Hard carbon negative electrode material and preparation method thereof, battery negative electrode plate and battery
Through the combination of biomass tar coating and dopants, the problems of large specific surface area and low interlayer spacing stability of hard carbon anode materials are solved, and the electrochemical performance of sodium-ion batteries and the first Coulombic efficiency and reversible specific capacity of the battery are significantly improved. .
Patent Information
- Application Number
- CN202411114721.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-10-11
AI Technical Summary
Existing hard carbon anode materials have large specific surface areas and low interlayer spacing stability, resulting in low initial Coulombic efficiency and specific capacity of sodium-ion batteries.
Biomass tar is used as the coating agent, mixed with pyrolytic carbon through organic solvent dissolution, and the biomass tar reacts and cracks under heating conditions to form a three-dimensional network structure, combined with the doping effect of the dopant, to reduce the specific surface area And improve the stability of layer spacing.
It significantly improves the electrochemical performance of hard carbon materials, improves the stability of interlayer spacing and the first Coulomb efficiency and reversible specific capacity of the battery.
Smart Images

Figure CN118754104A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of hard carbon negative electrode materials, and in particular to a hard carbon negative electrode material and a preparation method thereof, a battery negative electrode sheet and a battery. Background Art
[0002] As a new generation of energy storage batteries, sodium-ion batteries have rapidly entered the energy storage market with the characteristics of high energy storage and fast charge and discharge. As an excellent high-energy storage battery, the negative electrode material is the key to limiting its electrochemical performance. Among the negative electrode materials for sodium-ion batteries, hard carbon has the best performance. Hard carbon presents a "short-range order and long-range disorder" structure and has a larger interlayer spacing than graphite, which is very suitable for the embedding and storage of sodium ions. At present, the precursors of hard carbon materials are mainly biomass materials. Biomass materials have the characteristics of low cost and high capacity, and hard carbon materials can be prepared by high-temperature sintering. However, the hard carbon materials prepared by the above method generally have a large specific surface area and a low interlayer stability, resulting in low first coulombic efficiency and specific capacity of sodium-ion batteries. Summary of the invention
[0003] The present invention provides a hard carbon negative electrode material and a preparation method thereof, a battery negative electrode sheet and a battery, so as to solve the technical problems of large specific surface area and low interlayer stability of hard carbon negative electrode materials in the prior art.
[0004] To achieve the above object, the technical solution provided by the present invention is as follows: The first aspect of the present invention provides a method for preparing a hard carbon negative electrode material, comprising the following steps: S1, adding biomass tar to an organic solvent to dissolve it, and then adding a cross-linking agent to obtain a mixed liquid; S2, mixing pyrolytic carbon with a dopant to obtain a mixture, adding the mixed liquid to the mixture, stirring and heating to volatilize the organic solvent, heating the biomass tar to react and crack, and then coating the biomass tar on the surface of the pyrolytic carbon to obtain a coated material; S3, calcining the coated material obtained in step S2 to obtain the hard carbon negative electrode material.
[0005] Furthermore, in the step S1, the mass ratio of the biomass tar to the cross-linking agent is 9 to 99:1.
[0006] Furthermore, the mass ratio of the biomass tar to the pyrolytic carbon is 1:4-99.
[0007] Furthermore, the organic solvent in step S1 is selected from one or more of toluene, chloroform, glacial acetic acid, and ethanol.
[0008] Furthermore, the cross-linking agent in step S1 is selected from one or more of acrylic acid, methacrylic acid, divinylbenzene, and N-hydroxymethyl acrylamide.
[0009] Furthermore, the temperature for the reaction and cracking of the biomass tar in step S2 is 250°C to 400°C.
[0010] Furthermore, in step S2, the dopant is selected from one or more of boron-containing sodium salts and sulfur-containing sodium salts.
[0011] Furthermore, in the step S2, the mass ratio of the pyrolytic carbon to the dopant is 9 to 999:1.
[0012] Furthermore, the volatilization temperature of the organic solvent in step S2 is 62°C to 119°C.
[0013] Furthermore, in the step S3, the calcination temperature of the coating material is 1100° C. to 1600° C., and the calcination time is 0.5 h to 3 h.
[0014] Furthermore, the biomass tar and the pyrolytic charcoal are obtained by low-temperature pyrolysis of biomass materials, and the components of the biomass tar include hydroxyl derivatives containing benzene.
[0015] Furthermore, the biomass material is selected from one or more of coconut shells, bamboo, cotton stalks, reed stalks, and walnut shells.
[0016] Furthermore, the pyrolysis temperature of the biomass material is 350°C to 600°C.
[0017] The second aspect of the present invention provides a hard carbon negative electrode material prepared by the above preparation method.
[0018] The third aspect of the present invention provides a battery negative electrode sheet, which is obtained by mixing and grinding PVDF, acetylene black and the above-mentioned hard carbon negative electrode material, adding a binder and grinding to obtain a slurry, and coating the slurry on the surface of aluminum foil to obtain the battery negative electrode sheet.
[0019] A third aspect of the present invention provides a battery, which includes the above-mentioned battery negative electrode plate.
[0020] The preparation method of the hard carbon negative electrode material provided by the present invention uses biomass tar as a coating agent, adopts an organic solvent dissolving method to mix with pyrolytic carbon containing a dopant, and volatilizes the organic solvent by stirring and heating to achieve uniform coating of the pyrolytic carbon by the biomass tar, thereby avoiding the phenomenon of uneven coating of the pyrolytic carbon; by adding a cross-linking agent to react with the biomass tar to cross-link, the biomass tar is transformed from a branched structure to a three-dimensional network structure during the cracking process, thereby preventing the transformation of the biomass tar to soft carbon. In addition, the doping effect of the dopant and the coating are carried out together, which greatly improves the electrochemical performance of the hard carbon material while reducing the specific surface area of the hard carbon material, and improves the stability of the interlayer spacing. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0022] Figure 1 This is a TEM image of the hard carbon negative electrode material prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0023] In order to enable those skilled in the art to better understand the technical solutions in this application, the technical solutions in the embodiments of this application will be clearly and completely described below. Obviously, the described embodiments are only part of the embodiments of this application, not all of them. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0024] According to a first aspect of an embodiment of the present application, a method for preparing a hard carbon negative electrode material is provided, comprising the following steps: S1, adding biomass tar to an organic solvent to dissolve it, and then adding a cross-linking agent to obtain a mixed liquid; S2, mixing pyrolytic carbon with a dopant to obtain a mixture, adding the mixed liquid to the mixture, stirring and heating to volatilize the organic solvent, raising the temperature to react and crack the biomass tar, and then coating the biomass tar on the surface of the pyrolytic carbon to obtain a coated material; S3, calcining the coated material obtained in step S2 to obtain a hard carbon negative electrode material.
[0025] Currently, the industry uses coating processes to reduce the specific surface area of hard carbon materials, but the coating processes used all have the defect of uneven coating, which makes it difficult to effectively improve the first coulombic efficiency of hard carbon materials. In addition, various coating processes have problems such as slow coating speed, insufficient pyrolysis of coating sources, and high material loss rate.
[0026] The preparation method of the hard carbon negative electrode material provided in the embodiment of the present application uses biomass tar as a coating agent, adopts an organic solvent to dissolve and mix with pyrolytic carbon containing a dopant, and volatilizes the organic solvent by stirring and heating to achieve uniform coating of the pyrolytic carbon by the biomass tar, thereby avoiding the phenomenon of uneven coating of the pyrolytic carbon; by adding a cross-linking agent to react with the biomass tar to cross-link, the biomass tar is transformed from a branched structure to a three-dimensional network structure during the cracking process, thereby preventing the transformation of the biomass tar to soft carbon. In addition, the doping effect of the dopant and the coating are carried out together, which greatly improves the electrochemical performance of the hard carbon material while reducing the specific surface area of the hard carbon material, and improves the stability of the interlayer spacing.
[0027] In the embodiment of the present application, biomass tar is a byproduct produced during the pyrolysis of biomass materials. By using it as a coating agent for pyrolytic carbon, full utilization of biomass materials is achieved and production costs are controlled. In addition, in the preparation method of the hard carbon negative electrode material in the embodiment of the present application, the pyrolytic carbon and the dopant are mixed and the organic solvent dissolves the biomass hot tar, and then the order in which they enter the reactor is controlled, which ensures that the pyrolytic carbon and the solvent are fully stirred and avoids the phenomenon that some carbon powder floats on the surface of the solvent.
[0028] In the embodiment of the present application, biomass materials are used as raw materials to prepare pyrolytic carbon and biomass tar. Among them, the biomass material can be coconut shell, bamboo, cotton stalk, reed stalk, walnut shell, etc. The specific preparation method is as follows: 200 kg of coconut shell is placed in a pyrolysis furnace under a nitrogen environment (10L / min) at 400°C for 2 hours of low-temperature pyrolysis to obtain a mixture of about 72 kg of pyrolytic carbon material and 44 kg of biomass tar. Pyrolytic carbon can also be purchased.
[0029] During the pyrolysis of coconut shells, a large amount of organic gas will be generated, which will be discharged from the pyrolysis furnace through the exhaust pipe. The organic gas will be cooled and condensed into a liquid biomass tar mixture at the rear end of the exhaust pipe, so that it can be collected and separated from the pyrolytic carbon. The biomass tar mixture is subjected to static stratification treatment to obtain biomass tar. The above-mentioned biomass tar is mainly composed of the three elements of C, H, and O, and the main components include hydroxyl derivatives of benzene, as well as substances such as alkanes, acid esters, and ketones.
[0030] In the embodiment of the present application, after the biomass tar is precipitated from the organic solvent, it can be gradually transformed from a multi-branched long chain structure to a three-dimensional network chain structure at a temperature of 250°C to 400°C, wherein most of the CO bonds, C=O double bonds, and CH bonds will be broken, accompanied by H 2 O、CO 2 The gases are generated, and finally a three-dimensional network chain structure mainly composed of CC bonds and C=C double bonds is obtained, which also contains a small amount of CO bonds, C=O double bonds, and CH bonds. The three-dimensional network chain structure forms a thin film on the surface of the pyrolytic carbon to achieve the coating of the pyrolytic carbon.
[0031] According to a second aspect of an embodiment of the present application, a hard carbon negative electrode material prepared by the above preparation method is provided.
[0032] The third aspect of the embodiment of the present application provides a battery negative electrode sheet, which is obtained by mixing and grinding PVDF, acetylene black and the hard carbon negative electrode material prepared by the above-mentioned preparation method, adding a binder and grinding to obtain a slurry, and coating the slurry on the surface of aluminum foil to obtain a battery negative electrode sheet.
[0033] According to a fourth aspect of an embodiment of the present application, a battery is provided, the battery comprising the above-mentioned battery negative electrode sheet.
[0034] All reagents in the following examples are commercially available.
[0035] Example 1 A method for preparing a hard carbon negative electrode material comprises the following steps: 200 kg of coconut shells were placed in a pyrolysis furnace and subjected to low-temperature pyrolysis at 400 °C for 2 h under a nitrogen environment (10 L / min), yielding a mixture of about 72 kg of pyrolytic carbon material and 44 kg of biomass tar.
[0036] 500 g of biomass tar was added into 2000 mL of toluene to dissolve, and 26.32 g of cross-linking agent acrylic acid was added and stirred to obtain a mixed solution.
[0037] 4477.5 g of pyrolytic carbon and 22.5 g of sodium sulfite as a doping agent were mixed to obtain a mixture. The mixed solution was added to the mixture, stirred and heated to 100° C. to volatilize toluene, and then heated to 350° C. to react and crack the biomass tar, and then coated on the surface of the pyrolytic carbon to obtain a coated material.
[0038] The above-mentioned coating material is calcined at 1300° C. to obtain a hard carbon negative electrode material.
[0039] The specific surface area of the hard carbon negative electrode material was 4.52 m 2 / g. For the TEM images of the above hard carbon negative electrode materials, see Figure 1 .from Figure 1 The coating film on the surface of the hard carbon negative electrode material can be clearly seen.
[0040] The hard carbon negative electrode material is made into a battery negative electrode sheet according to the following steps: The hard carbon negative electrode material, PVDF and acetylene black were mixed and ground in a mass ratio of 90:5:5, and polyvinylidene fluoride binder was added dropwise after grinding for 5 minutes and then ground for another 5 minutes until the slurry was thin and thick. The ground slurry was evenly coated on the surface of aluminum foil with a thickness of 100 μm, dried at 120°C, and sliced to obtain a battery negative electrode sheet.
[0041] In a glove box under oxygen and water-free conditions, the negative electrode battery shell, the negative electrode sheet, the separator, the electrolyte, the sodium sheet (counter electrode), and the positive electrode battery shell are assembled in sequence, and after assembly, a small hydraulic press is used to compact the battery. After the battery is naturally placed for 6 hours, the electrochemical performance is tested using an electrochemical test system.
[0042] The first coulombic efficiency of the above battery is 88%, and the first reversible specific capacity is 331.6 mAh / g.
[0043] Example 2 A method for preparing a hard carbon negative electrode material comprises the following steps: The pyrolytic carbon and biomass tar prepared in Example 1 were used.
[0044] 500 g of biomass tar was added into 1000 mL of toluene to dissolve, and then 23.95 g of cross-linking agent divinylbenzene was added and stirred to obtain a mixed solution.
[0045] 4480.5 g of pyrolytic carbon and 19.5 g of sodium tetraborate as a dopant are mixed to obtain a mixture. The mixed solution is added to the mixture, stirred and heated to 100° C. to volatilize toluene, and then heated to 350° C. to react and crack the biomass tar, and then coated on the surface of the pyrolytic carbon to obtain a coated material.
[0046] The above-mentioned coating material is calcined at 1200° C. to obtain a hard carbon negative electrode material.
[0047] The specific surface area of the hard carbon negative electrode material was 5.92 m 2 / g.
[0048] The hard carbon negative electrode material is made into a battery negative electrode sheet according to the following steps: The hard carbon negative electrode material, PVDF and acetylene black were mixed and ground in a ratio of 90:5:5, and polyvinylidene fluoride binder was added dropwise after grinding for 5 minutes and then ground for another 5 minutes until the slurry was thin and thick. The ground slurry was evenly coated on the surface of aluminum foil with a thickness of 100 μm, dried at 120°C, and sliced to obtain a negative electrode sheet for the battery.
[0049] In a glove box under oxygen and water-free conditions, the negative electrode battery shell, the negative electrode sheet, the separator, the electrolyte, the sodium sheet (counter electrode), and the positive electrode battery shell are assembled in sequence, and after assembly, a small hydraulic press is used to compact the battery. After the battery is naturally placed for 6 hours, the electrochemical performance is tested using an electrochemical test system.
[0050] The first coulombic efficiency of the above battery is 86%, and the first reversible specific capacity is 328.8 mAh / g.
[0051] Example 3 A method for preparing a hard carbon negative electrode material comprises the following steps: The pyrolytic carbon and biomass tar prepared in Example 1 were used.
[0052] 500 g of biomass tar was added into 2000 mL of glacial acetic acid to dissolve, and then 18.80 g of methacrylic acid, a cross-linking agent, was added and stirred to obtain a mixed solution.
[0053] 4453.5 g of pyrolytic carbon and 44.5 g of sodium sulfite were mixed to obtain a mixture. The mixed solution was added to the mixture, stirred and heated to 100° C. to volatilize the glacial acetic acid, and then heated to 400° C. to react and crack the biomass tar, and then coated on the surface of the pyrolytic carbon to obtain a coated material.
[0054] The above-mentioned coating material is calcined at 1400° C. to obtain a hard carbon negative electrode material.
[0055] The specific surface area of the hard carbon negative electrode material was 4.85 m 2 / g.
[0056] The hard carbon negative electrode material is made into a battery negative electrode sheet according to the following steps: The hard carbon negative electrode material, PVDF and acetylene black were mixed and ground in a mass ratio of 90:5:5, and polyvinylidene fluoride binder was added dropwise after grinding for 5 minutes and then ground for another 5 minutes until the slurry was thin and thick. The ground slurry was evenly coated on the surface of aluminum foil with a thickness of 100 μm, dried at 120°C, and sliced to obtain a battery negative electrode sheet.
[0057] In a glove box under oxygen and water-free conditions, the negative electrode battery shell, the negative electrode sheet, the separator, the electrolyte, the sodium sheet (counter electrode), and the positive electrode battery shell are assembled in order, and after assembly, a small hydraulic press is used to compact the battery. After the battery is naturally placed for 6 hours, the electrochemical performance is tested using an electrochemical test system.
[0058] The first coulombic efficiency of the above battery is 87%, and the first reversible specific capacity is 329.4 mAh / g.
[0059] Example 4 A method for preparing a hard carbon negative electrode material comprises the following steps: The pyrolytic carbon and biomass tar prepared in Example 1 were used.
[0060] 500 g of biomass tar was added into 500 mL of ethanol to dissolve, and then 20.62 g of a cross-linking agent, N-hydroxymethyl acrylamide, was added and stirred to obtain a mixed solution.
[0061] 4416.8 g of pyrolytic carbon and 83.2 g of sodium perborate were mixed to obtain a mixture. The mixed solution was added to the mixture, stirred and heated to 105° C. to volatilize the ethanol, and then heated to 250° C. to react and crack the biomass tar, and then coated on the surface of the pyrolytic carbon to obtain a coated material.
[0062] The above-mentioned coating material is calcined at 1600° C. to obtain a hard carbon negative electrode material.
[0063] The specific surface area of the hard carbon negative electrode material was 5.63 m2 / g.
[0064] The hard carbon negative electrode material is made into a battery negative electrode sheet according to the following steps: The hard carbon negative electrode material, PVDF and acetylene black were mixed and ground in a mass ratio of 90:5:5, and polyvinylidene fluoride binder was added dropwise after grinding for 5 minutes and then ground for another 5 minutes until the slurry was thin and thick. The ground slurry was evenly coated on the surface of aluminum foil with a thickness of 100 μm, dried at 120°C, and sliced to obtain a battery negative electrode sheet.
[0065] In a glove box under oxygen and water-free conditions, the negative electrode battery shell, the negative electrode sheet, the separator, the electrolyte, the sodium sheet (counter electrode), and the positive electrode battery shell are assembled in sequence, and after assembly, a small hydraulic press is used to compact the battery. After the battery is naturally placed for 6 hours, the electrochemical performance is tested using an electrochemical test system.
[0066] The first coulombic efficiency of the above battery is 84%, and the first reversible specific capacity is 317.3 mAh / g.
[0067] Example 5 A method for preparing a hard carbon negative electrode material comprises the following steps: The pyrolytic carbon and biomass tar prepared in Example 1 were used.
[0068] 500 g of biomass tar was added to 1500 mL of ethanol to dissolve, and then 31.29 g of methacrylic acid, a cross-linking agent, was added and stirred to obtain a mixed solution.
[0069] 4367.3 g of pyrolytic carbon and 133.7 g of sodium thiosulfate were mixed to obtain a mixture. The mixed solution was added to the mixture, stirred and heated to 95° C. to volatilize the ethanol, and then heated to 200° C. to react and crack the biomass tar, and then coated on the surface of the pyrolytic carbon to obtain a coated material.
[0070] The above-mentioned coating material is calcined at 1350° C. to obtain a hard carbon negative electrode material.
[0071] The specific surface area of the hard carbon negative electrode material was 4.97 m 2 / g.
[0072] The hard carbon negative electrode material is made into a battery negative electrode sheet according to the following steps: The hard carbon negative electrode material, PVDF and acetylene black were mixed and ground in a mass ratio of 90:5:5, and polyvinylidene fluoride binder was added dropwise after grinding for 5 minutes and then ground for another 5 minutes until the slurry was thin and thick. The ground slurry was evenly coated on the surface of aluminum foil with a thickness of 100 μm, dried at 120°C, and sliced to obtain a battery negative electrode sheet.
[0073] In a glove box under oxygen and water-free conditions, the negative electrode battery shell, the negative electrode sheet, the separator, the electrolyte, the sodium sheet (counter electrode), and the positive electrode battery shell are assembled in sequence, and after assembly, a small hydraulic press is used to compact the battery. After the battery is naturally placed for 6 hours, the electrochemical performance is tested using an electrochemical test system.
[0074] The first coulombic efficiency of the above battery is 86%, and the first reversible specific capacity is 329.2 mAh / g.
[0075] Comparative Example 1 A method for preparing a conventional melt-coated hard carbon negative electrode material comprises the following steps: 100 g of asphalt with a softening point of 280° C. was mixed with 900 g of pyrolytic carbon, and the mixture was placed in a coating machine, stirred, heated to 400° C. and kept warm for 6 hours, and then heated to 800° C. and kept warm for 4 hours to obtain a coated material.
[0076] The above-mentioned coating material is calcined at 1300° C. to obtain a hard carbon negative electrode material.
[0077] The specific surface area of the hard carbon negative electrode material was 21.51 m 2 / g.
[0078] The hard carbon negative electrode material is made into a battery negative electrode sheet according to the following steps: The hard carbon negative electrode material, PVDF and acetylene black were mixed and ground in a mass ratio of 90:5:5, and polyvinylidene fluoride binder was added dropwise after grinding for 5 minutes and then ground for another 5 minutes until the slurry was thin and thick. The ground slurry was evenly coated on the surface of aluminum foil with a thickness of 100 μm, dried at 120°C, and sliced to obtain a battery negative electrode sheet.
[0079] In a glove box under oxygen and water-free conditions, the positive electrode sheet, the negative electrode sheet, the battery shell, and the electrolyte are assembled in order, and after assembly, a small hydraulic press is used to compact the battery. After the battery is naturally placed for 6 hours, the electrochemical performance is tested using an electrochemical test system.
[0080] The first coulombic efficiency of the above battery is 79%, and the first reversible specific capacity is 275.6 mAh / g.
[0081] Comparative Example 2 A method for preparing a conventional coated hard carbon negative electrode material comprises the following steps: 150 g of asphalt with a softening point of 150° C. was mixed with 850 g of pyrolytic carbon, and the mixture was placed in a fusion and rapidly stirred while heating to 200° C. and maintaining the temperature for 24 hours to obtain a coating material.
[0082] The above-mentioned coating material is calcined at 1250° C. to obtain a hard carbon negative electrode material.
[0083] The specific surface area of the hard carbon negative electrode material was 28.36 m 2 / g.
[0084] The hard carbon negative electrode material is made into a battery negative electrode sheet according to the following steps: The hard carbon negative electrode material, PVDF and acetylene black were mixed and ground in a mass ratio of 90:5:5, and polyvinylidene fluoride binder was added dropwise after grinding for 5 minutes and then ground for another 5 minutes until the slurry was thin and thick. The ground slurry was evenly coated on the surface of aluminum foil with a thickness of 100 μm, dried at 120°C, and sliced to obtain a battery negative electrode sheet.
[0085] In a glove box under oxygen and water-free conditions, the positive electrode sheet, the negative electrode sheet, the battery shell, and the electrolyte are assembled in order, and after assembly, a small hydraulic press is used to compact the battery. After the battery is naturally placed for 6 hours, the electrochemical performance is tested using an electrochemical test system.
[0086] The first coulombic efficiency of the above battery is 77%, and the first reversible specific capacity is 259.7 mAh / g.
[0087] The comparison of the electrochemical performance test results of the batteries of Examples 1 to 5 and Comparative Examples 1 and 2 is shown in Table 1.
[0088] Table 1 Comparison of battery electrochemical performance test results
[0089] From the comparison between Examples 1 to 5 and the comparative example, it can be seen that the preparation method of the hard carbon negative electrode material in the embodiment of the present application can effectively control the specific surface area of the hard carbon material to be within 6 m 2 / g, while the specific surface area of the hard carbon negative electrode material prepared by the traditional method is 21.51 m 2 / g; the first coulombic efficiency is also much higher than 79% of the comparative example. From the above data, it can be seen that the preparation method of the hard carbon negative electrode material in the embodiment of the present application can significantly improve the uniformity of the material coating, and the addition of the dopant greatly increases the first reversible specific capacity of the material.
[0090] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for preparing a hard carbon negative electrode material, characterized in that: The following steps are involved: S1, adding biomass tar into an organic solvent to dissolve, and then adding a cross-linking agent to obtain a mixed solution; S2, mixing pyrolytic carbon and a dopant to obtain a mixture, adding the mixed solution to the mixture, stirring and heating to volatilize the organic solvent, heating to react and crack the biomass tar, and then coating the biomass tar on the surface of the pyrolytic carbon to obtain a coating material; S3. calcining the coating material obtained in step S2 to obtain the hard carbon negative electrode material.
2. The method for preparing a hard carbon negative electrode material according to claim 1, characterized in that: In the step S1, the mass ratio of the biomass tar to the cross-linking agent is 9 to 99:
1.
3. The method for preparing a hard carbon negative electrode material according to claim 1, characterized in that: The mass ratio of the biomass tar to the pyrolysis carbon is 1:4-99.
4. The method for preparing a hard carbon negative electrode material according to claim 1, characterized in that: The organic solvent in step S1 is selected from one or more of toluene, chloroform, glacial acetic acid and ethanol.
5. The method for preparing a hard carbon negative electrode material according to claim 1, characterized in that: The cross-linking agent in step S1 is selected from one or more of acrylic acid, methacrylic acid, divinylbenzene, and N-hydroxymethyl acrylamide.
6. The method for preparing a hard carbon negative electrode material according to claim 1, characterized in that: The temperature for the reaction and cracking of the biomass tar in step S2 is 250°C to 400°C.
7. The method for preparing a hard carbon negative electrode material according to claim 1, characterized in that: In step S2, the dopant is selected from one or more of boron-containing sodium salts and sulfur-containing sodium salts.
8. The method for preparing a hard carbon negative electrode material according to claim 1, characterized in that: In the step S2, the mass ratio of the pyrolytic carbon to the dopant is 9 to 999:
1.
9. The method for preparing a hard carbon negative electrode material according to any one of claims 1 to 8, characterized in that: The volatilization temperature of the organic solvent in step S2 is 62°C to 119°C.
10. The method for preparing a hard carbon negative electrode material according to any one of claims 1 to 8, characterized in that: The calcination temperature of the coating material in step S3 is 1100° C. to 1600° C., and the calcination time is 0.5 h to 3 h.
11. The method for preparing a hard carbon negative electrode material according to any one of claims 1 to 8, characterized in that: The biomass tar and the pyrolytic charcoal are obtained by low-temperature pyrolysis of biomass materials, and the components of the biomass tar include hydroxyl derivatives containing benzene.
12. The method for preparing a hard carbon negative electrode material according to claim 11, characterized in that: The biomass material is selected from one or more of coconut shells, bamboo, cotton stalks, reed stalks, and walnut shells.
13. The method for preparing a hard carbon negative electrode material according to claim 11, characterized in that: The pyrolysis temperature of the biomass material is 350°C to 600°C.
14. The hard carbon negative electrode material prepared by the method for preparing the hard carbon negative electrode material according to any one of claims 1 to 13.
15. A battery negative electrode sheet, characterized in that: PVDF, acetylene black and the hard carbon negative electrode material prepared by the preparation method according to claims 1 to 13 are mixed and ground, and a binder is added dropwise and ground to obtain a slurry, and the slurry is coated on the surface of an aluminum foil to obtain the battery negative electrode sheet.
16. A battery, characterized in that: Including the battery negative electrode sheet as described in claim 15.
Citation Information
Patent Citations
Bamboo-based hard carbon active electrode material, preparation thereof and application of bamboo-based hard carbon active electrode material in sodium ion battery
CN115849333A
Negative electrode material and preparation method thereof, negative electrode plate and secondary battery
CN116154129A
Cited By
Preparation method of hard carbon material and application of hard carbon material in sodium-ion battery