Hot rolling process of TiNi-based shape memory alloy with wide phase transition temperature window

The hot rolling process of TiNiZr alloy broadens its martensite transformation temperature window, solves the problem of poor controllability of Ti-Ni-Zr high-temperature shape memory alloy actuator, and achieves higher precision control function.

CN118751687AActive Publication Date: 2024-10-11YANTAI UNIV

Patent Information

Application Number
CN202410729288.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-06
Publication Date
2024-10-11
Estimated Expiration
2044-06-06

AI Technical Summary

Technical Problem

The martensitic phase transformation temperature window of Ti-Ni-Zr high-temperature shape memory alloy is narrow, resulting in poor controllability of the driver. Existing technical methods such as diffusion annealing and magnetron sputtering are cumbersome and difficult to control. New methods need to be developed to broaden the phase. Variable temperature window to improve driving accuracy.

Method used

Using the hot rolling process of TiNi-based shape memory alloy, sponge titanium, electrolytic nickel and crystallized zirconium are used as raw materials, the alloy is prepared according to the atomic ratio of Ti36.5-Ni48.5-Zr15, vacuum arc melting and repeated melting are performed to prepare a uniform alloy Afterwards, it is water quenched and hot rolled, and gradually thinned to a plate-shaped alloy. It is maintained under vacuum and high temperature conditions and sprayed with an anti-oxidation coating.

Benefits of technology

It significantly broadens the martensitic transformation temperature window, improves the precise control function of TiNiZr high-temperature shape memory alloy, and enhances the controllability of intelligent drive materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118751687A_ABST
    Figure CN118751687A_ABST
Patent Text Reader

Abstract

The invention discloses a hot rolling process of a TiNi-based shape memory alloy wide phase transition temperature window, which comprises the following steps: S1, taking sponge titanium, electrolytic nickel and crystalline zirconium as raw materials, and preparing a TiNiZr alloy with the total mass of 100g according to the atomic ratio of chemical components of Ti (36.5)-Ni (48.5)-Zr (15); s2, according to the principle that a low-melting-point nickel material is placed at the bottom of a crucible and high-melting-point crystal zirconium is placed on the uppermost side of the crucible, the prepared raw materials placed in the crucible are placed in a vacuum arc melting furnace; and S3, the raw materials are repeatedly smelted for five times under the electric arc effect, and the TiNiZr alloy with the uniform components is prepared and obtained. The martensite phase transformation temperature window of the TiNiZr high-temperature shape memory alloy subjected to hot rolling treatment is obviously widened compared with the martensite phase transformation temperature window of the as-cast TiNiZr high-temperature shape memory alloy, so that the precise control of the intelligent driving material of the TiNiZr high-temperature shape memory alloy is favorably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of shape memory alloy wide phase transformation technology, and more particularly to the hot rolling process of TiNi-based shape memory alloys with wide phase transformation temperature windows. Background Technology

[0002] Ti-Ni-Zr alloys, due to their low cost and adjustable martensitic transformation temperature over a wide range, have significant potential applications in high-temperature actuation applications such as nuclear power plant actuators, aero engines, current overload protection, and fire alarm devices, making them one of the most promising high-temperature shape memory alloys currently available. However, similar to other Ti-Ni-based shape memory alloys, Ti-Ni-Zr high-temperature shape memory alloys have a relatively narrow martensitic transformation temperature window (Ms(Af)-Mf(As)) (maximum approximately 60-70℃), which results in poor controllability of actuators made from them. In recent years, researchers have designed and prepared "functionally graded shape memory alloys" by incorporating gradients in chemical composition, geometric structure, and microstructure into shape memory alloys to broaden the martensitic transformation temperature window and thus achieve precise control of shape memory alloy actuators.

[0003] Nevertheless, current techniques, such as diffusion annealing, magnetron sputtering, and additive manufacturing, are relatively cumbersome and difficult to control. Therefore, there is an urgent need to develop new methods to broaden the martensitic phase transformation temperature window of Ti-Ni-Zr high-temperature shape memory alloys, thereby improving the precise control function of its drive. Summary of the Invention

[0004] The purpose of this invention is to solve the above-mentioned technical problems by proposing a hot rolling process for TiNi-based shape memory alloys with a wide phase transformation temperature window.

[0005] To achieve the above objectives, the present invention adopts the following technical solution:

[0006] The hot rolling process for TiNi-based shape memory alloys with a wide phase transformation temperature window includes the following steps:

[0007] S1, using sponge titanium, electrolytic nickel and crystalline zirconium as raw materials, a TiNiZr alloy with a total mass of 100g was prepared according to the chemical composition of Ti36.5-Ni48.5-Zr15 atomic ratio;

[0008] S2. Following the principle of placing low-melting-point nickel material at the bottom of the crucible and high-melting-point crystalline zirconium at the top of the crucible, place the prepared raw materials in the crucible into a vacuum arc melting furnace.

[0009] S3, a TiNiZr alloy with uniform composition is prepared by repeatedly melting the raw materials five times under the action of electric arc;

[0010] S4, the uniformly smelted TiNiZr alloy is melted again into a liquid state and allowed to flow into a 10mm×20mm×100mm copper mold under the action of gravity, finally obtaining a long strip alloy of 10mm×20mm×70mm.

[0011] S5, the obtained long strip-shaped Ti-Ni-Zr alloy is placed in a heating device for heat preservation and water quenching treatment;

[0012] S6, the processed long strip of Ti-Ni-Zr alloy is put into the rolling mill for hot rolling, and the rolling depth is 0.02mm each time;

[0013] S7. After each hot rolling, the hot-rolled TiNiZr alloy is placed in a heating device and held at 900°C in a vacuum for 5 minutes before being taken out and hot-rolled again. This process is repeated until the plate alloy with a thickness of 10 mm is rolled to a thickness of 5 mm.

[0014] Preferably, before the ingredients are mixed in step S1, the sponge titanium, electrolytic nickel and crystalline zirconium raw materials are washed in anhydrous ethanol to remove various impurities.

[0015] Preferably, in step S2, before placing the prepared raw materials into the crucible of the vacuum arc melting furnace, the furnace body is evacuated to a vacuum level of 10. -3 Pa, high-purity argon gas at 0.5 Pa is introduced into the vacuum arc melting furnace.

[0016] Preferably, in step S5, a molecular pump is used to evacuate the heating device to a vacuum level of 1.0 × 10⁻⁶. -3 Pa, then hold at 900℃ for 6 hours and water quench, then place the homogenized TiNiZr alloy strip in a heating device and heat to 900℃ and hold for 5 minutes.

[0017] Preferably, the heating equipment includes a support frame, with a vacuum tube furnace and a conveying mechanism mounted on the upper end of one end of the support frame. The conveying mechanism includes two support plates fixed on the support frame, with multiple conveying rollers rotating between the two support plates. The rolling mill is mounted on the support frame and includes a first U-shaped plate fixed to the upper end of the two support plates. Three round rods capable of synchronous rotation are threaded through the first U-shaped plate. The bottom of the three round rods is fixedly connected to a screw, and a threaded cylinder threadedly connected to the screw is sleeved on the outside of the screw. A second U-shaped plate is fixed to the bottom of the three threaded cylinders, and multiple hot rolling rollers arranged in a V-shape are mounted on the bottom of the second U-shaped plate.

[0018] Preferably, three drive boxes are fixed on the first U-shaped plate, and the three round rods pass through the opposite drive boxes and are rotatably connected to them. A rotatably configured drive rod passes through the three drive boxes, and three worm gears are fixed on the drive rods. A worm wheel is installed at the upper end of each of the three round rods, and the worm gear meshes with the worm wheel. A motor is installed on the drive box, and the output end of the motor is fixedly connected to the drive rod.

[0019] Preferably, the system also includes a spraying mechanism for spraying a high-temperature oxidation-resistant coating onto the TiNiZr alloy. The spraying mechanism includes a material box installed at the bottom of a support frame, a high-pressure pump installed on the material box, a delivery pipe installed at the output end of the high-pressure pump, and a U-shaped pipe connected to the delivery pipe fixed on the support plate. The U-shaped pipe is equipped with multiple nozzles.

[0020] Preferably, the distance between the upper and lower inner walls of the U-shaped tube is greater than the diameter of the conveying roller.

[0021] Compared with the prior art, the beneficial effects of this invention are as follows:

[0022] The martensitic transformation temperature window of the hot-rolled TiNiZr high-temperature shape memory alloy of this invention is significantly wider than that of the as-cast TiNiZr high-temperature shape memory alloy, which will help improve the precise control of TiNiZr high-temperature shape memory alloy smart drive materials. Attached Figure Description

[0023] Figure 1 DSC curves of TiNiZr high-temperature shape memory alloy in the as-cast state and after hot rolling.

[0024] Figure 2 Metallographic images of hot-rolled TiNiZr high-temperature shape alloys at different magnifications;

[0025] Figure 3 This is a schematic diagram of the heating equipment and rolling mill in the hot rolling process of the TiNi-based shape memory alloy with a wide phase transformation temperature window proposed in this invention.

[0026] Figure 4 This is a schematic diagram of the drive box structure in the hot rolling process of the TiNi-based shape memory alloy with a wide phase transformation temperature window proposed in this invention.

[0027] Figure 5 This is a side view of a U-shaped tube in the hot rolling process of the TiNi-based shape memory alloy with a wide phase transformation temperature window proposed in this invention.

[0028] In the diagram: 1. Support frame, 2. Vacuum tube furnace, 3. Support plate, 4. Conveying roller, 5. Second U-shaped plate, 6. First U-shaped plate, 7. Threaded cylinder, 8. Screw, 9. Hot rolling roll, 10. Worm gear, 11. Round rod, 12. Material box, 13. High pressure pump, 14. Conveying pipe, 15. U-shaped pipe, 16. Motor, 17. Nozzle, 18. Drive box, 19. Drive rod, 20. Worm gear. Detailed Implementation

[0029] The technical solutions of the present invention will be clearly and completely described below with reference to the accompanying drawings of the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments.

[0030] Reference Figures 1-5 The hot rolling process for TiNi-based shape memory alloys with a wide phase transformation temperature window includes the following steps:

[0031] S1, using sponge titanium, electrolytic nickel and crystalline zirconium as raw materials, a TiNiZr alloy with a total mass of 100g was prepared according to the chemical composition of Ti36.5-Ni48.5-Zr15 atomic ratio;

[0032] S2. Following the principle of placing low-melting-point nickel material at the bottom of the crucible and high-melting-point crystalline zirconium at the top of the crucible, place the prepared raw materials in the crucible into a vacuum arc melting furnace.

[0033] S3, a TiNiZr alloy with uniform composition is prepared by repeatedly melting the raw materials five times under the action of electric arc;

[0034] S4, the uniformly smelted TiNiZr alloy is melted again into a liquid state and allowed to flow into a 10mm×20mm×100mm copper mold under the action of gravity, finally obtaining a long strip alloy of 10mm×20mm×70mm.

[0035] S5, the obtained long strip-shaped Ti-Ni-Zr alloy is placed in a heating device for heat preservation and water quenching treatment;

[0036] S6, the processed long strip of Ti-Ni-Zr alloy is put into the rolling mill for hot rolling, and the rolling depth is 0.02mm each time;

[0037] S7. After each hot rolling, the hot-rolled TiNiZr alloy is placed in a heating device and held at 900°C in a vacuum for 5 minutes before being taken out and hot-rolled again. This process is repeated until the plate alloy with a thickness of 10 mm is rolled to a thickness of 5 mm.

[0038] In this invention, before the ingredients are mixed in step S1, the raw materials of sponge titanium, electrolytic nickel and crystalline zirconium are washed in anhydrous ethanol to remove various impurities.

[0039] In this invention, in step S2, before placing the prepared raw materials into the crucible of the vacuum arc melting furnace, the furnace body is evacuated to a vacuum level of 10. -3 Pa, high-purity argon gas at 0.5 Pa is introduced into the vacuum arc melting furnace.

[0040] In this invention, step S5 involves using a molecular pump to evacuate the heating device to a vacuum level of 1.0 × 10⁻⁶. -3 Pa, then hold at 900℃ for 6 hours and water quench, then place the homogenized TiNiZr alloy strip in a heating device and heat to 900℃ and hold for 5 minutes.

[0041] In this invention, to avoid cracking of the alloy material due to a large temperature difference between the high-temperature lath-shaped TiNiZr alloy and the rolling mill rolls, the temperature of the hot rolling rolls is raised to 400°C. Furthermore, to prevent oxidation during the hot rolling process after the lath-shaped TiNiZr alloy (because high-Zr content TiNiZr alloys are highly susceptible to oxidation at high temperatures) is removed from the vacuum tube furnace, a high-temperature anti-oxidation coating is applied to the surface of the TiNiZr alloy. If edge cracks appear during hot rolling, the crack edges are ground off using a grinding wheel. If the surface anti-oxidation coating is damaged during rolling, a high-temperature anti-oxidation coating is applied again.

[0042] In this invention, by Figure 1 As shown in the figure, the hot-rolled TiNiZr high-temperature shape memory alloy exhibits a typical dendritic morphology, and high-magnification metallographic images show that a high density of (Ti,Zr)2Ni second phase is distributed at the grain boundaries.

[0043] In this invention, by Figure 2 It can be seen that both the as-cast and hot-rolled TiNiZr high-temperature shape memory alloys exhibit a one-step martensitic phase transformation during heating and cooling, namely B19... ˊ →B2 reverse martensitic transformation and B2→B19 ˊMartensitic transformation. Using the tangential method to obtain the martensitic transformation temperature, it was found that the reverse martensitic transformation temperature window (Af-As) during the heating process of the as-cast TiNiZr high-temperature shape memory alloy is approximately 82℃, and the normal martensitic transformation temperature window (Ms-Mf) during the cooling process is approximately 61℃. In contrast, the reverse martensitic transformation temperature window (Af-As) during the heating process of the hot-rolled TiNiZr high-temperature shape memory alloy is approximately 129℃, and the normal martensitic transformation temperature window (Ms-Mf) during the cooling process is approximately 134℃. This means that the martensitic transformation temperature window of the hot-rolled TiNiZr high-temperature shape memory alloy is significantly wider than that of the as-cast TiNiZr high-temperature shape memory alloy. This will help improve the precise control of TiNiZr high-temperature shape memory alloy intelligent drive materials. Figure 2 (a): As-cast state; (b): Hot-rolled state.

[0044] The heating device in this invention includes a support frame 1, a vacuum tube furnace 2 and a conveying mechanism installed at one end of the support frame 1. The conveying mechanism includes two support plates 3 fixed on the support frame 1, and multiple conveying rollers 4 rotating between the two support plates 3. The multiple conveying rollers 4 are driven by chains, sprockets and other transmissions to achieve synchronous rotation, which can convey TiNiZr high temperature shape memory alloy between the vacuum tube furnace 2 and the rolling mill.

[0045] The rolling mill is mounted on a support frame 1. The rolling mill includes a first U-shaped plate 6 fixed to the upper ends of two support plates 3. Three round rods 11 that can rotate synchronously are passed through the first U-shaped plate 6. Three drive boxes 18 are fixed on the first U-shaped plate 6. The three round rods 11 pass through the corresponding drive boxes 18 and are rotatably connected to them. A rotatably mounted drive rod 19 is passed through the three drive boxes 18. Three worm gears 20 are fixed on the drive rods 19. A worm wheel 10 is installed at the upper end of each of the three round rods 11. The worm gears 20 mesh with the worm wheels 10. A motor 16 is mounted on the drive box 18. The output end of the motor 16 is fixedly connected to the drive rod 19.

[0046] The bottom of the three round rods 11 is fixedly connected to the screw rod 8. The screw rod 8 is fitted with a threaded cylinder 7 that is threadedly connected to it. The bottom of the three threaded cylinders 7 is fixed with a second U-shaped plate 5. Multiple hot rolling rollers 9 arranged in a V-shape are installed at the bottom of the second U-shaped plate 5. The shape of the second U-shaped plate 5 is matched with the hot rolling rollers 9.

[0047] Specifically, the motor 16 drives the drive rod 19 to rotate, which in turn drives the worm gear 20 to rotate, which in turn drives the worm wheel 10 to rotate, thus enabling the three worm wheels 10 to rotate. This, in turn, enables the three round rods 11 to rotate synchronously. The rotation of the round rods 11 drives the screw 8 to rotate. Since the first U-shaped plate 6 cannot rotate, the rotation of the screw 8 enables the threaded cylinder 7 and the second U-shaped plate 5 to move, which can adjust the distance between the hot rolling roll 9 and the conveying roll 4 for hot rolling of the alloy. Since the bottom of the second U-shaped plate 5 is equipped with multiple hot rolling rolls 9 arranged in a V-shape, the distance of hot rolling of the alloy can be gradually increased through the hot rolling rolls 9, which is more conducive to the hot rolling and thinning of the alloy.

[0048] It also includes a spraying mechanism for spraying anti-high temperature oxidation coating on TiNiZr alloy. The spraying mechanism includes a material box 12 installed at the bottom of the support frame 1. A high-pressure pump 13 is installed on the material box 12. The inlet end of the high-pressure pump 13 is connected to the material box 12 through a short pipe. A delivery pipe 14 is installed at the output end of the high-pressure pump 13. A U-shaped tube 15 connected to the delivery pipe 14 is fixed on the support plate 3. Multiple nozzles 17 are provided on the U-shaped tube 15. When the high-pressure pump 13 is working, it can transport the anti-oxidation coating through the delivery pipe 14 into the U-shaped tube 15, and finally spray it out through the nozzles 17. The distance between the upper and lower inner walls of the U-shaped tube 15 is greater than the diameter of the delivery roller 4. Thus, when the alloy passes between the U-shaped tubes 15, an oxide layer can be sprayed onto the alloy.

[0049] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any equivalent substitutions or modifications made by those skilled in the art within the scope of the technology disclosed in the present invention, based on the technical solution and inventive concept of the present invention, should be covered within the scope of protection of the present invention.

Claims

1. Hot rolling process of TiNi-based shape memory alloy with wide phase transition temperature window, characterized in that: The following steps are involved: S1, using sponge titanium, electrolytic nickel and crystalline zirconium as raw materials, a TiNiZr alloy with a total mass of 100 g is prepared according to a chemical composition of Ti36.5-Ni48.5-Zr15 atomic ratio; S2, placing the prepared raw materials in the crucible in a vacuum arc melting furnace according to the principle of placing the low melting point nickel material at the bottom of the crucible and the high melting point crystalline zirconium at the top of the crucible; S3, repeatedly melting the raw materials under the action of electric arc for 5 times to obtain a TiNiZr alloy with uniform composition; S4, melting the uniformly smelted TiNiZr alloy again into a liquid state so that it flows into a copper mold of 10 mm×20 mm×100 mm under the action of gravity, and finally obtaining a long strip of alloy of 10 mm×20 mm×70 mm; S5, placing the obtained long strip Ti-Ni-Zr alloy in a heating device for heat preservation and water quenching; S6, putting the treated long strip Ti-Ni-Zr alloy into a rolling mill for hot rolling, with each rolling depth being 0.02 mm; S7, after each hot rolling, the hot-rolled TiNiZr alloy is placed in a heating device for vacuum insulation at 900°C for 5 minutes, then taken out and hot-rolled again. This process is repeated until the plate-shaped alloy with a thickness of 10 mm is rolled to a thickness of 5 mm.

2. The hot rolling process for a TiNi-based shape memory alloy with a wide phase transition temperature window according to claim 1, characterized in that: Before preparing the ingredients in S1, the sponge titanium, electrolytic nickel and crystalline zirconium raw materials are placed in anhydrous ethanol for cleaning to remove various impurities.

3. The hot rolling process for a TiNi-based shape memory alloy with a wide phase transition temperature window according to claim 1, characterized in that: In S2, before placing the prepared raw materials in the crucible of the vacuum arc melting furnace, the furnace body is evacuated to 10 -3 Pa, and 0.5Pa of high-purity argon gas is injected into the vacuum arc melting furnace.

4. The hot rolling process for a TiNi-based shape memory alloy with a wide phase transition temperature window according to claim 1, characterized in that: In S5, a molecular pump is used to evacuate the heating device to a vacuum of 1.0×10 -3 Pa, then kept at 900°C for 6h and water quenched, and the homogenized TiNiZr alloy strips were placed in a heating device and heated to 900°C and kept for 5 minutes.

5. The hot rolling process for a TiNi-based shape memory alloy with a wide phase transition temperature window according to claim 1, characterized in that: The heating device comprises a support frame (1), a vacuum tube furnace (2) and a conveying mechanism are installed on the upper end of one end of the support frame (1), the conveying mechanism comprises two support plates (3) fixed on the support frame (1), a plurality of conveying rollers (4) are rotated between the two support plates (3), the rolling mill is installed on the support frame (1), the rolling mill comprises a first U-shaped plate (6) fixed on the upper ends of the two support plates (3), three round rods (11) that can rotate synchronously are penetrated through the first U-shaped plate (6), the bottoms of the three round rods (11) are fixedly connected with screw rods (8), the outer part of the screw rod (8) is sleeved with a threaded barrel (7) threadedly connected thereto, the bottoms of the three threaded barrels (7) are fixed with a second U-shaped plate (5), and the bottom of the second U-shaped plate (5) is installed with a plurality of hot rolling rollers (9) arranged in a V shape.

6. The hot rolling process for a TiNi-based shape memory alloy with a wide phase transition temperature window according to claim 5, characterized in that: Three drive boxes (18) are fixed on the first U-shaped plate (6); the three round rods (11) respectively penetrate the opposite drive boxes (18) and are rotatably connected thereto; the three drive boxes (18) are penetrated by drive rods (19) which are rotatably arranged; three worms (20) are fixed on the drive rods (19); worm wheels (10) are installed at the upper ends of the three round rods (11); the worm wheels (20) are meshed with the worm wheels (10); a motor (16) is installed on the drive box (18); and an output end of the motor (16) is fixedly connected to the drive rod (19).

7. The hot rolling process for a TiNi-based shape memory alloy with a wide phase transition temperature window according to claim 5, characterized in that: The invention also comprises a spraying mechanism for spraying a high-temperature oxidation resistant coating on a TiNiZr alloy, the spraying mechanism comprising a material box (12) mounted at the bottom of a support frame (1), a high-pressure pump (13) mounted on the material box (12), a delivery pipe (14) mounted at the output end of the high-pressure pump (13), a U-shaped pipe (15) connected to the delivery pipe (14) fixed on the support plate (3), and a plurality of spray heads (17) arranged on the U-shaped pipe (15).

8. The hot rolling process for a TiNi-based shape memory alloy with a wide phase transition temperature window according to claim 7, characterized in that: The distance between the upper and lower inner walls of the U-shaped tube (15) is greater than the diameter of the conveying roller (4).

Citation Information

Patent Citations

  • Thermodiffusion method for manufacturing wide temperature range phase transition nickel titanium alloy

    CN101245438A

  • Preparation method of NiTiNbCo wide hysteresis memory alloy

    CN101608287A

  • Ti50+xNi50-2xSnx shape memory alloy and preparation method thereof

    CN102534346A

  • Preparation method for TiNi memory alloy panel

    CN104399750A

  • Shape memory alloy with good processability and high inverse phase transition temperature and preparation method

    CN114807680A

Cited By

  • Temperature control method, system and equipment for titanium alloy forging and medium

    CN121115944A