it is preferred that at least one surface, more preferably both surfaces, of the barrier layer 33 be subjected to chemical conversion treatment. The chemical conversion treatment is a treatment for forming a corrosion-resistant film on the surface of the barrier layer.

[0092] (Adhesive layer 34)

[0093] In the power storage device packaging material 3 , the adhesive layer 34 is a layer provided between the barrier layer 33 and the thermally-adhesive resin layer 35 as necessary in order to firmly adhere to the thermally-adhesive resin layer 35 .

[0094] The adhesive layer 34 is formed of an adhesive capable of bonding the barrier layer 33 and the heat-fusible resin layer 35. The composition of the adhesive used to form the adhesive layer may be, but is not particularly limited to, an adhesive composed of a polyester polyol compound and an alicyclic isocyanate compound.

[0095] The thickness of the adhesive layer 34 is, for example, about 1 to 40 μm, preferably about 2 to 30 μm.

[0096] (Thermal Fusible Resin Layer 35)

[0097] In the electricity storage device packaging material 3 , the heat-fusible resin layer 35 corresponds to the innermost layer and is a layer for sealing the electricity storage device element by heat-fusion bonding the heat-fusible resin layers to each other when assembling the electricity storage device.

[0098] The resin component used for the heat-fusible resin layer 35 is not particularly limited as long as it can be heat-fusible, and examples thereof include polyolefins and cyclic polyolefins commonly used in packaging materials for power storage devices.

[0099] Specifically, the polyolefins include polyethylenes such as low-density polyethylene, medium-density polyethylene, high-density polyethylene, and linear low-density polyethylene; crystalline or amorphous polypropylenes such as homopolypropylene, block copolymers of polypropylene (e.g., block copolymers of propylene and ethylene), and random copolymers of polypropylene (e.g., random copolymers of propylene and ethylene); terpolymers of ethylene-butene-propylene, etc. Among these polyolefins, polyethylene and polypropylene are preferred.

[0100] The above-mentioned cyclopolyolefin is a copolymer of an olefin and a cyclic monomer. As the olefin of the structural monomer of the above-mentioned cyclopolyolefin, for example, ethylene, propylene, 4-methyl-1-pentene, butadiene, isoprene, etc. can be cited. In addition, as the cyclic monomer of the above-mentioned cyclopolyolefin structural monomer, for example, cyclic olefins such as norbornene can be cited, and specifically, cyclic dienes such as cyclopentadiene, dicyclopentadiene, cyclohexadiene, and norbornadiene can be cited. Among these polyolefins, cyclic olefins can be cited preferably, and norbornene can be cited more preferably. As a structural monomer, styrene can also be cited.

[0101] Among these resin components, crystalline or amorphous polyolefins, cyclic polyolefins, and polymer blends thereof are preferred, and more preferred are polyethylene, polypropylene, copolymers of ethylene and norbornene, and polymer blends of two or more thereof.

[0102] The heat-adhesive resin layer 35 may be formed of a single resin component or a blended polymer of two or more resin components. In addition, the heat-adhesive resin layer 35 may be formed of only one layer or two or more layers of the same or different resin components.

[0103] The thickness of the heat-adhesive resin layer 35 may be, but is not particularly limited to, about 2 to 2000 μm, preferably about 5 to 1000 μm, and more preferably about 10 to 500 μm.

[0104] In addition, the melting point of the heat-fusible resin layer 35 of the all-solid-state battery outer packaging material, which is particularly suitable for the all-solid-state battery outer packaging material as the adhesive film 1 for metal terminals of the present invention, is preferably 150-250°C, more preferably 180-270°C, further preferably 200-270°C, and further preferably 200-250°C.

[0105] In addition, as the resin contained in the heat-fusible resin layer 35 of the outer packaging material for all-solid batteries, polyolefins such as polypropylene and polyethylene, acid-modified polyolefins such as acid-modified polypropylene and acid-modified polyethylene, polybutylene terephthalate, etc. can be cited. Among them, polybutylene terephthalate has excellent heat resistance, so in the outer packaging material for all-solid batteries, the heat-fusible resin layer 35 is preferably formed of a polybutylene terephthalate film. In addition, by forming the heat-fusible resin layer 35 from a polybutylene terephthalate film, its adhesion with the homopolymer PBT layer of the adhesive film for metal terminals of the present invention is also very good. The polybutylene terephthalate film forming the heat-fusible resin layer 35 may be formed by laminating a previously prepared polybutylene terephthalate film with the adhesive layer 34 or by forming a film by melt-extruding a resin forming the polybutylene terephthalate film and laminating it with the adhesive layer 34 at the same time.

[0106] The polybutylene terephthalate film may be a stretched polybutylene terephthalate film or an unstretched polybutylene terephthalate film, and is preferably an unstretched polybutylene terephthalate film.

[0107] The polybutylene terephthalate film preferably comprises homopolybutylene terephthalate.

[0108] The heat-fusible resin layer 35 may be formed by only one layer, or may be formed by two or more layers of the same or different resins. In the case where the heat-fusible resin layer 35 is formed by two or more layers, it is preferred that at least one layer is formed by a polybutylene terephthalate film, and the polybutylene terephthalate film is the innermost layer of the outer packaging material for the all-solid-state battery. In addition, the layer bonded to the adhesive layer 34 is preferably a polybutylene terephthalate film. In the case where the heat-fusible resin layer 35 is formed by two or more layers, the layer not formed by the polybutylene terephthalate film may be a layer formed by a polyolefin such as polypropylene, polyethylene, or an acid-modified polyolefin such as acid-modified polypropylene, acid-modified polyethylene, etc. However, since polyolefins and acid-modified polyolefins have lower durability under high temperature environments than polybutylene terephthalate, the heat-fusible resin layer 35 is preferably made of only a polybutylene terephthalate film.

[0109] 2. Power storage devices

[0110] The electric storage device 10 of the present invention comprises: an electric storage device element 4 including at least a positive electrode, a negative electrode and an electrolyte; an outer packaging material 3 for an electric storage device that seals the electric storage device element 4; and metal terminals 2 that are electrically connected to the positive electrode and the negative electrode, respectively, and extend to the outside of the outer packaging material 3 for the electric storage device. The electric storage device 10 of the present invention is characterized in that the adhesive film 1 for metal terminals of the present invention is provided between the metal terminal 2 and the outer packaging material 3 for the electric storage device. That is, the electric storage device 10 of the present invention can be manufactured by a method having a step of providing the adhesive film 1 for metal terminals of the present invention between the metal terminal 2 and the outer packaging material 3 for the electric storage device.

[0111] Specifically, the present invention provides an electrical storage device 10 using the electrical storage device outer packaging material 3 by placing the adhesive film 1 for metal terminals of the present invention between the metal terminals 2 and the heat-fusible resin layer 35 in a state where the metal terminals 2 connected to the positive electrode and the negative electrode are respectively extended to the outside, and covering the electrical storage device element 4 having at least a positive electrode, a negative electrode and an electrolyte with the electrical storage device outer packaging material 3 in such a manner that a flange portion (a region where the heat-fusible resin layers 35 are in contact with each other is the peripheral portion 3a of the electrical storage device outer packaging material 3) of the electrical storage device outer packaging material 3 can be formed at the periphery of the electrical storage device element 4, and heat-sealing the heat-fusible resin layers 35 at the flange portion to each other. In addition, when the electrical storage device outer packaging material 3 is used to accommodate the electrical storage device element 4, the electrical storage device outer packaging material 3 is used in such a manner that the heat-fusible resin layer 35 of the electrical storage device outer packaging material 3 becomes the inner side (the surface in contact with the electrical storage device element 4).

[0112] The outer packaging material for the storage device of the present invention can be suitable for storage devices such as batteries (including capacitors (condenser), capacitors (capacitor) and the like). In addition, the outer packaging material for the storage device of the present invention can be used for any of primary batteries and secondary batteries, preferably secondary batteries. The type of secondary battery to which the outer packaging material for the storage device of the present invention is applicable is not particularly limited, and for example, lithium ion batteries, lithium ion polymer batteries, all-solid batteries, semi-solid batteries, quasi-solid batteries, polymer batteries, all-resin batteries, lead batteries, nickel / hydrogen batteries, nickel / cadmium batteries, nickel / iron batteries, nickel / zinc batteries, silver oxide / zinc batteries, metal-air batteries, multivalent cation batteries, capacitors (condenser), capacitors (capacitor), etc. Among these secondary batteries, lithium ion batteries and lithium ion polymer batteries can be cited as applicable objects of the outer packaging material for the storage device of the present invention.

[0113] Among them, the adhesive film 1 for a metal terminal of the present invention can be preferably applied to an all-solid-state battery.

[0114] Example

[0115] The present invention is described in detail below with reference to the following examples and comparative examples, but the present invention is not limited to the technical solutions of the examples.

[0116] <Preparation of adhesive film for metal terminals>

[0117] Example 1

[0118] A homopolybutylene terephthalate film (melting point 223° C., thickness 100 μm) formed of homopolybutylene terephthalate (homo-PBT) was prepared, and a single layer of the homopolybutylene terephthalate film was used as an adhesive film for a metal terminal.

[0119] Comparative Example 1

[0120] A polybutylene terephthalate film (melting point 215° C., thickness 100 μm) containing 7.0 mass % of an elastomer (block copolymer of polybutylene terephthalate and polyether) was prepared, and the elastomer-containing polybutylene terephthalate film was used as a single layer as an adhesive film for metal terminals.

[0121] Comparative Examples 2 and 3

[0122] A copolymerized polybutylene terephthalate film (thickness 100 μm) formed of copolymerized polybutylene terephthalate (copolymerized PBT) was prepared, and a single layer of the copolymerized polybutylene terephthalate film was used as an adhesive film for metal terminals. Copolymerized polybutylene terephthalate is a polybutylene terephthalate structure in which terephthalic acid and 1,4-butanediol as main components constitute two structural units, and dodecanedioic acid as a minor component is block polymerized relative to the polybutylene terephthalate structure. Dodecanedioic acid is a structure introduced into the resin by copolymerization with the above-mentioned 1,4-butanediol. The content of dodecanedioic acid in the copolymerized polybutylene terephthalate used in Comparative Example 2 is 12% by mass, and the melting point is 205°C. The content of dodecanedioic acid in the copolymerized polybutylene terephthalate used in Comparative Example 3 is 5% by mass, and the melting point is 216°C.

[0123] Comparative Example 4

[0124] A homopolyethylene terephthalate film (melting point 252° C., thickness 100 μm) formed of homopolyethylene terephthalate (homoPET) was prepared, and a single layer of the homopolyethylene terephthalate film was used as an adhesive film for a metal terminal.

[0125] Comparative Example 5

[0126] A maleic anhydride-modified homopolypropylene film (melting point 162° C., thickness 100 μm) was prepared, and this single-layer film was used as an adhesive film for metal terminals.

[0127] Comparative Example 6

[0128] A copolymerized polyethylene terephthalate film (melting point 215° C., thickness 100 μm) formed of copolymerized polyethylene terephthalate (co-PET) was prepared and used as an adhesive film for metal terminals. Co-polyethylene terephthalate contains about 10% by mass of neopentyl glycol as a diol component.

[0129] (Preparation of outer packaging materials for all-solid-state batteries)

[0130] First, an outer packaging material for a fully solid-state battery is prepared. As a substrate layer, a substrate layer obtained by corona treatment of the bonding surface side of a polyethylene terephthalate film (25 μm) is prepared. In addition, as a barrier layer, an aluminum alloy foil (JIS H4160: 1994A8021H-O, 40 μm thick) is prepared. Next, a heat-fusible resin layer (50 μm) is prepared using the same resin as the resin constituting the film used in Example 1 and Comparative Examples 1 to 6. As described later, in the following <Measurement of sealing strength at 150°C (heat resistance evaluation)>, an outer packaging material for a fully solid-state battery using a heat-fusible resin layer that is the same as the adhesive film for metal terminals in Example 1 and Comparative Examples 1 to 6 is evaluated. However, the resin of Comparative Example 5 uses an unmodified resin (homopolymer PP, melting point 162°C) that is the same resin as the film. The substrate layer and the barrier layer were bonded together using a two-component curing polyurethane adhesive (polyol compound and aromatic isocyanate compound) by dry lamination to form a laminate of substrate layer (25 μm) / adhesive layer (3 μm) / barrier layer (40 μm). Next, the barrier layer side of the obtained laminate was bonded to a heat-fusible resin layer by dry lamination using a resin composition of a polyester polyol compound (a product to which a hydrolysis inhibitor was added) and an alicyclic isocyanate compound (containing isophorone isocyanate), and an adhesive layer (3 μm) / heat-fusible resin layer (50 μm) was laminated on the barrier layer. Next, the obtained laminate was subjected to an aging treatment at 80°C for 72 hours, and by heating, an outer packaging material having a laminate having a substrate layer (polyethylene terephthalate film (25 μm)) / adhesive layer (cured product of a two-component curing polyurethane adhesive (3 μm)) / barrier layer (aluminum alloy foil (40 μm)) / adhesive layer (cured product of a resin composition containing a polyester polyol compound and an alicyclic isocyanate compound (3 μm)) / thermo-fusible resin layer (50 μm) laminated in this order was obtained.

[0131] (Preparation of Metal Terminal with Adhesive Film for Metal Terminal)

[0132] A 400μm thick aluminum alloy foil×TD45mm×MD60mm thick aluminum terminal was used as a metal terminal, and it was sintered with a treatment agent composed of three components of acrylic resin, chromium (III) nitrate compound and phosphoric acid so that the treatment layer had a thickness of about 100nm to produce a surface-treated metal terminal. Next, two pieces of adhesive films for metal terminals cut into a size of TD10mm×MD55mm were prepared, and the two pieces of adhesive films for metal terminals were arranged on both sides at a position 10mm away from the end of the surface-treated metal terminal in a manner consistent with the center in the width direction of the surface-treated metal terminal, and heat-sealed at 240°C×0.25MPa (surface pressure applied to the silicone rubber)×16 seconds using a flat plate press with a metal pressure head of 3.0mm thick and 40 hardness silicone rubber attached to the top and bottom, to produce a metal terminal with an adhesive film for metal terminal in which adhesive film for metal terminal / metal terminal / adhesive film for metal terminal were stacked in sequence. At this time, the MD of the metal terminal and the MD of the adhesive film for the metal terminal are arranged to be perpendicular to each other. However, for Comparative Example 5 in which a maleic anhydride-modified homopolypropylene film is used as the metal terminal side resin, the metal terminal with the adhesive film for the metal terminal is prepared under the conditions of 190°C×0.25MPa (surface pressure applied to the silicone rubber)×16 seconds.

[0133] <Measurement of seal strength at 150°C (Evaluation of the sealability of metal terminals in high temperature environments)>

[0134] Prepare an outer packaging material for a solid-state battery and cut it into a size of TD60mm×MD150mm. As described above, the heat-fusible resin layer of the outer packaging material for a solid-state battery is formed by the same resin as the adhesive film for the metal terminal of Example 1 and Comparative Examples 1 to 6, respectively (only Comparative Example 5 is unmodified homopolymer PP). Next, the heat-fusible resin layers of the outer packaging material for a solid-state battery (outer packaging material) are folded in half in the length direction (MD) with each other as the inner side (TD60mm×MD75mm), and the metal terminal with the adhesive film for the metal terminal prepared as described above (45mm wide×60mm long) is sandwiched between the two layers. At this time, the metal terminal with the adhesive film for the metal terminal is clamped in such a way that the MD of the adhesive film for the metal terminal and the MD of the outer packaging material are perpendicular to each other and abut against the inner part of the fold of the outer packaging material. In this state, heat sealing was performed using a sealing device with upper and lower metal pressure heads of 7 mm width at the sealing temperatures described in Table 1 (190°C×1.0MPa×5 seconds for Comparative Example 5, 240°C×1.0MPa×12 seconds for Example 1, Comparative Examples 1 to 3, and 6, and 280°C×1.0MPa×12 seconds for Comparative Example 4). The width of 7 mm is the MD direction of the outer packaging material. In addition, these heat sealing conditions are temperature conditions applicable to the resin used for the adhesive film for metal terminals. The heat-sealed portion of the resulting laminate has a structure in which outer packaging material / adhesive film for metal terminals / metal terminals / adhesive film for metal terminals / outer packaging material are stacked in sequence. Next, the laminate is cut in a direction perpendicular to the width of 7 mm to obtain a sample with a width of 15 mm. At this time, sampling is performed from the center of the laminate. The width of 15 mm is the TD direction of the outer packaging material. Then, the outer packaging material and the metal terminal on one side of the sample were clamped with a chuck, and the outer packaging material and the metal terminal were stretched in a 180° direction at a speed of 300 mm / min at 150°C in a tensile tester with a constant temperature bath, and the sealing strength at 150°C was measured. The heat resistance was evaluated according to the following standards. The results are shown in Table 1.

[0135] A+: Sealing strength is 50N / 15mm or more.

[0136] A: The sealing strength is 40 N / 15 mm or more and less than 50 N / 15 mm.

[0137] B: The sealing strength is 30 N / 15 mm or more and less than 40 N / 15 mm.

[0138] C: Sealing strength is less than 30N / 15mm.

[0139] <Evaluation of damage on the surface of the base material layer of the outer packaging material in the measurement of the seal strength at 150°C>

[0140] When the sample was sealed in the above <Measurement of Seal Strength at 150° C. (Evaluation of Heat Resistance)>, the surface of the base material layer of the outer packaging material was visually observed and the damage on the surface of the base material layer was evaluated according to the following criteria.

[0141] A: There is no change in the appearance of the surface of the base material layer.

[0142] B: The surface of the base material layer is slightly whitened.

[0143] C: The surface of the base material layer melts, and irregularities are generated on the surface.

[0144] <Measurement of water vapor permeability coefficient (Evaluation of water vapor barrier properties)>

[0145] Two pieces of 100×100 mm aluminum foil (100 μm thick) were prepared and sintered with a treatment agent composed of three components: acrylic resin, chromium (III) nitrate compound, and phosphoric acid so that the treatment layer had a thickness of about 100 nm to produce aluminum foil. Two pieces of adhesive films for metal terminals of the embodiment and comparative example with a size of 100×100 mm were prepared. Two pieces of adhesive films for metal terminals were sandwiched between two pieces of aluminum foil and heat-sealed on three sides with a width of 3 mm. Heat-sealing was performed at the sealing temperatures listed in Table 1 (190°C×1.0 MPa×5 seconds for comparative example 5, 240°C×1.0 MPa×12 seconds for embodiment 1, comparative examples 1 to 3, and 6, and 280°C×1.0 MPa×12 seconds for comparative example 4). On the side that was not heat-sealed, 0.3 g of silica gel (particle size Φ2 to 5 mm) was placed between the two pieces of adhesive films for metal terminals. The side that was not heat-sealed before was heat-sealed with a width of 3 mm under the above three conditions, and then the three sides were heat-sealed and silicone-sealed. After being stored for one month under the conditions of 65°C and 90% RH, the water vapor transmission coefficient (g·mm / m) was calculated from the weight increase and the thickness of the adhesive film for the metal terminal of the sealed part (the remaining thickness after sealing). 2 ·day). Based on the water vapor permeability coefficient, the water vapor barrier property was evaluated according to the following criteria. The results are shown in Table 1.

[0146] A: Water vapor permeability coefficient is 5g·mm / m 2 · Below the day.

[0147] B: Water vapor transmission coefficient greater than 5g·mm / m 2 ·day and 10g·mm / m 2 · Below the day.

[0148] C: Water vapor permeability coefficient greater than 10g·mm / m 2 ·sky.

[0149] [Table 1]

[0150]

[0151] The adhesive film for metal terminals of Example 1 has a surface formed of a homopolybutylene terephthalate layer including a homopolybutylene terephthalate film, and has both high sealing properties to metal terminals and excellent water vapor barrier properties in a high temperature environment.

[0152] As described above, the present invention provides the following technical solutions.

[0153] Item 1. An adhesive film for metal terminals, which is arranged between a metal terminal electrically connected to an electrode of a storage device element and an outer packaging material for the storage device that seals the storage device element, and the adhesive film for metal terminals is characterized in that: a surface of at least one side of the adhesive film for metal terminals is formed by a homopolymer polybutylene terephthalate layer containing a homopolymer polybutylene terephthalate film.

[0154] Item 2. The adhesive film for a metal terminal according to Item 1, wherein the resin forming the surface on the side of the power storage device outer packaging material and the resin forming the surface on the side of the metal terminal are the same resin.

[0155] Item 3. The adhesive film for a metal terminal according to Item 1 or Item 2, wherein the adhesive film for a metal terminal is a single layer.

[0156] Item 4. The adhesive film for a metal terminal according to any one of Items 1 to 3, wherein the total thickness of the adhesive film for a metal terminal is 50 μm or more and 500 μm or less.

[0157] Item 5. The adhesive film for a metal terminal according to any one of Items 1 to 4, wherein the electricity storage device packaging material is an all-solid-state battery packaging material.

[0158] Item 6. A metal terminal with an adhesive film for a metal terminal, the metal terminal being formed by attaching the adhesive film for a metal terminal according to any one of Items 1 to 5 to a metal terminal.

[0159] Item 7. A storage device, comprising: the storage device element comprising at least a positive electrode, a negative electrode and an electrolyte; the storage device outer packaging material that seals the storage device element; and the metal terminals that are electrically connected to the positive electrode and the negative electrode, respectively, and extend to the outside of the storage device outer packaging material, wherein the storage device is characterized in that an adhesive film for metal terminals described in any one of items 1 to 5 is provided between the metal terminals and the storage device outer packaging material.

[0160] Item 8. A method for manufacturing an energy storage device, the energy storage device comprising: the energy storage device element comprising at least a positive electrode, a negative electrode and an electrolyte; the energy storage device outer packaging material for sealing the energy storage device element; and the metal terminals electrically connected to the positive electrode and the negative electrode, respectively, and extending to the outside of the energy storage device outer packaging material, the method for manufacturing the energy storage device being characterized in that it comprises: providing an adhesive film for the metal terminal described in any one of items 1 to 5 between the metal terminal and the energy storage device outer packaging material, and sealing the energy storage device element with the energy storage device outer packaging material.

[0161] Item 9. A kit comprising an adhesive film for metal terminals and an outer packaging material for a storage device, wherein the kit is characterized in that: a surface of at least one side of the adhesive film for metal terminals is formed by a homopolymer polybutylene terephthalate layer comprising a homopolymer polybutylene terephthalate film, and when in use, it is used in the following manner: the adhesive film for metal terminals is arranged between a metal terminal electrically connected to an electrode of a storage device element and an outer packaging material for the storage device that seals the storage device element, and the storage device is sealed with the outer packaging material for the storage device.

[0162] Item 10. A method for manufacturing an adhesive film for metal terminals, wherein the adhesive film for metal terminals is arranged between a metal terminal electrically connected to an electrode of a storage device element and an outer packaging material for the storage device that seals the storage device element, and the method for manufacturing the adhesive film for metal terminals is characterized in that: a surface of at least one side of the adhesive film for metal terminals is formed by a homopolymer polybutylene terephthalate layer comprising a homopolymer polybutylene terephthalate film.

[0163] Description of Reference Numerals

[0164] 1: Adhesive film for metal terminal; 2: Metal terminal; 3: Outer packaging material for storage device; 3a: Peripheral portion of outer packaging material for storage device; 4: Storage device element; 10: Storage device; 11: Intermediate layer; 12a: First resin layer; 12b: Second resin layer; 13: Adhesion promoter layer; 31: Base material layer; 32: Adhesive layer; 33: Barrier layer; 34: Adhesive layer; 35: Thermally fusible resin layer.

Claims

1. An adhesive film for metal terminals, provided between a metal terminal electrically connected to an electrode of an electric storage device element and an outer packaging material for an electric storage device that seals the electric storage device element, wherein the adhesive film for metal terminals is characterized by: At least one surface of the adhesive film for metal terminal is formed of a homopolybutylene terephthalate layer including a homopolybutylene terephthalate film.

2. The adhesive film for metal terminals according to claim 1, Features: The resin forming the surface on the side of the outer packaging material for the power storage device and the resin forming the surface on the side of the metal terminal are the same resin.

3. The adhesive film for metal terminal according to claim 1 or 2, Features: The adhesive film for metal terminals is a single layer.

4. The adhesive film for metal terminal according to claim 1 or 2, Features: The adhesive film for a metal terminal has a total thickness of 50 μm to 500 μm.

5. The adhesive film for metal terminal according to claim 1 or 2, Features: The outer packaging material for an electricity storage device is an outer packaging material for an all-solid-state battery.

6. A metal terminal with an adhesive film for a metal terminal, Features: The adhesive film for a metal terminal according to claim 1 or 2 is attached to a metal terminal.

7. An electric storage device, include: The electricity storage device element includes at least a positive electrode, a negative electrode and an electrolyte; the electricity storage device outer packaging material that seals the electricity storage device element; and the metal terminals electrically connected to the positive electrode and the negative electrode, respectively, and extending to the outside of the outer packaging material for the power storage device, wherein the power storage device is characterized in that: The adhesive film for metal terminal according to claim 1 or 2 is provided between the metal terminal and the outer packaging material for the electric storage device.

8. A method for manufacturing an electric storage device, wherein the electric storage device include: The electricity storage device element comprises at least a positive electrode, a negative electrode and an electrolyte; The outer packaging material for the power storage device for sealing the power storage device element; and the metal terminals electrically connected to the positive electrode and the negative electrode, respectively, and extending to the outside of the outer packaging material for the power storage device, wherein the method for manufacturing the power storage device is characterized by comprising: A step of providing the adhesive film for metal terminal according to claim 1 or 2 between the metal terminal and the outer packaging material for the electric storage device, and sealing the electric storage device element with the outer packaging material for the electric storage device.

9. A kit comprising an adhesive film for a metal terminal and an outer packaging material for an electric storage device, wherein: At least one surface of the adhesive film for metal terminal is formed of a homopolymer polybutylene terephthalate layer including a homopolymer polybutylene terephthalate film. When used, the adhesive film for metal terminals is disposed between metal terminals electrically connected to electrodes of an electric storage device element and an electric storage device packaging material sealing the electric storage device element, and the electric storage device is sealed with the electric storage device packaging material.

10. A method for producing an adhesive film for a metal terminal, the adhesive film for a metal terminal being provided between a metal terminal electrically connected to an electrode of an electric storage device element and an outer packaging material for an electric storage device that seals the electric storage device element, the method for producing an adhesive film for a metal terminal being characterized by: At least one surface of the adhesive film for metal terminal is formed of a homopolybutylene terephthalate layer including a homopolybutylene terephthalate film.